A deep eutectic solvent-based electrolyte and its application
By developing eutectic solvent-based electrolytes and using the combination of polynitrile monomers and metal salts, the thermal response self-polymerization of lithium-ion batteries under high temperature conditions is achieved, and the problem of thermal runaway in lithium-ion batteries is solved, which is significantly Improves battery safety and cycling performance.
Patent Information
- Application Number
- CN202110123744.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Existing lithium-ion batteries are prone to thermal runaway in high temperatures or extreme conditions, resulting in fire, combustion and explosion, which poses serious safety hazards. The existing thermal blocking measures have a great impact on the room temperature ionic conductivity and electrochemical performance of the battery. , it is difficult to effectively block the reaction of high-temperature batteries at room temperature.
A low-eutectic solvent-based electrolyte was developed. By combining polynitrile monomers, ionically polymerizable monomers and metal salts, an eutectic solvent-based electrolyte with thermally responsive self-polymerization and thermal runaway control was prepared, and the room temperature ion was ionized. The conductivity is 1×10-5S/cm-9×10-3S/cm, and the electrochemical window is greater than 4.4V. It can initiate the polymerization of the precursor under high temperature conditions to form a high polymer, increasing the battery impedance to block the battery reaction.
It significantly improves the safety and circulation performance of the secondary battery, can effectively prevent the occurrence of thermal runaway under high temperature conditions, improves the safety and reliability of the battery, and is suitable for various secondary battery applications.
Smart Images

Figure CN114512719B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a low eutectic solvent-based electrolyte, in particular to a low eutectic solvent-based electrolyte, a thermally responsive self-polymerizing low eutectic solvent-based electrolyte for preventing thermal runaway, and applications thereof in forming secondary batteries. Background Art
[0002] In addition to meeting the requirements of long driving range and high-power charging and discharging, safety performance is equally important for power lithium-ion batteries used in electric vehicles. However, when lithium-ion batteries based on conventional carbonate-based liquid electrolytes are abused, short-circuited, used at high temperatures or in extreme conditions, a large amount of heat will be released in a short period of time inside the battery, which will then ignite the organic electrolyte, eventually causing many major safety hazards such as battery fire, combustion, and even explosion. Even the Tesla electric car in the United States, which is currently considered the safest, has experienced many safety accidents such as electric car fire, combustion, and explosion in just a few years, despite the use of complex battery management systems and safety protection measures. Undoubtedly, the safety hazards of the above-mentioned lithium batteries will pose a great threat to the personal and life safety of consumers, and will ultimately affect the rapid promotion and application of electric vehicles. Not only electric vehicles, but also mobile smart devices such as smart phones and laptops that use liquid lithium-ion batteries still have the major safety hazards mentioned above. Therefore, improving the safety of lithium batteries has become a major key issue of concern to the scientific research and industry communities.
[0003] In order to significantly improve and effectively solve the safety hazards of existing lithium batteries, people usually adopt various strategies to improve the safety characteristics of lithium-ion batteries: 1. Improve the high-temperature dimensional thermal stability of the diaphragm through ceramic coating to avoid internal short circuit caused by the contact between the positive and negative electrodes due to thermal shrinkage of the diaphragm, thereby slowing down or avoiding the thermal runaway reaction; 2. Coat the diaphragm with a polymer that only melts at a specific temperature, and use the melting of the polymer to block the lithium ion transmission channel between the positive and negative electrodes inside the battery, thereby effectively avoiding thermal runaway of the lithium battery. The above two treatment methods can improve the safety of lithium batteries to a certain extent, but their shortcomings are also obvious. Both of them are to treat or modify the lithium-ion battery diaphragm, so they cannot effectively inhibit the occurrence of heat generation reactions inside lithium-ion batteries and the continuous deterioration of performance from the source of liquid electrolyte. In fact, when the internal temperature of the lithium battery continues to rise, it will even intensify this heat generation reaction, making the lithium-ion battery more prone to combustion or explosion within a certain period of time. In addition to the diaphragm level, researchers have also conducted some research on the thermal blocking strategy of lithium batteries at the binder level: one type is to melt a low-melting point polymer to form a barrier to produce a blocking effect; the other type is to form a polymer that increases the battery impedance to block electronic conduction and produce a blocking effect. At this stage, polymers that increase battery impedance usually use polybiphenyl, polycyclohexylbenzene, polydifluorobiphenyl, polypyrrole, polythiophene, polyaniline, phenylene and polyphenylene vinyl. CN107749480A discloses a lithium-ion battery with a safe structure and thermal blocking characteristics; when the temperature of the battery exceeds 90°C, the adhesive melts, blocking the electrode active material from reacting with the electrolyte inside the pores, timely blocking the thermal runaway reaction, and improving the thermal stability of the battery. The binder is composed of two or more components of polyvinylidene fluoride, styrene-butadiene rubber, polyethylene wax, polypropylene wax, polymethyl methacrylate, homopolyoxymethylene and polyphenylene ether. However, during high temperature testing, battery expansion occurs. At the same time, CN108470947A discloses a lithium battery electrolyte with added thermal blocking additives, which can cover the surface of the diaphragm when overcharge occurs, forming a dense barrier layer, hindering the overcharge reaction. It is not only resistant to overcharge, but also has little effect on normal charge and discharge behavior. However, its disadvantages are that the amount added is large, and the voltage needs to reach a high level (5.5V) to completely block the circuit, which greatly limits its practical application.
[0004] The above-mentioned thermal blocking is to block the lithium battery by adding polymers, but from a practical point of view, there are still many problems to be solved: the addition of polymers has a negative impact on the room temperature ionic conductivity of the electrolyte, thereby weakening its electrochemical performance at room temperature, and the polymer cannot completely block the reaction between batteries, and cannot form a timely and effective blockade for high-temperature batteries. Therefore, this type of electrolyte system is only suitable for working under low current conditions, and it is difficult to be applied in lithium batteries working at room temperature. Therefore, the electrolyte, as the ion migration medium inside the lithium-ion battery, has become a key research object for improving the safety of lithium-ion batteries.
