Method for preparing large-size single-layer nanosheet by intercalating and stripping layered oxide in one step
Through the organic amine solution intercalation peeling technology, the problems of uneven thickness distribution and high preparation cost of nanosheets were solved, and high-quality large-size single-layer nanosheets were obtained, which were suitable for the peeling of traditional layered oxides and improved nanomaterials application potential.
Patent Information
- Application Number
- CN202411182849.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the prior art, when preparing large-size single-layer nanosheets, the thickness distribution is wide and the lateral size is small. The traditional liquid-phase peeling method requires multiple steps and strong acid treatment, resulting in high production cost and limited application of nanosheets.
The intercalation of layered oxides is peeled off by organic amine solution, and the cationic coordination intercalation layer between the amine-containing organic molecules and the layered oxide layer is then washed in ethanol solvent and oscillated in deionized water to obtain high Large-size single-layer nanosheets of mass.
The nanosheets are significantly increased lateral dimensions, avoid structural defects and stress fractures, improve the operability and mechanical strength of nanomaterials, simplify the preparation process, and reduce costs.
Smart Images

Figure CN119059553A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanosheet materials, and in particular relates to a method for preparing large-size single-layer nanosheets by realizing intercalation and exfoliation of layered oxides in one step. Background Art
[0002] Large-size (ratio of nanosheet diameter to thickness) two-dimensional (2D) nanosheets have always been one of the research focuses in the field of materials. These materials have a thickness of nm and a lateral size of μm. The direct liquid phase exfoliation method is usually used to completely exfoliate layered materials to obtain single-layer nanosheets, but this method will result in a wide distribution of nanosheet thickness and a small lateral size, and the basal surface of the obtained nanosheets may be greatly changed. So far, a small number of layered materials have been shown to spontaneously exfoliate to obtain single-layer nanosheets when immersed in an appropriate suspension medium. This thermodynamically driven exfoliation process is limited to the charged layer and is similar to the dissolution process of salt. Since the bonding between layers in layered materials is highly anisotropic (resulting in their sheet-like morphology), the dissolution is limited to the stacking direction of the charged layers, so this type of layered materials is also named "one-dimensional (1D) dissolution" materials. Other materials such as antimony phosphate, 2:1 type clay minerals, mullite or limonite type of titanate, layered perovskites, etc. are all such spontaneously exfoliated layered materials.
[0003] The existing technology for preparing titanate nanosheets by spontaneous 1D dissolution mainly involves exfoliation in a two-step process using liquid phase exfoliation to obtain nanosheets. 0.8 Ti 1.73 Li 0.27 O 4 For example, the precursor synthesis preparation needs to be obtained by solid phase reaction at 1100 ° C. The potassium ions between the layers are repeatedly treated with strong acid HCl to exchange with hydrogen ions, making the base surface acidic. At the same time, the lithium ions in the structure are completely leached out, and the layer structure (H 1.07 Ti 1.73 O 4 ·H 2 O) due to the release of lithium ions. Subsequently, the acidified protonated titanate solution is mixed with an aqueous tetraalkylammonium hydroxide solution, such as tetrabutylammonium hydroxide (TBAOH). The introduction of a strong base not only provides a higher charge density, but also makes the bulky cation (TBA + ) diffuses fully between the layers, exceeding the threshold for the onset of 1D dissolution. By adjusting the acidification time and different oscillation modes, Ti with adjustable lateral size can be obtained. 0.87 O 2 -Nanosheets.
