Cathode head of plasma torch and preparation method thereof
By employing a structural design of a cathode core, a hafnium carbide or zirconium carbide transition layer, and a tantalum-hafnium carbon alloy coating on the cathode head of a steam torch, combined with plasma thermal spraying and rapid sintering processes, the problem of short cathode material lifespan was solved, and the ablation resistance and high-temperature resistance of the cathode head were improved.
Patent Information
- Application Number
- CN202011155686.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-10-26
AI Technical Summary
The cathode head of the existing steam torch is made of hafnium metal, and its lifespan is difficult to meet application requirements under 50kW power conditions.
The cathode head adopts an inside-out structure design, including a cathode core, a hafnium carbide or zirconium carbide transition layer, and a tantalum-hafnium carbon alloy coating. It is prepared by plasma thermal spraying and rapid sintering process to form a complete crystal structure, which improves the bonding strength and ablation resistance.
It extends the service life of cathode materials, prevents the coating from peeling off during high-temperature ablation, and improves ablation resistance and high-temperature resistance.
Smart Images

Figure HDA0002742650800000011 
Figure HDA0002742650800000012 
Figure HDA0002742650800000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plasma torches, in particular to a cathode head of a plasma torch. Background Art
[0002] A plasma torch, also known as a plasma spray gun, is a discharge device that can produce a directional "low temperature" (about 2000-20000K) plasma jet. Plasma torches can be divided into four types according to the different forms of the medium: argon torch, nitrogen torch, air torch, and steam torch. Among them, the research on steam torch is relatively less.
[0003] At present, the cathode head of the steam torch is mainly made of metal hafnium. However, the life of metal hafnium as the cathode of the steam torch is difficult to meet its application requirements under the power condition of 50kW.
[0004] Therefore, it is urgent to develop a new cathode head for a plasma torch to extend the life of the cathode material in the plasma torch. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the object of the present invention is to provide a cathode head of a plasma torch, which prolongs the life of the cathode material in the plasma torch.
[0006] In order to achieve the object of the present invention, the technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides a cathode head of a plasma torch, which includes a cathode core, a hafnium carbide or zirconium carbide transition layer, and a tantalum hafnium carbon alloy coating from the inside to the outside; the material of the cathode core is a single metal hafnium or a hafnium alloy.
[0008] Preferably, the thickness of the hafnium carbide or zirconium carbide transition layer is 1-15 μm.
[0009] Preferably, the thickness of the tantalum-hafnium-carbon alloy coating is 10-100 μm.
[0010] In a second aspect, the present invention provides a method for preparing a cathode head of a plasma torch, comprising the following steps:
[0011] (1) Spraying transition layer material hafnium carbide or zirconium carbide on the surface of the cathode core;
[0012] (2) spraying a coating material of tantalum hafnium pentacarbon tetrachloride (Ta4HfC5) onto the surface obtained in step (1);
[0013] (3) Sintering the material obtained in step (2) to completely crystallize the transition layer material and the coating material.
[0014] Preferably, step (1) adopts plasma thermal spraying, the powder feeding gas pressure is 0.65MPa-0.95MPa, and the powder feeding rate is 45g / min-55g / min.
[0015] Preferably, step (2) adopts plasma thermal spraying, the powder feeding gas pressure is 0.55MPa-0.75MPa, and the powder feeding rate is 35g / min-45g / min.
[0016] Furthermore, the sintering temperature in step (3) is 800° C. to 1760° C., and the sintering is stopped when the transition layer and the tantalum-hafnium-carbon alloy coating are completely crystallized.
[0017] Preferably, the sintering temperature is controlled to be 1300° C. to 1450° C., and the sintering time is controlled to be within 30 minutes.
[0018] It should be noted that the cathode core surface described in the aforementioned preparation method of the present invention does not include the contact surface between the cathode core and the base, that is, the contact surface between the cathode core and the base does not need to be sprayed with transition layer material and coating material.
[0019] In a third aspect, the present invention provides a plasma torch, comprising the cathode head described above.
[0020] The raw materials and reagents involved in the present invention are all common commercially available products, and the operations involved are all routine operations in the art unless otherwise specified.