[0005] Low eutectic solvents are completely different from carbonate solvents used in traditional liquid electrolytes. They were first proposed by Abbott et al. in 2003. At present, most low eutectic solvents are obtained by mixing hydrogen bond acceptors (such as quaternary ammonium salts, quaternary phosphonium salts, imidazole salts, etc.) and hydrogen bond donors (such as amides, carboxylic acids and polyols, etc.). The physicochemical properties of low eutectic solvents are very similar to those of ionic liquids, so some people classify it as a new type of ionic liquid or quasi-ionic liquid. At the same time, low eutectic solvents have great solubility with metal lithium salts, wide electrochemical window, high boiling point, non-volatility and other characteristics. It is a very potential electrolyte solvent system and is currently attracting much attention. Low eutectic solvents have been studied and applied to a certain extent in the field of electrochemistry. CN110120543A invented a low eutectic solvent, electrolyte and flow battery for liquid flow batteries. The low eutectic solvent is prepared by mixing a hydrogen bond acceptor and a hydrogen bond donor (a mixed solution of ethylene carbonate (EC) and dimethyl carbonate (DMC)) in a molar ratio of 1:2, heating the reaction, and adding one or more of the following additives; it increases the diffusion coefficient of ions in the electrolyte of the flow battery, reduces the internal resistance of the battery, and thus improves the battery charge and discharge performance. CN109119692A invented a low-temperature resistant electrolyte and a low-temperature resistant lithium-sulfur battery containing the electrolyte. The characteristic of the battery is that a deep eutectic ionic liquid is introduced into an ether electrolyte. Due to its strong hydrogen bonding effect, while effectively reducing its own lattice energy and freezing point, it improves the ion transfer rate of the organic electrolyte-based lithium-sulfur battery under low temperature conditions, thereby improving the ionic conductivity of the electrolyte and improving the phase interface stability between the electrode and the electrolyte. In 2018, "Angewandte Chemie International Edition" reported that the low eutectic solvent formed by caprolactam / acetamide was used to dissolve polysulfides, thereby forming a high-efficiency lithium-sulfur electrolyte in combination with ordinary electrolytes, but the cycle performance and rate performance were poor. The above three low eutectic solvents are all used in combination with ordinary electrolytes, which seriously weakens the inherent advantages of low eutectic solvents, and cannot fundamentally solve the problems of ordinary electrolytes, nor do they have thermal runaway protection functions. In order to further enhance the safety and performance advantages of electrolytes, the development of completely low eutectic solvent-based electrolytes has become one of the strategies to solve the above battery safety and electrochemical performance problems.
[0006] Combining the inherent advantages of low eutectic solvents, developing low eutectic solvent-based electrolytes with thermal responsive self-polymerization thermal blocking and thermal runaway prevention to replace high-temperature flammable organic electrolytes is expected to improve its safety while ensuring multiple performances of the battery such as electrochemistry. Summary of the invention
[0007] The present invention aims to provide a deep eutectic solvent-based electrolyte, a thermally responsive self-polymerizing deep eutectic solvent-based electrolyte that prevents thermal runaway, and their use in constituting a secondary battery.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A low eutectic solvent-based electrolyte, wherein the low eutectic solvent-based electrolyte is a polynitrile monomer, a monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized, and a metal salt; wherein the room temperature ionic conductivity of the low eutectic solvent-based electrolyte is 1×10 -5 S / cm-9×10 -3 S / cm, and the electrochemical window is greater than 4.4V.
[0010] The polynitrile monomers account for 35%-75% of the mass fraction of the low eutectic solvent-based electrolyte; the monomers that can form a low eutectic solvent with the polynitrile monomers and can be ionically polymerized account for 15%-55% of the mass fraction of the low eutectic solvent-based electrolyte; and the metal salt accounts for 10%-50% of the mass fraction of the low eutectic solvent-based electrolyte.
[0011] Specifically, the polynitrile monomers account for 40%-50% of the mass fraction of the low eutectic solvent-based electrolyte; the monomers that can form a low eutectic solvent with the polynitrile monomers and can be ionically polymerized account for 40%-50% of the mass fraction of the low eutectic solvent-based electrolyte; and the metal salts account for 10%-20% of the mass fraction of the low eutectic solvent-based electrolyte.
