A high-precision contamination method for small-area silicone rubber test pieces

By configuring artificial filth components and combining ultrasonic vibration and bowstring method, the problem of filth simulation and uniform coating on small-area silicone rubber test pieces is solved, and high-precision filth coating is achieved, reducing experimental errors and uneven filth problems are noted. .

CN114487726BActive Publication Date: 2024-12-03STATE GRID ZHEJIANG ELECTRIC POWER CO LTD PANAN COUNTY POWER SUPPLY CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111586887.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-12-03
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high-precision filth simulation and uniform smearing on small-area silicone rubber test pieces, resulting in large experimental errors and poor filth effect.

Method used

By configuring artificial filth components according to the hydrophobicity of the insulator, the filth treatment is performed using ultrasonic vibration and bowstring method to ensure uniform adhesion and fluidization of the filthy liquid, avoiding the agglomeration of filthy particles, and simplifying the weighing operation by multiplication preparation and balanced splitting method.

Benefits of technology

A more accurate filth simulation is achieved, experimental errors are reduced, the uniform distribution and fluidization effect of filth is ensured, and the accuracy and consistency of filth is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-precision contamination method for a small-area silicone rubber test piece, comprising the following steps: S1 configuring components of artificial contamination, S2 obtaining the mass m of the artificial contamination, adding water and stirring to form an artificial contamination liquid, S3 treating the silicone rubber test piece, S4 ultrasonic vibration and contamination treatment, and S5 test piece preservation. The invention has the following advantages: since S1 configures the components of artificial contamination according to the hydrophobicity of the insulator, better simulation can be achieved; the method of preparing a solution by multiplying the mass m and then taking it out evenly in S2 avoids the difficulty of directly weighing contamination of too small a mass, simplifies the experimental operation, and reduces the experimental error; S4 uses ultrasonic vibration mechanical external force to disperse contamination particles so as to inhibit the agglomeration between particles; during ultrasonic vibration, the contamination is treated by using a bowstring method, which can not only avoid the formation of surface texture of the test piece painted with a brush, but also effectively solves the problem that the existing contamination method is difficult to contaminate evenly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-precision contamination method for a small-area silicone rubber test piece. Background Art

[0002] Compared with the previous porcelain and glass insulators, silicone rubber insulators have the characteristics of strong hydrophobicity, light weight, and easy maintenance. In recent years, they have been widely used in the fields of electricity, railways, etc. With the increase in the use of silicone rubber insulators, silicone rubber insulators are seriously polluted by air pollution, especially under DC voltage, which affects the external insulation safety and operation reliability of the system. Under the condition of serious pollution, silicone rubber will accelerate aging and reduce its service life, and there is a risk of large-scale power outages caused by large-scale effectiveness. Therefore, the accurate and controllable sample preparation of silicone rubber for different pollution tests is of great significance to explore the effect of silicone rubber attached pollution under artificial fog and cleaning agent immersion. The discharge characteristics and mechanisms of silicone rubber insulators under lubrication are of great significance. The common method for studying the flashover characteristics of silicone rubber insulators is to use a quantitative brushing method to conduct artificial pollution tests on a small area of ​​silicone rubber sheets. However, the existing regulations do not make clear provisions in the following aspects: (1) The salt and ash specifications used to prepare artificial pollution are not determined; (2) It is difficult to directly weigh the artificial pollution on a small area of ​​the test piece; (3) Since the silicone rubber surface is highly hydrophobic, it is difficult for the pollution to adhere to it, and the groups between the pollution particles will agglomerate, which also makes it difficult for the pollution to spread on the surface of the test piece; (4) The existing brushing pollution method is difficult to achieve uniform brushing. Summary of the invention

[0003] The purpose to be achieved by the present invention is to provide a high-precision contamination method for a small-area silicone rubber test piece, which can not only better simulate the contamination situation, but also effectively reduce the experimental error.