[0021] Based on the common knowledge in this field, the above-mentioned preferred conditions can be combined with each other to obtain a specific implementation method.
[0022] The beneficial effects of the present invention are:
[0023] The invention adopts a tantalum-hafnium-carbon alloy coating to protect the hafnium cathode core, and through a rapid sintering process, the tantalum-hafnium-carbon alloy coating has a complete crystal structure, thereby improving the ablation resistance and high temperature resistance of the plasma torch cathode head, thereby extending the service life of the plasma torch cathode head.
[0024] In the spraying process of the tantalum-hafnium-carbon alloy coating, the present invention further uses hafnium carbide or zirconium carbide as a transition layer for pre-spraying, thereby overcoming the interface stress between the tantalum-hafnium-carbon alloy coating and the hafnium cathode core, solving the problem that the cathode core and the tantalum-hafnium-carbon alloy coating material are prone to cracking due to inconsistent thermal expansion coefficients, and also avoiding the tantalum-hafnium-carbon alloy coating from falling off due to excessive interface stress during ion torch sintering.
[0025] The present invention further controls the crystallization degree of the transition layer by controlling the rate and temperature of thermal spraying, thereby improving the bonding strength between the tantalum-hafnium-carbon alloy coating and the hafnium cathode core, and preventing the external tantalum-hafnium-carbon alloy coating from falling off due to high-temperature ablation of the plasma torch cathode during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 This is a SEM image of the cathode interface morphology of the cathode head prepared by the preparation method of the present invention in the experimental example of the present invention.
[0029] Figure 2 These are SEM images of cathode heads prepared in Comparative Example 1 and Comparative Example 2 in the experimental examples of the present invention; wherein (a) is Comparative Example 1, and (b) is Comparative Example 2.
[0030] Figure 3 This is a comparison result of the cathode material life in the experimental example of the present invention.
[0031] Figure 4 1 and 1 are the transmission electron microscope test results of the alloy cathode hafnium core and the pure hafnium core in the experimental example of the present invention; wherein (a) is alloy hafnium, and (b) is pure metal hafnium. DETAILED DESCRIPTION
[0032] The object of the present invention is to provide a cathode head of a plasma torch, which can prolong the life of the cathode material in the plasma torch.
[0033] The cathode head of the plasma torch provided by the present invention comprises a cathode core, a hafnium carbide or zirconium carbide transition layer, and a tantalum-hafnium-carbon alloy coating from the inside to the outside; the material of the cathode core is metal single substance hafnium or a hafnium alloy.
[0034] The purity of the tantalum-hafnium-carbon alloy of the tantalum-hafnium-carbon alloy coating is greater than 99%, and the purity of the hafnium carbide or zirconium carbide transition layer is greater than 99%.
[0035] In a specific embodiment of the present invention, the thickness of the hafnium carbide or zirconium carbide transition layer is preferably 1 to 15 μm.
[0036] If the thickness of the transition layer is too low, the bonding strength between the tantalum-hafnium-carbon alloy coating and the cathode core cannot be effectively improved, and the effect in extending the service life of the cathode head is limited; if the transition layer is too thick, the transition layer is easy to fall off due to the effect of tension.
[0037] In a specific embodiment of the present invention, the thickness of the tantalum-hafnium-carbon alloy coating is preferably 10-100 μm.
[0038] The present invention further provides a method for preparing a cathode head of a plasma torch, comprising the following steps:
[0039] (1) Spraying transition layer material hafnium carbide or zirconium carbide on the surface of the cathode core;
[0040] (2) spraying a coating material of tantalum hafnium pentacarbon tetrachloride (Ta4HfC5) onto the surface obtained in step (1);
[0041] (3) Sintering the material obtained in step (2) to completely crystallize the transition layer material and the coating material.
[0042] In a specific embodiment of the present invention, the particle size of the hafnium carbide powder is 2 μm to 5 μm, and the particle size of the zirconium carbide powder is 5 μm to 8 μm.