[0012] The polynitrile monomers are malononitrile, succinonitrile, 2,2-dimethyl malononitrile, 1,2,3-propanetricarbonitrile, iminodiacetonitrile, trans-butylene dinitrile, thiomalononitrile, benzylmalononitrile, acetylmalononitrile, tetrachloroterephthalonitrile, benzazomalononitrile, tetrafluoroterephthalonitrile, tetrafluorophthalonitrile, tetrafluoroisophthalonitrile, 4-fluorophthalonitrile, cis-malononitrile, 2-bromomalononitrile, 3-hydroxyglutaronitrile, 2-fluoroterephthalonitrile, 1-naphthylmalononitrile, 2-phenylmalononitrile, 4- Fluoroisophthalonitrile, 4-bromophthalonitrile, 2-benzylmalononitrile, 3-chlorophthalonitrile, 3,4-dinitrilephenol, 3-fluorophthalonitrile, 3-nitrophthalonitrile, 3,4-pyridine dinitrile, phthalonitrile, isophthalonitrile, fumaronitrile, 3-methylphthalonitrile, naphthalene-1,4-nitrile terephthalonitrile, thiomalononitrile, 2-aminoisophthalonitrile, 4-methylphthalonitrile, 4-nitrophthalonitrile, diaminomaleonitrile, o-chlorobenzylidenemalononitrile, 4-aminophthalonitrile, o- Chlorobenzylidene malononitrile, anthracene-9,10-dinitrile, 4-methoxyisophthalonitrile, 4,4'-biphenyl dinitrile, ethoxymethylene malononitrile, pyridine-2,4-dinitrile, pyridine-2,3-dinitrile, dimethylaminomethylene malononitrile, p-toluenesulfonic acid amino malononitrile, 1,4-dinitrile cyclobutane, 2,5-dichloroterephthalonitrile, (phenylhydrazono) malononitrile, 4-hydroxybenzylidene malononitrile, 6-bromonaphthalene-2,3-dinitrile, 2,5-dimethylterephthalonitrile, 3,6 -dihydroxyphthalonitrile, (4-methoxybenzyl)malononitrile, (2-furanyl)malononitrile, 2-amino-4,5-imidazole dinitrile, 2,3-diamino-2-succinonitrile, 3-acetyl-3-methylpentane dinitrile, 2-(1-phenylethylidene)malononitrile, 2-(4-methoxybenzyl)malononitrile, (3,4-dihydroxybenzyl)malononitrile, [bis(methylthio)methylene]propane dinitrile, benzyl malononitrile, malononitrile dimerization, 1,3,5-cyclohexanetricarbonitrile,
[0013] One or more of 2,4,6-tribromobenzene-1,3,5-trinitrile, 1,3,5-cyclohexanetrinitrile, 2,3,5,6-pyrazinetetranitrile, tetrakis(4-cyanophenyl)ethylene, and tetramethylsuccinonitrile;
[0014] Further, the polynitrile monomer is one or more of malononitrile, succinonitrile, 2,2-dimethylmalononitrile, 1,2,3-propanetricarbonitrile, iminodiacetonitrile, and trans-butylenedinitrile;
[0015] The monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized is one or more of a 1,3,5-trioxane monomer, a lactam monomer, and an epoxy monomer; further, a 1,3,5-trioxane monomer or a lactam monomer
[0016] The metal salts are lithium salts, sodium salts and potassium salts.
[0017] The 1,3,5-trioxane monomer is shown in general formula 1:
[0018]
[0019] Wherein, R1, R2, R3 can be the same or different and can be selected from H, halogen or C 1-5 An alkyl group, wherein the value of x ranges from 1 to 5;
[0020] The lactam monomer is shown in general formula 2:
[0021]
[0022] Among them, the value range of z is 1-10;
[0023] Epoxy monomers are shown in general formula 3:
[0024]
[0025] Among them, the value range of p is 1-10;
[0026] The lithium salt is one or more of lithium hexafluorophosphate, lithium dioxydifluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bisoxalatoborate, lithium bisfluorooxalatoborate, lithium trifluoromethylsulfonate, lithium bisfluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, and lithium hexafluoroarsenate;
[0027] The sodium salt is one or more of sodium hexafluorophosphate, sodium dioxydifluorophosphate, sodium tetrafluoroborate, sodium perchlorate, sodium bisoxalatoborate, sodium bisfluorooxalatoborate, sodium trifluoromethanesulfonate, sodium bisfluoromethanesulfonyl imide, and sodium bisfluorosulfonyl imide;
[0028] The potassium salt is one or more of potassium hexafluorophosphate, potassium dioxydifluorophosphate, potassium tetrafluoroborate, potassium perchlorate, potassium bisoxalatoborate, potassium bisfluorooxalatoborate, potassium trifluoromethanesulfonate, potassium bisfluoromethanesulfonyl imide, and potassium bisfluorosulfonyl imide.
[0029] When the metal salt in the electrolyte is a metal salt capable of initiating polymerization of a precursor at high temperature, the electrolyte is a thermally responsive self-polymerizing low eutectic solvent-based electrolyte for preventing thermal runaway, wherein the metal salt is one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium dioxydifluorophosphate, lithium difluorooxalatoborate, sodium tetrafluoroborate, sodium hexafluorophosphate, sodium dioxydifluorophosphate, sodium difluorooxalatoborate, potassium tetrafluoroborate, potassium hexafluorophosphate, potassium dioxydifluorophosphate, and potassium difluorooxalatoborate;
[0030] Alternatively, when the metal salt in the electrolyte does not have the function of initiating polymerization of the precursor at high temperature, an initiator is added to the electrolyte to form a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention; wherein the initiator accounts for 0.1%-5% (preferably 1%-3%) of the mass fraction of the low eutectic solvent-based electrolyte; the initiator is an anionic polymerization initiator or a cationic polymerization initiator.
[0031] When the monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized is a 1,3,5-trioxane monomer as shown in general formula 1 or an epoxy monomer as shown in general formula 3, a cationic polymerization initiator is added to the electrolyte; wherein the cationic polymerization initiator is one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium dioxydifluorophosphate, lithium difluorooxalatoborate, sodium tetrafluoroborate, sodium hexafluorophosphate, sodium dioxydifluorophosphate, sodium difluorooxalatoborate, potassium tetrafluoroborate, potassium hexafluorophosphate, potassium dioxydifluorophosphate, potassium difluorooxalatoborate, aluminum chloride, ferric chloride, boron trifluoride, boron trifluoride ether, phosphorus pentafluoride, niobium pentachloride, titanium tetrachloride, zinc chloride, aluminum trifluoromethanesulfonate, bismuth chloride, perchloric acid, urea, boric acid, and acetic acid;
[0032] When the monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized is a lactam monomer shown in general formula 2, an anionic polymerization initiator is added to the electrolyte; wherein the anionic polymerization initiator is one or more of lithium sheets, lithium powder, sodium sheets, sodium powder, potassium sheets, potassium powder, lithium hydroxide, sodium hydroxide, potassium hydroxide, caprolactam magnesium bromide, aminocaproic acid, and caprolactam sodium salt.