[0004] The current method of preparing nanosheets by ultrasonic treatment cannot provide fine size and structure control, which will inevitably lead to a wide thickness distribution and flake fracture of the obtained nanosheets, so the maximum aspect ratio inherent in the diameter of the original flakes cannot be achieved. The nanosheets obtained by traditional liquid phase exfoliation need to be further processed before they can be implemented in some applications, such as the formation of heterostructures, permeation-selective microporous membranes, textured (barrier) membranes or composite materials, which require nanosheets of uniform thickness and larger size. However, the current liquid phase exfoliation method has a long preparation cycle and usually involves the step of ion replacement using hydrochloric acid or other strong acids. The resulting waste acid treatment costs further increase the preparation cost of nanosheets. Summary of the invention
[0005] The present invention aims to solve the technical problems mentioned in the background technology, and provides a method for preparing large-sized single-layer nanosheets by intercalation stripping of layered oxides in one step. The main principle is that organic molecules containing amine groups in an organic amine solution are coordinated and intercalated with cations (such as sodium, potassium ions, etc.) between layered oxide layers. The layered material after intercalation of the organic molecules containing amine groups is washed with an ethanol solvent, excess organic solution is removed, and it is redispersed in deionized water, and then high-quality and large-sized nanosheets are obtained by sufficient shaking, shaking, and centrifugation. The present invention uses an organic amine solution as an intercalation solvent, the intercalation reaction efficiency is high, the reaction pathway is relatively mild, the lattice defects caused by the ion escape in the structure are avoided during the stripping process, and the stress-induced fracture during the stripping process is also suppressed, thereby obtaining a nanosheet with a significantly increased lateral size, which greatly improves the operability of the application of nanomaterials.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing large-sized single-layer nanosheets by intercalation exfoliation of layered oxides in one step comprises mixing layered oxides with organic amine solutions to obtain layered oxides with organic amine intercalation and increased interlayer spacing, washing to remove excess organic amine solution, dispersing the layered oxides in deionized water, and oscillating to obtain large-sized single-layer nanosheet dispersions.
[0008] Furthermore, the excess organic amine solution is removed by washing with ethanol; and the shaking is performed on a shaker in order to evenly disperse the large-sized single-layer nanosheets in the deionized water.
[0009] In the method for preparing large-sized single-layer nanosheets of the present invention, a layered oxide is fully mixed with an organic amine solution, a large number of organic molecules containing amine groups are coordinated and intercalated with metal cations between the layered oxide layers to obtain an organic amine-intercalated layered oxide with an increased interlayer spacing, the excess organic amine solution is removed by washing with ethanol, and then the layered oxide is dispersed in deionized water and fully shaken on a shaker to obtain a large-sized single-layer nanosheet dispersion.
[0010] Furthermore, the initial lateral size of the layered oxide is 100-150 μm.
[0011] Furthermore, the layered oxide is a titanium-based oxide or a cobalt-manganese-based oxide, for example, the layered oxide is K 0.8 Ti 1.73 Li 0.27 O 4 or NaCoMnO.
[0012] Furthermore, the organic amine in the organic amine solution is ethylenediamine hydrochloride, ifosfamide, ethyl carbamate or N-methylmethylamine.
[0013] Furthermore, the concentration of the organic amine solution is 0.5-5 mol / L.
[0014] Furthermore, during the coordination intercalation process, the organic amine solution is replaced every 12-48 hours. Each time the organic amine solution is replaced, the mixture is centrifuged at 10,000 rpm for 10 minutes, the supernatant is removed, and then the organic amine solution is added again.
[0015] Furthermore, the oscillation time is 1-7 days.
[0016] Furthermore, the oscillation time is 7 days.
[0017] Furthermore, the concentration of the large-size single-layer nanosheet dispersion is 0.5-2 mg / mL.
[0018] Furthermore, the large-sized single-layer nanosheet has a lateral size of 10-20 μm and a thickness of 5-10 nm.