[0043] Furthermore, the spraying process of the transition layer material is specifically as follows: plasma thermal spraying of hafnium carbide or zirconium carbide powder is performed by a thermal spraying machine to obtain a hafnium carbide / zirconium carbide coating, and during the thermal spraying, the current is 600A to 650A and the voltage is 65V to 70V;
[0044] The main gas in the plasma spraying process is argon gas, which is a monatomic gas, easy to start an arc at high frequency, and has good arc maintenance stability. Furthermore, the main gas pressure in the plasma spraying process is controlled to be 0.6MPa~0.8MPa, and the gas flow rate in the spraying process is 40lpm~45lpm;
[0045] The auxiliary gas in the plasma spraying process is hydrogen, which has high dissociation energy and thermal conductivity, low density, and has a positive contribution to arc voltage and arc temperature;
[0046] The powder feeding gas during the plasma spraying process is nitrogen, the powder feeding gas pressure is 0.55MPa-0.75MPa, and the powder feeding rate is 35g / min-45g / min, preferably 40g / min.
[0047] Preferably, the thickness of the hafnium carbide transition layer is less than 10 μm, and the thickness of the zirconium carbide transition layer is less than 15 μm.
[0048] In a specific embodiment of the present invention, the powder particle size of the tantalum hafnium pentoxide is 10 μm to 15 μm.
[0049] Furthermore, the spraying process of the coating material tantalum hafnium pentacarbon tetraoxide is specifically as follows: plasma thermal spraying of tantalum hafnium pentacarbon tetraoxide powder is performed by a thermal spraying machine to obtain a coating, and during the thermal spraying, the current is 630A to 700A and the voltage is 65V to 70V;
[0050] The main gas in the plasma spraying process is argon gas, the main gas pressure is 0.7MPa~0.9MPa, and the gas flow rate during the spraying process is 55lpm~65lpm;
[0051] The auxiliary gas in the plasma spraying process is hydrogen, which has high dissociation energy and thermal conductivity, low density, and has a positive contribution to arc voltage and arc temperature;
[0052] The powder feeding gas during the plasma spraying process is nitrogen, the powder feeding gas pressure is 0.65MPa-0.95MPa, and the powder feeding rate is 45g / min-55g / min, preferably 50g / min.
[0053] During the spraying process, due to the high phase change temperature of tantalum hafnium pentoxide, the thermal spraying temperature cannot completely crystallize the material, so secondary sintering is required to increase the completeness of its crystallization. The increase in the degree of crystallization can improve the bonding strength of the tantalum hafnium carbon alloy coating, thereby extending the service life of the cathode head.
[0054] Specifically, the sprayed cathode material is placed in a rapid sintering furnace for sintering. Since conventional sintering causes serious diffusion between the metal hafnium and the zirconium carbide / hafnium carbide interface, a rapid sintering furnace is needed to ensure the integrity of the interface. The sintering temperature is controlled at 800°C to 1760°C, and the sintering is stopped when the transition layer and the tantalum hafnium carbon alloy coating are completely crystallized. Furthermore, the results of XRD phase testing show that the sintering effect is best in the temperature range of 1300°C to 1450°C, and the sintering time is usually controlled within 30 minutes.
[0055] Since the cathode head needs to be in contact with the copper base for heat dissipation, the contact surface between the cathode core and the copper base does not need to be sprayed with the coating mentioned above in the present invention. The treatment method of this contact surface is the same as the conventional treatment method in the field, and it can be sintered using spark plasma sintering (SPS).
[0056] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0057] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0058] The preferred embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that the following examples are provided only for the purpose of illustration and are not intended to limit the scope of the present invention. Those skilled in the art may make various modifications and substitutions to the present invention without departing from the purpose and spirit of the present invention.
[0059] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0060] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0061] Example 1
[0062] This embodiment is used to illustrate the cathode head of the plasma torch and the preparation method thereof according to the present invention.