[0033] When the monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized is a 1,3,5-trioxane monomer or an epoxy monomer, wherein the metal salt is one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium dioxydifluorophosphate, lithium difluorooxalate borate, sodium tetrafluoroborate, sodium hexafluorophosphate, sodium dioxydifluorophosphate, sodium difluorooxalate borate, potassium tetrafluoroborate, potassium hexafluorophosphate, potassium dioxydifluorophosphate, and potassium difluorooxalate borate, the amount of initiator is 0%; when the metal salt is one or more of lithium perchlorate, lithium bisoxalatoborate, lithium trifluoromethanesulfonate, lithium bisfluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium hexafluoroarsenate, sodium perchlorate, sodium bisoxalatoborate, sodium trifluoromethanesulfonate, sodium bisfluoromethanesulfonyl imide, sodium bisfluorosulfonyl imide, potassium perchlorate, potassium bisoxalatoborate, potassium trifluoromethanesulfonate, potassium bisfluoromethanesulfonyl imide, and potassium bisfluorosulfonyl imide, the amount of initiator used is 0.1%-5%;
[0034] When a low eutectic solvent solution can be formed with a polynitrile monomer and the ionically polymerizable monomer is a lactam monomer, the initiator is one or more of lithium flakes, lithium powder, sodium flakes, sodium powder, potassium flakes, potassium powder, lithium hydroxide, sodium hydroxide, potassium hydroxide, caprolactam magnesium bromide, aminocaproic acid, and caprolactam sodium salt, and the mass fraction of the initiator in the low eutectic solvent solution-based electrolyte is 0.1%-5%.
[0035] When the assembled secondary battery uses an alkali metal (such as lithium metal, sodium metal, potassium metal) as the negative electrode, and when the monomer that can form a low eutectic solvent with the polynitrile monomer and the ion-polymerizable monomer is a lactam monomer, no anionic initiator may be added.
[0036] A method for preparing the deep eutectic solvent-based electrolyte:
[0037] a) uniformly mixing the polynitrile monomer and the monomer that can form a deep eutectic solvent with the polynitrile monomer and can be ionically polymerized in the above proportion to obtain a room temperature deep eutectic solvent;
[0038] b) adding a metal salt in the above-mentioned proportion to the above-mentioned uniformly mixed low eutectic solvent and stirring and mixing, thereby obtaining a low eutectic solvent-based electrolyte; or, adding a metal salt and an initiator in the above-mentioned proportion to the above-mentioned uniformly mixed low eutectic solvent and stirring and mixing, thereby obtaining a thermally responsive self-polymerizing low eutectic solvent-based electrolyte with thermal runaway prevention.
[0039] An application of the low eutectic solvent-based electrolyte: application of the low eutectic solvent-based electrolyte or the thermally responsive self-polymerizing low eutectic solvent-based electrolyte to prevent thermal runaway in a secondary battery.
[0040] A secondary battery comprises a positive electrode, a negative electrode, a separator, and an electrolyte between the positive and negative electrodes, wherein the electrolyte is the low eutectic solvent-based electrolyte or the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention.
[0041] The secondary battery assembly is a button-type battery, a steel-shell cylindrical battery, an aluminum-shell cylindrical battery, a steel-shell square battery, an aluminum-shell square battery or a soft-pack battery.
[0042] The advantages of the present invention are:
[0043] The room temperature ionic conductivity of the deep eutectic solvent-based electrolyte of the present invention is 1×10 -5 S / cm-9×10 -3S / cm, the electrochemical window is greater than 4.4V, which can match higher voltage positive electrode materials, can significantly improve the energy density of secondary batteries, and the assembled secondary batteries have good cycle performance. At the same time, the low eutectic solvent-based electrolyte of the present invention has a simple preparation process and low cost; it has a high boiling point and is not easy to volatilize. At the same time, the low eutectic solvent-based electrolyte can effectively inhibit the growth of negative electrode dendrites, improve the interface stability compatibility and long cycle performance. And the electrolyte obtained after adding an initiator to the electrolyte has the characteristics of thermal response self-polymerization and thermal runaway prevention.
[0044] The secondary battery assembled with the deep eutectic solvent-based electrolyte with the characteristics of thermal response self-polymerization and thermal runaway prevention of the present invention has excellent charging and discharging and long cycle performance at room temperature. At the same time, the deep eutectic solvent-based electrolyte also has the unique characteristics of thermal response self-polymerization and thermal runaway prevention, that is, thermal response self-polymerization can occur under relatively high temperature conditions (90°C-250°C), thereby forming an effective thermal blockage for the secondary battery, avoiding the ignition and explosion of the battery, and effectively preventing the occurrence of thermal runaway, significantly improving the safety and reliability of the secondary battery in extreme special cases such as high temperature thermal shock, combustion test, nail penetration test, external short circuit test, overcharge test, etc. Therefore, the electrolyte is particularly suitable for secondary batteries (such as secondary lithium ion batteries, secondary lithium metal batteries, secondary lithium sulfur batteries, secondary sodium ion batteries, secondary sodium metal batteries, secondary sodium sulfur batteries, secondary potassium ion batteries, secondary potassium metal batteries, secondary potassium sulfur batteries). BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a digital photo of the thermally responsive self-polymerizing low eutectic solvent-based electrolyte for preventing thermal runaway provided in Example 1 of the present invention.
[0046] Figure 2 This is the long cycle performance curve of the lithium iron phosphate / lithium metal battery assembled with the thermally responsive self-polymerizing thermal runaway-proof low eutectic solvent-based electrolyte provided in Example 1 of the present invention at room temperature.
[0047] Figure 3 This is the long cycle performance curve of a lithium cobalt oxide / lithium metal battery assembled with the low eutectic solvent-based electrolyte provided in Example 2 of the present invention (which is also a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention) at room temperature.
[0048] Figure 4 This is a diagram of the thermal blocking effect of a lithium cobalt oxide / lithium metal battery assembled with the low eutectic solvent-based electrolyte provided in Example 2 of the present invention (which is also a low eutectic solvent-based electrolyte that is thermally responsive and self-polymerized to prevent thermal runaway) when encountering high temperature (130°C).
[0049] Figure 5This is the charge and discharge curve of a nickel-cobalt-aluminum / lithium metal battery assembled with a low-melting solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention provided in Example 8 of the present invention at room temperature. DETAILED DESCRIPTION
[0050] The specific implementation modes of the present invention are further described below in conjunction with examples. It should be noted that the specific implementation modes described here are only for illustrating and explaining the present invention, and are not limited to the present invention.