[0019] Compared with the prior art, the present invention has the following advantages and technical effects:
[0020] The method of directly coordinating and intercalating the stripping of the nanosheets by the organic molecules containing amine groups is superior to the existing stripping technology. The conventional liquid phase stripping method is usually used, and the nanosheets obtained by adding tetrabutylammonium hydroxide (TBAOH) for two-step stripping have a diameter of 3 μm. The nanosheets obtained by the present invention can maintain a complete crystal structure under a mild stripping process without defects, and thus have higher mechanical strength, so that the diameter of the nanosheets is significantly increased, and oxide nanosheets with a lateral size of 10-20 μm are obtained. The method of the present invention is suitable for the stripping of conventional layered oxides such as titanium oxide and cobalt-manganese-based oxides. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 is K in Example 1 0.8 Ti 1.73 Li 0.27 O 4 SEM images of the precursor;
[0023] Figure 2 This is a scanning electron microscope image of the large-sized single-layer nanosheet after peeling in Example 1;
[0024] Figure 3 is dispersed in ethylenediamine hydrochloride solution (H 3 O) 0.2 EDA 0.6 Ti 1.73 Li 0.27 O 4 Optical image of nanosheets (i.e., nanosheets after exfoliation) in solution;
[0025] Figure 4 This is a transmission electron microscope image of the large-sized single-layer nanosheet obtained by peeling in Example 1;
[0026] Figure 5 is Na in Example 2 0.6 Mn 0.6 Co 0.4 O 2 SEM images of the precursor;
[0027] Figure 6 This is a scanning electron microscope image of the large-sized single-layer nanosheet after peeling in Example 2;
[0028] Figure 7 This is a transmission electron microscopy image of the large-sized single-layer nanosheet obtained by peeling in Example 2. DETAILED DESCRIPTION
[0029] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0030] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0031] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0032] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0033] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0034] Unless otherwise specified, the room temperature in the embodiments of the present invention is 25±2°C.
[0035] All raw materials used in the examples of the present invention are commercially available.
[0036] An embodiment of the present invention provides a method for preparing large-sized single-layer nanosheets by intercalation exfoliation of layered oxides in one step, wherein the layered oxides are mixed with an organic amine solution to obtain a layered oxide with an increased interlayer spacing and coordinated intercalation of amine-containing organic molecules, the excess organic amine solution is washed to remove, and the layered oxides are dispersed in deionized water and shaken to obtain a large-sized single-layer nanosheet dispersion.
[0037] In some embodiments of the present invention, the excess organic amine solution is removed by washing with ethanol; and the shaking is performed on a shaker in order to evenly disperse the large-sized single-layer nanosheets in the deionized water.
[0038] In the method for preparing large-sized single-layer nanosheets of the present invention, a layered oxide is fully mixed with an organic amine solution, a large number of organic molecules containing amine groups are coordinated and intercalated with metal cations between the layered oxide layers to obtain an organic amine-intercalated layered oxide with an increased interlayer spacing, the excess organic amine solution is removed by washing with ethanol, and then the layered oxide is dispersed in deionized water and fully shaken on a shaker to obtain a large-sized single-layer nanosheet dispersion.
[0039] In some embodiments of the present invention, the initial lateral size of the layered oxide is 100-150 μm.
[0040] In some embodiments of the present invention, the layered oxide is a titanium-based oxide or a cobalt-manganese-based oxide. For example, the layered oxide is K 0.8 Ti 1.73 Li 0.27 O 4 or NaCoMnO.
[0041] In some embodiments of the present invention, the organic amine in the organic amine solution is ethylenediamine hydrochloride, ifosfamide, ethyl carbamate, N-methyl methylamine. In some embodiments of the present invention, the concentration of the organic amine solution is 0.5-5 mol / L (0.5-5M), for example, the concentration of the organic amine solution can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 3 mol / L, 4 mol / L or 5 mol / L.
[0042] In some embodiments of the present invention, during the coordination intercalation process, the organic amine solution is replaced every 12-48 hours. Each time the organic amine solution is replaced, the mixture is centrifuged at 10,000 rpm for 10 minutes, the supernatant is removed, and then the organic amine solution is added again.