[0063] 1. Raw materials
[0064] Hafnium metal cathode core, hafnium carbide, tantalum hafnium pentoxide (Ta4HfC5);
[0065] 2. Preparation method
[0066] (1) using a thermal sprayer to spray hafnium carbide on the surface of the cathode core at a temperature of 1050°C and a thickness of 2.5 μm;
[0067] (2) using a thermal sprayer to spray tantalum hafnium pentacarbon tetraoxide (Ta4HfC5) onto the surface obtained in step (1), the spraying condition is 1430° C., and the spraying thickness is 80 μm;
[0068] (3) After spraying, the sample was placed in a high-temperature gas sintering furnace for sintering at an average heating rate of 50°C / min to 1430°C and sintered for 60 minutes. Inert gas was introduced during the entire process to allow the transition layer material and the coating material to completely crystallize. The sample was then cooled to room temperature at a cooling rate of 30°C / min.
[0069] Example 2
[0070] This embodiment is used to illustrate the cathode head of the plasma torch and the preparation method thereof according to the present invention.
[0071] 1. Raw materials
[0072] Hafnium alloy cathode core, zirconium carbide, tantalum hafnium pentoxide (Ta4HfC5);
[0073] 2. Preparation method
[0074] (1) Spraying zirconium carbide on the surface of the cathode core using a thermal spraying machine at a spraying condition of 1200°C and a spraying thickness of 2 μm;
[0075] (2) using a thermal sprayer to spray tantalum hafnium pentacarbon tetraoxide (Ta4HfC5) onto the surface obtained in step (1), the spraying condition is 1430° C., and the spraying thickness is 80 μm;
[0076] (3) After spraying, the material is placed in a high-temperature gas sintering furnace for sintering at an average heating rate of 50°C / min to 1350°C and sintered for 75 minutes to allow the transition layer material and the coating material to be completely crystallized, and then cooled to room temperature at a cooling rate of 30°C / min.
[0077] Example 3
[0078] The difference between this embodiment and embodiment 1 is that a hafnium alloy cathode core is used to replace the metal hafnium cathode core.
[0079] Example 4
[0080] The difference between this embodiment and embodiment 2 is that a metal hafnium cathode core is used to replace the hafnium alloy cathode core.
[0081] Comparative Example 1
[0082] 1. Raw materials: metal hafnium cathode core, hafnium carbide;
[0083] 2. Preparation method
[0084] (1) using a thermal sprayer to spray hafnium carbide on the surface of the cathode core at a temperature of 1050°C and a thickness of 2.5 μm;
[0085] (2) After spraying, the coating was placed in a high-temperature gas sintering furnace for sintering at a heating rate of 50°C / min to 1050°C for 30 minutes to allow the coating material to completely crystallize, and then cooled to room temperature at a cooling rate of 30°C / min.
[0086] Comparative Example 2
[0087] 1. Raw materials
[0088] Hafnium metal cathode core, tantalum hafnium pentoxide (Ta4HfC5);
[0089] 2. Preparation method
[0090] (1) A thermal spraying machine is used to spray tantalum hafnium pentacarbon tetraoxide on the surface of the cathode core at a spraying temperature of 1430°C and a spraying thickness of 80 μm;
[0091] (2) After spraying, the coating was placed in a high-temperature sintering furnace for sintering at a heating rate of 50°C / min to 1430°C and sintered for 80 minutes to allow the coating material to completely crystallize, and then cooled to room temperature at a cooling rate of 30°C / min.
[0092] Experimental example
[0093] 1. Detection object
[0094] Cathode heads and pure metal hafnium cathode cores (without coating) prepared in Example 1, Example 4 and Comparative Examples 1-2.
[0095] 2. Detection method
[0096] 2.1 Bonding between cathode core, transition layer and tantalum-hafnium-carbon alloy coating
[0097] The cross section of the cathode head is observed by SEM scanning to check whether there are defects in the bonding between the cathode core, the transition layer and the tantalum-hafnium-carbon alloy coating.
[0098] 2.2 Cathode material life
[0099] A metal hafnium cathode core (cathode material) with a length of 10 mm and a diameter of 5.5 mm was tested. The cathode heads prepared in Example 1 and Example 4 and a pure metal hafnium cathode core were tested on a plasma steam torch with a power of 50 kW. The cathode core ablation time (all 10 mm length was burned out) was used to characterize the life of the cathode material.