[0051] The present invention is firstly a low eutectic solvent-based electrolyte. The low eutectic solvent-based electrolyte is a polynitrile monomer, a monomer and a metal salt that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized, and is a brand-new low eutectic solvent-based electrolyte; and the low eutectic solvent-based electrolyte has the characteristics of large mutual solubility between ordinary low eutectic solvents and metal lithium salts, wide electrochemical window, high boiling point, non-volatility, etc.; and the low eutectic solvent-based electrolyte is easy to prepare, simple in process, and low in cost; and the electrochemical window of the low eutectic solvent-based electrolyte is greater than 4.4V, which can effectively match higher voltage positive electrode materials, can significantly improve the energy density and cycle performance of secondary batteries, and is a very potential electrolyte system. In addition, the electrolyte is added with an initiator to form a low-melting solvent-based electrolyte that can have thermal response self-polymerization to prevent thermal runaway. At a relatively high temperature (90°C-250°C), the initiator can induce ion polymerization of specific components in the electrolyte to form a high polymer, which significantly increases the battery impedance and causes the battery to form a short circuit, thereby achieving the effect of blocking the battery, significantly improving the safety of secondary batteries in extreme special situations such as high-temperature thermal shock, combustion test, nail penetration test, external short circuit test, and overcharge test.
[0052] Example 1
[0053] In a glove box filled with argon, 2.5 g of trioxymethylene and 2.5 g of 1,2,3-propanetricarbonitrile were stirred and mixed at room temperature, and then 0.76 g of lithium bis(fluoromethanesulfonyl)imide was added and mixed evenly to obtain a low eutectic solvent-based electrolyte, and then 0.12 g of lithium bis(fluorooxalatoborate) was added to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention (see Figure 1 ). 0.15 mL of the above-mentioned low eutectic solvent-based electrolyte for thermal response self-polymerization and thermal runaway prevention is added dropwise to a lithium battery using glass fiber as a support material, lithium iron phosphate as a positive electrode, and lithium as a negative electrode, thereby obtaining a lithium battery for thermal response self-polymerization and thermal runaway prevention.
[0054] Depend on Figure 1 It can be seen that the formed thermally responsive self-polymerizing low-melting solvent-based electrolyte with thermal runaway prevention is transparent and homogeneous.
[0055] The battery cycle test was performed using the above method: the battery charge and discharge range was 2.75V-4V, the charge and discharge rate was 0.3C, and the test temperature was room temperature (see Figure 2 ).
[0056] Depend on Figure 2 It can be seen that the lithium iron phosphate / lithium metal battery assembled with the low-melting solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention exhibits good cycle stability (the capacity hardly decays after 48 cycles; and the coulombic efficiency is close to 100%).
[0057] At the same time, according to the above records, lithium bis(fluoromethanesulfonyl imide) and lithium bis(fluorooxalate borate) in the low eutectic solvent-based electrolyte are replaced by sodium bis(fluoromethanesulfonyl imide) and sodium bis(fluorooxalate borate, and the positive and negative electrodes are replaced by sodium vanadium phosphate and molybdenum disulfide, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the battery is assembled using the electrolyte to obtain a sodium ion battery; at the same time, according to the above records, lithium bis(fluoromethanesulfonyl imide) and lithium bis(fluorooxalate borate) in the low eutectic solvent-based electrolyte are replaced by potassium bis(fluoromethanesulfonyl imide) and potassium bis(fluorooxalate borate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive and negative electrodes are replaced by Prussian blue and graphite using the electrolyte to obtain a potassium ion battery; the electrolytes formed above are all transparent and homogeneous.
[0058] Example 2
[0059] In a glove box filled with argon, 2.5 g of trioxymethylene and 2.5 g of succinonitrile were stirred for 5 minutes at room temperature to mix evenly, and then 0.76 g of lithium difluorooxalate borate was added and stirred for 5 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte. The electrolyte also has the function of exothermic response self-polymerization thermal runaway, and is also a low eutectic solvent-based electrolyte for thermal response self-polymerization and thermal runaway prevention. 0.15 mL of the above-mentioned low eutectic solvent-based electrolyte for thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a polyethylene diaphragm as a supporting material, lithium cobalt oxide as a positive electrode, and lithium as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0060] At the same time, according to the above records, the lithium bifluorooxalate borate in the low eutectic solvent-based electrolyte is replaced by sodium bifluorooxalate borate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium vanadium fluorophosphate and metallic sodium by using the electrolyte, so as to obtain a high-voltage sodium metal battery; at the same time, according to the above records, the lithium bifluorooxalate borate in the low eutectic solvent-based electrolyte is replaced by potassium bifluorooxalate borate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with Prussian blue and potassium metal by using the electrolyte, so as to obtain a potassium metal battery; the formed electrolyte is also transparent and homogeneous.
[0061] The lithium battery obtained above was used to perform battery cycling and adaptive high temperature thermal blocking tests, specifically:
[0062] Adaptive high temperature thermal blocking test: The battery charge and discharge range is 3V-4.3V, the charge and discharge current ratio is 0.3C, the test temperature is room temperature and cycled 10 times, and the temperature is raised to 130℃ to examine its high temperature thermal blocking effect (see Figure 3 ).
[0063] Depend on Figure 3 It can be seen that the 4.3V lithium cobalt oxide / lithium metal battery assembled with the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention exhibits excellent long-cycle stability (the capacity retention rate after 100 cycles is 89.9%). Figure 4 It can be seen that the 4.3V lithium cobalt oxide / lithium metal battery assembled with the thermally responsive self-polymerizing low-eutectic solvent-based electrolyte that prevents thermal runaway blocks the battery reaction within 15 minutes at 130°C, significantly improving the safety of the lithium battery.