[0004] In order to solve the above technical problems, the present invention is implemented by the following technical solutions: a high-precision contamination method for a small-area silicone rubber test piece, comprising the following steps:

[0005] S1: The components of artificial pollution are configured according to the hydrophobicity of the insulator. When the hydrophobicity of the insulator is lost, the artificial pollution includes diatomaceous earth and soluble salt, and the mass ratio of diatomaceous earth to soluble salt is 6:1. When the insulator has good hydrophobicity, the artificial pollution includes kaolin and soluble salt, and the mass ratio of kaolin to soluble salt is 6:1.

[0006] S2: The mass m of artificial pollution is obtained according to the area of ​​the silicone rubber test piece and the required salt density and ash density. The calculation formula is:

[0007] m=ρ ESDD / ρ NSDD ×S; where: ρ ESDD is the equivalent salt density, ρNSDD is the equivalent gray density, S is the area of ​​the silicone rubber test piece;

[0008] The calculated mass m is enlarged N times and weighed into a test tube or / and a measuring cylinder, and water is added to the test tube or / and the measuring cylinder to fully stir and dissolve, and the conductivity of the artificial dirty liquid is not greater than 0.05S / m at 20°C;

[0009] S3: evenly coat a layer of dry diatomaceous earth on the silicone rubber test piece, then divide the artificial dirty liquid prepared in S2 into M parts, where: M=N, and drop one of the divided artificial dirty liquid on the treated silicone rubber test piece through a rubber dropper;

[0010] S4: placing the silicone rubber test piece treated in S3 on an ultrasonic vibration platform for ultrasonic vibration treatment, and performing smearing treatment by the bowstring method during the ultrasonic vibration treatment, the frequency of the ultrasonic wave is 40-60 Hz, the sound pressure intensity is not less than 130 dB, the ultrasonic amplitude is 80% of the maximum amplitude, the ultrasonic vibration is performed for 50 cycles, the ultrasonic time and interval time of each cycle are 60 s and 5 s respectively, and the smearing speed is 1 m / s;

[0011] S5: Dry the silicone rubber test piece after the treatment in S4 in the shade and store it.

[0012] Preferably, the specific surface area of ​​the diatomaceous earth in S1 is greater than 10.9 m 2 / g, the total pore volume of diatomite is > 0.037 cm 3 / g, the average pore size of diatomaceous earth is >10.9nm.

[0013] Preferably, the kaolin in S1 is industrial raw material grade kaolin.

[0014] Preferably, the soluble salts in S1 include NaCl and CaSO4, and the mass ratio of NaCl to CaSO4 is 1:4.

[0015] Preferably, the mass after being enlarged N times in S2 is weighed by an electronic balance, and N is 50-100.

[0016] Preferably, the amount of water added during sufficient stirring and dissolution in S2 is twice, and the mass of the water added twice is 190-210 ml.

[0017] Preferably, the water in S2 is added to the test tube or / and the measuring cylinder through a rubber dropper, and the mass of the water added twice is equal.

[0018] Preferably, the diatomaceous earth in S3 is evenly coated on the silicone rubber test piece through a dry sponge mass, and after coating, excess diatomaceous earth on the surface of the silicone rubber test piece is blown off by an ear cleaning bulb.

[0019] Preferably, the string of the bow string method in S4 is a wet cotton thread.

[0020] Preferably, the shade drying operation in S5 is performed by shielding with a light-proof shielding cover, and the moisture in the shielding cover is extracted by a dehumidifier.