[0100] 2.3 Transmission electron microscopy test
[0101] The microstructure of the alloy cathode hafnium core and the pure hafnium core was verified by transmission electron microscopy.
[0102] 3. Test results
[0103] 3.1 Scanning electron microscopy
[0104] The SEM images of the cathode heads prepared in Example 1 and Example 4 are similar and have no significant difference. Figure 1 It can be seen that the cathode core of the cathode head prepared by the preparation method of the present invention is completely bonded to the transition layer, and the transition layer is also completely bonded to the tantalum-hafnium-carbon alloy coating without defects.
[0105] The cathode interface morphology of the cathode head prepared in Comparative Example 1 detected by SEM is as follows: Figure 2 As shown in (a), the metal hafnium is relatively completely bonded to the transition layer with almost no defects.
[0106] The cathode interface morphology of the cathode head prepared in Comparative Example 2 detected by SEM is as follows: Figure 2 As shown in (b), there is a protruding part in the cross section of the direct bonding between metal hafnium and tantalum hafnium pentoxide, which will accelerate the melting of the material during the ablation process.
[0107] 3.2 Cathode material life
[0108] Test results see Figure 3The life of the water vapor ion torch of the cathode head made of pure hafnium material is 168 hours, the life of comparative example 1 is 172 hours, the life of comparative example 2 is 162 hours, and the life of metal hafnium / hafnium carbide / tetratantalum hafnium carbide (Example 1) and metal hafnium / zirconium carbide / tetratantalum hafnium carbide (Example 4) are both more than 280 hours. It can be seen that the coating can greatly improve the life of the cathode material.
[0109] 3.3 Transmission electron microscopy
[0110] The comparison results of the hafnium alloy cathode core and the metal hafnium cathode core used in Examples 1 and 4 are shown in FIG. Figure 4 (a) and (b) show that the crystal structure of the hafnium alloy is relatively complex and the lattice constant is relatively small. In comparison, the lattice constant of pure hafnium is relatively large, and its structure is conducive to heat conduction and has better heat dissipation performance, thereby indirectly improving its performance.
[0111] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A cathode head of a plasma torch, characterized in that: The cathode head comprises a cathode core, a hafnium carbide or zirconium carbide transition layer, and a tantalum-hafnium-carbon alloy coating from the inside to the outside; The material of the cathode core is metal element hafnium or hafnium alloy; The thickness of the hafnium carbide or zirconium carbide transition layer is 1-15 μm; The thickness of the tantalum-hafnium-carbon alloy coating is 10-100 μm.
2. A method for preparing a cathode head of a plasma torch, characterized in that: The steps include: (1) Spraying transition layer material hafnium carbide or zirconium carbide on the surface of the cathode core; (2) spraying a coating material of tetratantalum hafnium carbide onto the surface obtained in step (1); (3) sintering the material obtained in step (2) to completely crystallize the transition layer material and the coating material; The material of the cathode core is metal element hafnium or hafnium alloy; The thickness of the hafnium carbide or zirconium carbide transition layer formed by spraying in step (1) is 1-15 μm.
3. The preparation method according to claim 2, characterized in that: Step (1) uses plasma thermal spraying, the powder feeding gas pressure is 0.55MPa~0.75MPa, and the powder feeding rate is 35g / min~45g / min.
4. The preparation method according to claim 2, characterized in that: Step (2) uses plasma thermal spraying, the powder feeding gas pressure is 0.65MPa~0.95MPa, and the powder feeding rate is 45g / min~55g / min.
5. The preparation method according to claim 4, characterized in that: The sintering temperature in step (3) is 800°C to 1760°C, and the sintering is stopped when the transition layer and the tantalum-hafnium-carbon alloy coating are completely crystallized.
6. The preparation method according to claim 5, characterized in that: The sintering temperature is 1300℃~1450℃.
7. The preparation method according to any one of claims 2 to 6, characterized in that The cathode core surface does not include the contact surface between the cathode core and the base.
8. A plasma torch, characterized in that: Comprising the cathode head as claimed in claim 1.