[0064] Example 3
[0065] In a glove box filled with argon, 2.5 g of propylene oxide and 2.5 g of succinonitrile were stirred for 5 minutes at room temperature to mix evenly, and then 0.365 g of lithium bis(oxalatoborate) was added to obtain a low eutectic solvent-based electrolyte, and then 0.365 g of lithium hexafluorophosphate was added and stirred for 10 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.10 mL of the above-mentioned low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a spandex membrane as a supporting material, lithium cobalt oxide as a positive electrode, and silicon carbon as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0066] At the same time, according to the above records, lithium bis(oxalatoborate) and lithium hexafluorophosphate in the low eutectic solvent-based electrolyte are replaced by sodium bis(oxalatoborate) and sodium hexafluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive and negative electrodes are replaced with sodium iron sulfate and hard carbon by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, sodium bis(oxalatoborate) and sodium hexafluorophosphate in the low eutectic solvent-based electrolyte are replaced by potassium bis(oxalatoborate) and potassium hexafluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive and negative electrodes are replaced with potassium vanadium pentoxide and graphene by using the electrolyte, so as to obtain a potassium ion battery; the formed electrolyte is also transparent and homogeneous.
[0067] Example 4
[0068] In a glove box filled with argon, 1.5 g of vinyl ether and 1.5 g of malononitrile were stirred for 20 minutes at room temperature to mix, and then 0.7 g of lithium dioxydifluorophosphate was added and mixed evenly to obtain a low eutectic solvent-based electrolyte. The electrolyte also has the function of exothermic response self-polymerization thermal runaway, and is also a low eutectic solvent-based electrolyte for thermal response self-polymerization and thermal runaway prevention. 0.15 mL of the above-mentioned low eutectic solvent-based electrolyte for thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a seaweed fiber non-woven membrane as a supporting material, lithium iron phosphate as a positive electrode, and graphite as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0069] At the same time, according to the above records, the lithium dioxydifluorophosphate in the low eutectic solvent-based electrolyte is replaced by sodium dioxydifluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium iron sulfate and hard carbon by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, the lithium dioxydifluorophosphate in the low eutectic solvent-based electrolyte is replaced by potassium dioxydifluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with polyaniline and potassium metal by using the electrolyte, so as to obtain a potassium metal battery; the formed electrolyte is also transparent and homogeneous.
[0070] Example 5
[0071] In a glove box filled with argon, 1.5 g of dibromotripropionaldehyde and 1.5 g of glutaronitrile were stirred for 25 minutes at room temperature to mix evenly, and then 0.375 g of lithium perchlorate was added to obtain a low eutectic solvent-based electrolyte, and then 0.375 g of lithium hexafluorophosphate was added and stirred for 10 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.2 mL of the above-mentioned low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a polyamide membrane as a supporting material, sulfurized pyrolysis polyacrylonitrile as a positive electrode, and lithium as a negative electrode, thereby obtaining a thermal responsive self-polymerization and thermal runaway-proof lithium-sulfur battery.
[0072] At the same time, according to the above records, lithium perchlorate and lithium hexafluorophosphate in the low eutectic solvent-based electrolyte are replaced by sodium perchlorate and sodium hexafluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium ion fluorophosphate and sodium titanium oxide by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, lithium perchlorate and lithium hexafluorophosphate in the low eutectic solvent-based electrolyte are replaced by potassium perchlorate and potassium hexafluorophosphate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with styrene and potassium metal by using the electrolyte, so as to obtain a potassium metal battery; the formed electrolyte is also transparent and homogeneous.
[0073] Example 6
[0074] In a glove box filled with argon, 1.5 g of chlorotrimethylolaldehyde and 1.5 g of succinonitrile were stirred for 15 minutes at room temperature to mix evenly, and then 0.35 g of lithium trifluoromethanesulfonate was added to obtain a low eutectic solvent-based electrolyte, and then 0.7 g of lithium tetrafluoroborate was added and stirred for 6 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.4 mL of the above-mentioned low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with polyethylene terephthalate film as a supporting material, lithium iron phosphate as a positive electrode, and lithium as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0075] At the same time, according to the above records, lithium trifluoromethanesulfonate and lithium tetrafluoroborate in the low eutectic solvent-based electrolyte are replaced by sodium trifluoromethanesulfonate and sodium tetrafluoroborate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with Prussian blue and sodium metal by using the electrolyte, so as to obtain a sodium metal battery; at the same time, according to the above records, lithium trifluoromethanesulfonate and lithium tetrafluoroborate in the low eutectic solvent-based electrolyte are replaced by potassium trifluoromethanesulfonate and potassium tetrafluoroborate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with layered metal oxides and red phosphorus by using the electrolyte, so as to obtain a potassium ion battery; the formed electrolyte is also transparent and homogeneous.
[0076] Example 7
[0077] In a glove box filled with argon, 0.35 g of enantholactam and 1 g of succinonitrile were stirred for 40 minutes at room temperature to mix, and then 0.8 g of lithium trifluoromethanesulfonate and 0.05 g of lithium difluorooxalate borate were added to obtain a low eutectic solvent-based electrolyte, and 0.008 g of isocyanate was added and continued to stir for 5 minutes to mix evenly, and finally 0.05 g of sodium powder was added to obtain a low eutectic solution-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.4 mL of the above-mentioned low eutectic solution-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a polyimide non-woven membrane as a supporting material, a nickel-cobalt-manganese ternary positive electrode material as a positive electrode, and graphite as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0078] At the same time, according to the above records, lithium trifluoromethanesulfonate and lithium bisfluorooxalate borate in the low eutectic solution-based electrolyte are replaced by sodium trifluoromethanesulfonate and sodium bisfluorooxalate borate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium vanadium fluorophosphate and hard carbon by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, lithium bisfluoromethanesulfonyl imide and lithium bisfluorooxalate borate in the low eutectic solvent-based electrolyte are replaced by potassium bistrifluoromethanesulfonyl imide and potassium bisfluorooxalate borate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with potassium cobaltate and red phosphorus by using the electrolyte, so as to obtain a potassium ion battery; the formed electrolyte is also transparent and homogeneous.