[0021] In summary, the advantages of the present invention are as follows: S1 configures the components of artificial pollution, S2 obtains the mass m of artificial pollution, and adds water to stir to form artificial pollution liquid, S3 treats the silicone rubber test piece, S4 ultrasonic vibration and smearing treatment, and S5 the test piece preservation method realizes high-precision smearing of small-area silicone rubber test pieces. Since S1 configures the components of artificial pollution according to the hydrophobicity of the insulator, better simulation can be achieved. In S2, the mass m of artificial pollution is obtained by the area of ​​the silicone rubber test piece and the required salt density and ash density, and the mass m is enlarged by N times. In S3, the artificial pollution liquid is divided into M parts. Since N=M, the method of preparing a solution by doubling the mass m and then taking it out evenly avoids the difficulty of directly weighing too small a mass of pollution, simplifies the experimental operation, and reduces the experimental error. A layer of diatomaceous earth is evenly coated on the silicone rubber test piece, so that the prepared artificial pollution can be adsorbed on the surface of the test piece without destroying its own hydrophobicity. S4 places the silicone rubber test piece on an ultrasonic vibration platform, and uses ultrasonic vibration mechanical external force to break up the pollution particles to inhibit the particles from moving. Since the prepared artificial dirt contains the most SiO2 particles with a diameter of several microns, the frequency of the ultrasound is 40-60Hz, the sound pressure intensity is not less than 130dB, the ultrasonic amplitude is 80% of the maximum amplitude, and the ultrasonic vibration is performed for 50 cycles, with the ultrasonic time and interval time of each cycle being 60s and 5s respectively, so that the critical fluidization velocity of the dirt is the lowest, the fluidization quality is guaranteed, and it is more conducive to the inhibition between the dirt groups. In addition, the ultrasonic vibration is performed for 50 cycles, with the ultrasonic time and interval time of each cycle being 60s and 5s respectively, and the vibration frequency can resonate with the dirt particles to inhibit the group agglomeration, solving the problem that the original coating method repeatedly coats the test piece but the coating effect is not good; and during the ultrasonic vibration, the bowstring method is used for coating, and the coating speed is 1m / s, which can not only avoid the formation of surface texture of the test piece coated with a brush, but also effectively solve the problem that the existing coating method is difficult to coat evenly. In S5, the storage is carried out after the shade drying operation, which can avoid the influence of humidity on the silicone rubber test piece. DETAILED DESCRIPTION

[0022] A high-precision contamination method for a small-area silicone rubber test piece comprises the following steps:

[0023] S1: The components of artificial pollution are configured according to the hydrophobicity of the insulator. When the hydrophobicity of the insulator is lost, the artificial pollution includes diatomaceous earth and soluble salt, and the mass ratio of diatomaceous earth to soluble salt is 6:1. When the insulator has good hydrophobicity, the artificial pollution includes kaolin and soluble salt, and the mass ratio of kaolin to soluble salt is 6:1.

[0024] S2: The mass m of artificial pollution is obtained according to the area of ​​the silicone rubber test piece and the required salt density and ash density. The calculation formula is:

[0025] m=ρ ESDD / ρ NSDD ×S; where: ρ ESDD is the equivalent salt density, ρ NSDD is the equivalent gray density, S is the area of ​​the silicone rubber test piece;

[0026] The calculated mass m is enlarged N times and weighed into a test tube or / and a measuring cylinder, and water is added to the test tube or / and the measuring cylinder to fully stir and dissolve, and the conductivity of the artificial dirty liquid is not greater than 0.05S / m at 20°C;

[0027] S3: evenly coat a layer of dry diatomaceous earth on the silicone rubber test piece, then divide the artificial dirty liquid prepared in S2 into M parts, where: M=N, and drop one of the divided artificial dirty liquid on the treated silicone rubber test piece through a rubber dropper;

[0028] S4: placing the silicone rubber test piece treated in S3 on an ultrasonic vibration platform for ultrasonic vibration treatment, and performing smearing treatment by the bowstring method during the ultrasonic vibration treatment, the frequency of the ultrasonic wave is 40-60 Hz, the sound pressure intensity is not less than 130 dB, the ultrasonic amplitude is 80% of the maximum amplitude, the ultrasonic vibration is performed for 50 cycles, the ultrasonic time and interval time of each cycle are 60 s and 5 s respectively, and the smearing speed is 1 m / s;

[0029] S5: Dry the silicone rubber test piece after the treatment in S4 in the shade and store it.