[0043] In some embodiments of the present invention, the oscillation time is 1-7 days, for example, the oscillation time can be 1 day, 1.5 days, 2 days, 3 days, 4 days, 5 days, 6 days, 7 days, and preferably the oscillation time is 7 days.
[0044] In some embodiments of the present invention, the concentration of the large-sized single-layer nanosheet dispersion is 0.5-2 mg / mL.
[0045] In some embodiments of the present invention, the large-sized single-layer nanosheet has a lateral size of 10-20 μm and a thickness of 5-10 nm.
[0046] The technical solution of the present invention is further illustrated by the following embodiments.
[0047] In the following examples, K 0.8 Ti 1.73 Li 0.27 O 4 The preparation method of the precursor is as follows: potassium carbonate, titanium dioxide and lithium oxide powder are mixed and ground evenly in proportion, and then heated to 1100°C in air in a muffle furnace for 20 hours. After annealing, K with a lateral size of 100 μm is obtained. 0.8 Ti 1.73 Li 0.27 O 4 Precursor. Extending the heating time to 48h, after annealing, K with a lateral size of 150μm can be obtained. 0.8 Ti 1.73 Li 0.27 O4 Precursor.
[0048] Example 1
[0049] 500 mg K 0.8 Ti 1.73 Li 0.27 O 4 The precursor (initial lateral size of 150 μm) was dispersed in 50 mL of 1 M ethylenediamine hydrochloride solution and stirred at room temperature for 72 h to obtain a layered (H 3 O) 0.2 EDA 0.6 Ti 1.73 Li 0.27 O 4 The material was prepared by replacing the ethylenediamine hydrochloride solution every 24 hours, centrifuging at 10000 rpm for 10 minutes, removing the supernatant, re-adding the ethylenediamine hydrochloride solution, and repeating the subsequent operation to obtain a sample after the organic molecule containing an amine group was intercalated and coordinated;
[0050] The sample after coordination and intercalation of the amine-containing organic molecules was washed twice with ethanol to remove excess ethylenediamine hydrochloride solution, 100 mL of deionized water was added to 100 mg of the sample after coordination and intercalation of the amine-containing organic molecules, and the mixture was shaken in a shaker for 1 week (7 days) to obtain a large-size single-layer nanosheet dispersion (concentration of 1 mg / mL) after complete exfoliation. The nanosheet had a lateral size of 20 μm and a thickness of 5 nm.
[0051] Figure 1 is K in Example 1 0.8 Ti 1.73 Li 0.27 O 4 The SEM image of the precursor shows that the precursor has a distinct layered structure with a size of 150 μm;
[0052] Figure 3 is dispersed in aqueous solution (H 3 O) 0.2 EDA 0.6 Ti 1.73 Li 0.27 O 4 The optical image of the nanosheet solution (i.e., nanosheet after exfoliation) shows that the nanosheet has a good dispersion and exfoliation effect;
[0053] Figure 2 This is a scanning electron microscope image of the large-sized single-layer nanosheet after peeling in Example 1. Figure 4 This is a transmission electron microscope image of the large-sized single-layer nanosheet obtained by peeling in Example 1. It can be seen that the thickness of the single-layer nanosheet is at the nanometer level and the peeling effect is good.
[0054] Example 2
[0055] Na 0.6 Mn 0.6 Co 0.4 O 2 The synthesis method is as follows: Mn(CH 3 COO 2 ·4H 2 O、Co(CH 3 COO 2 ·4H 2 O and NaNO 3 The precipitate was dissolved in pure water according to the stoichiometric ratio (0.6:0.4:0.6) and dried on a hot plate at 130°C overnight. The precipitate was annealed at 300°C in air for 20 hours, and then heated at 750°C in air for 20 hours. After annealing, Na 0.6 Mn 0.6 Co 0.4 O 2 powder.