[0079] Example 8
[0080] In a glove box filled with argon, 0.4g of caprolactam and 1g of succinonitrile were stirred for 10 minutes at room temperature to mix, and then 0.8g of lithium bis(trifluoromethanesulfonyl imide) was added to obtain a low eutectic solvent-based electrolyte, and then 0.008g of isocyanate was added and stirred for 5 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.15mL of the above-mentioned low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with a nylon non-woven membrane as a supporting material, a nickel-cobalt-aluminum ternary material as a positive electrode, and lithium as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery, and the battery was used for battery cycle testing. The battery charge and discharge range is 2.75V-4.3V, the charge and discharge rate is 0.3C, and the test temperature is room temperature. (See Figure 5 )
[0081] Depend on Figure 5 It can be seen that the 4.3V nickel-cobalt-aluminum / lithium metal battery assembled based on the thermally responsive low eutectic solvent-based electrolyte has a stable charge and discharge curve at room temperature and a discharge capacity of 193.3 mAh g -1 , proving its excellent interfacial compatibility with nickel-cobalt-aluminum and lithium metals.
[0082] At the same time, according to the above records, the lithium bis(trifluoromethanesulfonyl imide) in the low eutectic solvent-based electrolyte is replaced by sodium bis(trifluoromethanesulfonyl imide), and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium vanadium phosphate and antimony oxide using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, the lithium bis(trifluoromethanesulfonyl imide) in the low eutectic solvent-based electrolyte is replaced by potassium bis(trifluoromethanesulfonyl imide), and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with potassium manganate and potassium metal using the electrolyte, so as to obtain a potassium metal battery, and the formed electrolyte is also transparent and homogeneous.
[0083] Example 9
[0084] In a glove box filled with argon, 0.4 g of propiolactam and 1 g of malononitrile were stirred for 40 minutes at room temperature to mix evenly, and then 0.8 g of lithium bis(fluorosulfonyl)imide was added to obtain a low eutectic solvent-based electrolyte, and then 0.008 g of lithium hydroxide was added and stirred for 5 minutes to mix evenly to obtain a low eutectic solution-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.4 mL of the above-mentioned low eutectic solution-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with glass fiber as a supporting material, a nickel-cobalt-aluminum ternary positive electrode material as a positive electrode, and lithium as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0085] At the same time, according to the above records, lithium bis(fluoromethanesulfonyl)imide is replaced by sodium bis(fluoromethanesulfonyl)imide, and a low-melting solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium manganese oxide and tin antimony composite materials by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, lithium bis(fluoromethanesulfonyl)imide is replaced by potassium bis(fluoromethanesulfonyl)imide, and a low-melting solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with Prussian blue and graphite by using the electrolyte, so as to obtain a potassium ion battery; the formed electrolyte is also transparent and homogeneous.
[0086] Example 10
[0087] In a glove box filled with argon, 0.4 g of butyrolactam and 1 g of succinonitrile were stirred for 5 minutes at room temperature, and then 0.1 g of lithium hexafluorophosphate and 0.4 g of lithium bis(oxalatoborate) were added and stirred for 10 minutes to mix evenly to obtain a low eutectic solvent-based electrolyte, and 0.05 g of lithium powder was added to obtain a low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention. 0.15 mL of the above-mentioned low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention was added dropwise to a lithium battery with cellulose as a supporting material, lithium cobalt oxide as a positive electrode, and graphite as a negative electrode, thereby obtaining a thermal response self-polymerization and thermal runaway prevention lithium battery.
[0088] At the same time, according to the above records, lithium hexafluorophosphate and lithium bisoxalatoborate in the low eutectic solvent-based electrolyte are replaced by sodium hexafluorophosphate and sodium bisoxalatoborate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with sodium cobalt oxide and antimony carbon composite materials by using the electrolyte, so as to obtain a sodium ion battery; at the same time, according to the above records, lithium hexafluorophosphate and lithium bisoxalatoborate in the low eutectic solvent-based electrolyte are replaced by potassium hexafluorophosphate and potassium bisoxalatoborate, and then the low eutectic solvent-based electrolyte with thermal response self-polymerization and thermal runaway prevention is continuously prepared according to the above records, and the positive electrode and the negative electrode are replaced with potassium cobaltate and sulfide by using the electrolyte, so as to obtain a potassium ion battery; the formed electrolyte is also transparent and homogeneous.