[0030] The components of artificial pollution are configured by S1, the mass m of artificial pollution is obtained by S2, and water is added to stir to form artificial pollution liquid, S3 silicone rubber test piece is treated, S4 ultrasonic vibration and pollution treatment, S5 test piece preservation method realizes high-precision pollution of small area silicone rubber test piece, because S1 configures the components of artificial pollution according to the hydrophobicity of the insulator, therefore, better simulation can be achieved, S2 obtains the mass m of artificial pollution by the area of ​​the silicone rubber test piece and the required salt density and ash density, and the mass m is enlarged by N times, S3 divides the artificial pollution liquid into M parts, because N=M, the method of preparing the solution by doubling the mass m and then taking it out evenly avoids the difficulty of directly weighing the pollution of too small mass, simplifies the experimental operation, and reduces the experimental error, and evenly coats a layer of diatomaceous earth on the silicone rubber test piece, so that the prepared artificial pollution can be adsorbed on the surface of the test piece without destroying its own hydrophobicity, S4 places the silicone rubber test piece on the ultrasonic vibration platform, and uses ultrasonic vibration mechanical external force to disperse the pollution particles to inhibit the agglomeration between the particles, because The prepared artificial dirt contains the most SiO2 particles with a particle size of several microns. Therefore, the frequency of the ultrasonic wave is 40-60Hz, the sound pressure intensity is not less than 130dB, the ultrasonic amplitude is 80% of the maximum amplitude, and the ultrasonic vibration is performed for 50 cycles. The ultrasonic time and interval time of each cycle are 60s and 5s respectively, so that the critical fluidization velocity of the dirt is the lowest, the fluidization quality is guaranteed, and it is more conducive to the inhibition between the dirt groups. In addition, the ultrasonic vibration is performed for 50 cycles. The vibration frequency of each cycle is 60s and 5s respectively, which can resonate with the dirt particles to inhibit the group agglomeration, solving the problem that the original coating method repeatedly coats the test piece but the coating effect is not good; moreover, during the ultrasonic vibration, the bowstring method is used for coating, and the coating speed is 1m / s, which can not only avoid the formation of surface texture of the test piece coated with a brush, but also effectively solve the problem that the existing coating method is difficult to coat evenly. In S5, it is stored after drying in the shade to avoid the influence of humidity on the silicone rubber test piece.

[0031] The specific surface area of ​​diatomaceous earth in S1 is > 10.9 m 2 / g, the total pore volume of diatomite is > 0.037 cm 3 / g, the average pore size of diatomite is greater than 10.9nm. Diatomite with large specific surface area, total pore volume and average pore size has a faster hydrophobic migration speed and can better simulate the required hydrophobicity of the insulator surface. The kaolin in S1 is industrial raw material grade kaolin. Industrial raw material grade kaolin has the slowest hydrophobic migration speed and can better simulate the required hydrophobicity of the insulator surface. The soluble salts in S1 include NaCl and CaSO4, and the mass ratio of NaCl and CaSO4 is 1:4. NaCl represents the easily soluble components in the soluble salts on the insulator, and CaSO4 represents the insoluble components. Mixing the two in a ratio of 1:4 is more in line with the actual pollution situation.

[0032] The mass of S2 after being enlarged N times is weighed by an electronic balance, and N is 50-100, which can change the order of magnitude of the calculated artificial contamination mass from milligrams to grams, facilitates the weighing of operators, and ensures the accuracy of the weighing process. Before use, white paper needs to be placed on the electronic balance to reduce the adhesion of artificial contamination on the electronic balance. When S2 is fully stirred and dissolved, the amount of water added is twice, and the mass of the water added twice is 190-210 ml. The water in S2 is added to the test tube or / and the measuring cylinder through a rubber dropper, and the mass of the water added twice is equal. In this embodiment, the mass of the water added twice is 200 ml, which can fully dissolve the artificial contamination. The rubber dropper can well control the mass of water added to ensure that the surface of the test sample reaches the required degree of contamination.