[0056] 500 mg Na 0.6 Mn 0.6 Co 0.4 O 2 (initial lateral size of 100 μm) was dispersed in 50 mL of 1 M N-ethylenediamine hydrochloride solution and stirred at room temperature for 72 h to obtain a layered (H 3 O) 0.2 EDA 0.6 Co 0.8 Mn 1.2 O 4 The material was prepared by replacing the ethylenediamine hydrochloride solution every 12 hours, centrifuging at 10000 rpm for 10 minutes, removing the supernatant, re-adding the ethylenediamine hydrochloride solution, and repeating the subsequent operation to obtain a sample after coordination and intercalation of an organic molecule containing an amine group;
[0057] The sample after coordination and intercalation of the amine-containing organic molecule was washed twice with ethanol to remove the excess ethylenediamine hydrochloride solution. 50 mL of deionized water was added to 100 mg of the sample after coordination and intercalation of the amine-containing organic molecule, and the sample was shaken in a shaker for 4 days to obtain a large-sized single-layer nanosheet (Co 0.4 Mn 0.6 O 2 ) dispersion (concentration is 2 mg / mL), the lateral size of the nanosheets is 12 μm and the thickness is 5 nm.
[0058] Figure 5 is Na in Example 2 0.6 Mn 0.6 Co 0.4 O 2The SEM image of the precursor shows that the precursor has an obvious layered structure with a size of 100 μm;
[0059] Figure 6 This is a scanning electron microscope image of the large-sized single-layer nanosheet after peeling in Example 2. It can be seen that the lateral size of the precursor is 12 μm.
[0060] Figure 7 This is a transmission electron microscope image of the large-sized single-layer nanosheet obtained by peeling in Example 2. It can be seen that the thickness of the single-layer nanosheet is at the nanometer level and the peeling effect is good.
[0061] Example 3
[0062] The same as Example 1, except that the 1M ethylenediamine hydrochloride solution is replaced by 2M ifosfamide, and the nanosheet after peeling has a lateral size of 15 μm and a thickness of 10 nm.
[0063] Example 4
[0064] 500 mg K 0.8 Ti 1.73 Li 0.27 O 4 (initial lateral dimension is 100 μm) dispersed in 50 mL 1 M urethane solution, stirred at room temperature for 96 h, and replaced to obtain a layered material coordinated by an organic molecule containing an amino group. The urethane solution was replaced every 48 h, centrifuged at 10000 rpm for 10 minutes, the supernatant was removed, and the urethane solution was added again;
[0065] The sample after coordination and intercalation of the amine-containing organic molecules was washed twice with ethanol to remove excess ethyl formate solution, 50 mL of deionized water was added to 100 mg of the sample after coordination and intercalation of the amine-containing organic molecules, and the mixture was shaken in a shaker for 3 days to obtain a large-size single-layer nanosheet dispersion (concentration of 2 mg / mL) after complete exfoliation. The nanosheet had a lateral size of 10 μm and a thickness of 5 nm.
[0066] Example 5
[0067] 500 mg K 0.8 Ti 1.73 Li 0.27 O 4 (initial lateral dimension is 100 μm) dispersed in 50 mL of 0.5 M N-methylamine solution, stirred at room temperature for 72 h, replaced to obtain amine-containing molecular coordination layered material, replaced N-methylamine solution every 48 h, centrifuged at 10000 rpm for 10 min, removed the supernatant, and re-added N-methylamine solution;
[0068] The sample after coordination and intercalation of the amine-containing organic molecules was washed twice with ethanol to remove excess N-methylamine solution, and 200 mL of deionized water was added to 100 mg of the sample after coordination and intercalation of the amine-containing organic molecules. The sample was shaken in a shaker for 1 day to obtain a large-size single-layer nanosheet dispersion (concentration of 0.5 mg / mL) after complete exfoliation. The nanosheet had a lateral size of 10 μm and a thickness of 10 nm.