[0033] The diatomaceous earth in S3 is evenly coated on the silicone rubber test piece through a dry sponge ball, and after coating, the excess diatomaceous earth on the surface of the silicone rubber test piece is blown off by an ear cleaning bulb, so that a hydrophilic surface can be attached to the surface of the silicone rubber. The configured dirty liquid has a good adsorption effect, and the thickness of the coated diatomaceous earth is thin, which will not affect the experimental results. The string of the bowstring method in S4 uses a wet cotton thread. The bowstring is fixed on the electric slide rail and does not completely contact the dirty surface. The slide rails on both sides evenly drive the cotton thread back and forth to form a water film on the surface of the sample, so that the dirt can be evenly attached to the surface of the sample. The wet cotton thread and the adhesion of the silicone rubber surface are used to form a water film on the surface to achieve uniform contamination, avoiding the surface texture of the dirty layer caused by brushing with a brush. The shade drying operation in S5 is performed by shielding with an opaque shielding cover, and the moisture in the shielding cover is extracted by a dehumidifier, which can avoid the influence of external conditions such as light and humidity on the silicone rubber test piece and reduce the error of experimental results caused by various factors.

[0034] The above description is only a specific embodiment of the present invention, but the technical features of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are included in the patent scope of the present invention.

Claims

1. A high-precision contamination method for a small-area silicone rubber test piece, characterized in that: The following steps are involved: S1: The components of artificial pollution are configured according to the hydrophobicity of the insulator. When the hydrophobicity of the insulator is lost, the artificial pollution includes diatomaceous earth and soluble salt, and the mass ratio of diatomaceous earth to soluble salt is 6:

1. When the insulator has good hydrophobicity, the artificial pollution includes kaolin and soluble salt, and the mass ratio of kaolin to soluble salt is 6:

1. S2: The mass m of artificial pollution is obtained according to the area of ​​the silicone rubber test piece and the required salt density and ash density. The calculation formula is: m=p ESDD / r NSDD ×S; Where: ρ ESDD is the equivalent salt density, ρ NSDD is the equivalent gray density, S is the area of ​​the silicone rubber test piece; The calculated mass m is enlarged N times and weighed into a test tube or / and a measuring cylinder, and water is added to the test tube or / and the measuring cylinder to fully stir and dissolve, and the conductivity of the artificial dirty liquid is not greater than 0.05 S / m at 20°C; S3: evenly coat a layer of dry diatomaceous earth on the silicone rubber test piece, then divide the artificial dirty liquid prepared in S2 into M parts, where: M=N, and drop one of the divided artificial dirty liquids on the treated silicone rubber test piece through a rubber dropper; S4: The silicone rubber test piece treated in S3 is placed on an ultrasonic vibration platform for ultrasonic vibration treatment, and the contamination treatment is performed by the bowstring method during the ultrasonic vibration treatment. The frequency of the ultrasonic wave is 40-60 Hz, the sound pressure intensity is not less than 130 dB, the ultrasonic amplitude is 80% of the maximum amplitude, and the ultrasonic vibration is performed for 50 cycles. The ultrasonic time and interval time of each cycle are 60 s and 5 s respectively, and the contamination speed is 1 m / s; S5: drying the silicone rubber test piece after the treatment in S4 in the shade and performing storage treatment; The specific surface area of ​​diatomaceous earth in S1 is > 10.9 m 2 / g, the total pore volume of diatomite is > 0.037 cm 3 / g, the average pore size of diatomite is >10.9 nm; When S2 is fully stirred and dissolved, water is added twice, and the mass of water added each time is 190-210 ml.

2. A high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The kaolin in S1 is industrial raw material grade kaolin.

3. A high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The soluble salts in S1 include NaCl and CaSO4, and the mass ratio of NaCl to CaSO4 is 1:

4.

4. A high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The mass of S2 after being enlarged N times is weighed by an electronic balance, and N is 50-100.

5. The high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The water in S2 is added into the test tube and / or measuring cylinder through a rubber-tipped dropper, and the mass of water added each time is equal.

6. A high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The diatomaceous earth in S3 is evenly coated on the silicone rubber test piece through a dry sponge mass, and after coating, the excess diatomaceous earth on the surface of the silicone rubber test piece is blown off by an ear cleaning bulb.

7. A high-precision contamination method for a small-area silicone rubber test piece according to claim 1, characterized in that: The bow string method in S4 uses wet cotton thread.