[0069] Example 6
[0070] The same as Example 1, except that the concentration of the ethylenediamine hydrochloride solution is 2M. At this time, the organic molecules containing amine groups are coordinated and intercalated with the metal cations between the layered oxide layers. The lateral size of the nanosheets in this example is 15 μm and the thickness is 10 nm.
[0071] Example 7
[0072] The same as Example 1, except that the concentration of the ethylenediamine hydrochloride solution is 5M. At this time, the organic molecules containing amine groups are coordinated and intercalated with the metal cations between the layered oxide layers. The lateral size of the nanosheets in this example is 10 μm and the thickness is 10 nm.
[0073] Example 8
[0074] The same as Example 1, except that the concentration of the ethylenediamine hydrochloride solution is 0.5M. At this time, the organic molecules containing amine groups are coordinated and intercalated with the metal cations between the layered oxide layers. The lateral size of the nanosheets in this example is 15 μm and the thickness is 5 nm.
[0075] Comparative Example 1 Traditional method (method of patent CN 113443655 A)
[0076] K 2 CO 3 , Li 2 CO 3 and TiO 2 The mixture was ground and mixed at a molar ratio of 0.4:0.14:1.73, placed in a Pt crucible, decarburized at 800°C for 1 hour, and ground again for 30 minutes after cooling. Finally, the sample was calcined at 1100°C in a Pt crucible for 1 week to prepare the flaky calcium-type layered titanate K 0.8 Ti 1.73 Li 0.27 O 4 Then add 1 mol / L hydrochloric acid, mix and stir, and the proton exchange time is 2 days to obtain acidified H 1.07 Ti 1.73 O 4 ·H 2O. By calculating the concentration of H ions in the acidified sample, adding a tetrabutylammonium hydroxide solution of equal concentration, shaking it in a shaker for one week, the H ions bound to the interlayer are fully neutralized to obtain a single-layer nanosheet dispersion, in which the lateral size of the nanosheet is only 3μm and the thickness is 1-5nm.
[0077] It can be seen that the conventional tetrabutylammonium hydroxide liquid phase exfoliation method involves acidified ion exchange and tetrabutylammonium hydroxide solution treatment, and the aspect ratio of the obtained nanosheets is much smaller than that obtained by the present invention. At the same time, the cost of waste acid treatment increases the preparation cost of the nanosheets, and the steps are cumbersome, which hinders the subsequent application of the nanosheets.
[0078] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides, characterized in that: The layered oxide is mixed with an organic amine solution to obtain an organic amine intercalated layered oxide with increased interlayer spacing, and the excess organic amine solution is washed away, and then the layered oxide is dispersed in deionized water and shaken to obtain a large-size single-layer nanosheet dispersion.
2. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 1, characterized in that: The initial lateral dimensions of the layered oxide are 100-150 μm.
3. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 2, characterized in that: The layered oxide is a titanium-based oxide or a cobalt-manganese-based oxide.
4. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 1, characterized in that: The organic amine in the organic amine solution is ethylenediamine hydrochloride, ifosfamide, ethyl carbamate or N-methylmethylamine.
5. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 1, characterized in that: The concentration of the organic amine solution is 0.5-5 mol / L.
6. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 1, characterized in that: The shaking time is 1-7 days.
7. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 6, characterized in that: The shaking period was 7 days.
8. The method for preparing large-sized single-layer nanosheets by one-step intercalation and exfoliation of layered oxides according to claim 1, characterized in that: The large-size single-layer nanosheet has a lateral size of 10-20 μm and a thickness of 5-10 nm.
Citation Information
Patent Citations
Method of preparing graphene powder
CN103922331A
Environment-friendly synthesis method of two-dimensional transition metal carbide or nitride nanosheets
CN106744732A
Three-dimensional porous titanium dioxide foam block body and preparation method thereof
CN108855017A
Self-supporting flexible super-hydrophilic titanium oxide film and preparation method thereof
CN108864463A
Preparation method of nano titanium oxide nanosheet and wood surface treatment process
CN114804196A