Claims
1. A thermally responsive self-polymerizing low eutectic solvent-based electrolyte for preventing thermal runaway, characterized in that: The low eutectic solvent-based electrolyte is a polynitrile monomer, a monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized, and a metal salt; wherein the room temperature ionic conductivity of the low eutectic solvent-based electrolyte is 1×10 -5 S / cm - 9×10 -3 S / cm, electrochemical window greater than 4.4 V; The polynitrile monomers account for 35% to 75% of the mass fraction of the low eutectic solvent-based electrolyte; the monomers that can form a low eutectic solvent with the polynitrile monomers and can be ionically polymerized account for 15% to 55% of the mass fraction of the low eutectic solvent-based electrolyte; the metal salt accounts for 10% to 50% of the mass fraction of the low eutectic solvent-based electrolyte; The monomer that can form a low eutectic solvent with the polynitrile monomer and can be ionically polymerized is one or more of a lactam monomer and an epoxy monomer; The polynitrile monomers are malononitrile, succinonitrile, 2,2-dimethyl malononitrile, 1,2,3-propanetricarbonitrile, iminodiacetonitrile, trans-butylene dinitrile, thiomalononitrile, benzylmalononitrile, acetylmalononitrile, tetrachloroterephthalonitrile, benzazomalononitrile, tetrafluoroterephthalonitrile, tetrafluorophthalonitrile, tetrafluoroisophthalonitrile, 4-fluorophthalonitrile, cis-malononitrile, 2-bromomalononitrile, 3-hydroxyglutaronitrile, 2-fluoroterephthalonitrile, 1-naphthylmalononitrile, 2-phenylmalononitrile, 4-fluoroisophthalonitrile, 4-bromophthalonitrile, 2-benzylmalononitrile, 2-phenylmalononitrile, 4-fluoroisophthalonitrile, 4-bromophthalonitrile, 2-benzylmalononitrile, 2-phenylmalononitrile, 2-phenylisophthalonitrile, 4-bromophthalonitrile, 2-phenyl- ... 3-chlorophthalonitrile, 3,4-dinitrilephenol, 3-fluorophthalonitrile, 3-nitrophthalonitrile, 3,4-pyridine dinitrile, phthalonitrile, isophthalonitrile, fumaronitrile, 3-methylphthalonitrile, naphthalene-1,4-dinitrile, terephthalonitrile, thiomalononitrile, 2-aminoisophthalonitrile, 4-methylphthalonitrile, 4-nitrophthalonitrile, diaminomaleic acid dinitrile, o-chlorobenzylidenemalononitrile, 4-aminophthalonitrile, o-chlorobenzylidenemalononitrile, anthracene-9,10-dinitrile, 4-methoxyisophthalonitrile, 4,4' -biphenyl dinitrile, ethoxymethylene malononitrile, pyridine-2,4-dinitrile, pyridine-2,3-dinitrile, dimethylaminomethylene malononitrile, p-toluenesulfonic acid amino malononitrile, 1,4-dinitrile cyclobutane, 2,5-dichloroterephthalonitrile, (phenylhydrazono) malononitrile, 4-hydroxybenzylidene malononitrile, 6-bromonaphthalene-2,3-dinitrile, 2,5-dimethylterephthalonitrile, 3,6-dihydroxyphthalonitrile, (4-methoxybenzylene) malononitrile, (2-furanylene) malononitrile, 2-amino-4,5-imidazole dinitrile, 2, One or more of 3-diamino-2-succinonitrile, 3-acetyl-3-methylpentane dinitrile, 2-(1-phenylethylidene)malononitrile, 2-(4-methoxybenzyl)malononitrile, (3,4-dihydroxybenzyl)malononitrile, [bis(methylthio)methylene]propane dinitrile, benzyl malononitrile, malononitrile dimerization, 1,3,5-cyclohexanetrinitrile, 2,4,6-tribromobenzene-1,3,5-trinitrile, 1,3,5-cyclohexanetrinitrile, 2,3,5,6-pyrazine tetranitrile, tetrakis(4-nitrilephenyl)ethylene, and tetramethylsuccinonitrile; The lactam monomer is shown in general formula 2: Formula 2 Among them, the value range of z is 1-10; The epoxy monomer is shown in general formula 3: Formula 3 Among them, the value range of p is 1-10; When the monomer that can form a low eutectic solvent with the polynitrile monomer and the ion-polymerizable monomer is an epoxy monomer, wherein the metal salt is one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium dioxydifluorophosphate, lithium difluorooxalatoborate, sodium tetrafluoroborate, sodium hexafluorophosphate, sodium dioxydifluorophosphate, sodium difluorooxalatoborate, potassium tetrafluoroborate, potassium hexafluorophosphate, potassium dioxydifluorophosphate, and potassium difluorooxalatoborate, the amount of initiator is 0%; When the metal salt is one or more of lithium perchlorate, lithium bisoxalatoborate, lithium trifluoromethanesulfonate, lithium bisfluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium hexafluoroarsenate, sodium perchlorate, sodium bisoxalatoborate, sodium trifluoromethanesulfonate, sodium bisfluoromethanesulfonyl imide, sodium bisfluorosulfonyl imide, potassium perchlorate, potassium bisoxalatoborate, potassium trifluoromethanesulfonate, potassium bisfluoromethanesulfonyl imide, and potassium bisfluorosulfonyl imide, the amount of initiator is 0.1%-5%; when a low eutectic solvent can be formed with a polynitrile monomer and the ion-polymerizable monomer is a lactam monomer, the initiator is one or more of lithium flakes, lithium powder, sodium flakes, sodium powder, potassium flakes, potassium powder, lithium hydroxide, sodium hydroxide, potassium hydroxide, caprolactam magnesium bromide, aminocaproic acid, and caprolactam sodium salt, and the mass fraction of the initiator in the low eutectic solvent-based electrolyte is 0.1%-5%.
2. A method for preparing the thermally responsive self-polymerizing thermal runaway-proof deep eutectic solvent-based electrolyte according to claim 1, characterized in that: a) uniformly mixing the polynitrile monomer and the monomer that can form a deep eutectic solvent with the polynitrile monomer and can be ionically polymerized in the above proportion to obtain a room temperature deep eutectic solvent; b) adding metal salts in the above-mentioned proportions to the above-mentioned uniformly mixed low eutectic solvent and stirring and mixing them, thereby obtaining a low eutectic solvent-based electrolyte; or, adding metal salts and initiators in the above-mentioned proportions to the above-mentioned uniformly mixed low eutectic solvent and stirring and mixing them, thereby obtaining a thermally responsive self-polymerizing low eutectic solvent-based electrolyte that prevents thermal runaway.
3. An application of a thermally responsive self-polymerizing thermal runaway-proof eutectic solvent-based electrolyte as claimed in claim 1, characterized in that: Application of the deep eutectic solvent-based electrolyte or the thermally responsive self-polymerizing thermal runaway-proof deep eutectic solvent-based electrolyte in secondary batteries.
4. A secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte between the positive and negative electrodes, characterized in that; The electrolyte is the thermally responsive self-polymerizing low eutectic solvent-based electrolyte for preventing thermal runaway as described in claim 1.
5. The secondary battery according to claim 4, characterized in that: The secondary battery assembly is a button-type battery, a steel-shell cylindrical battery, an aluminum-shell cylindrical battery, a steel-shell square battery, an aluminum-shell square battery or a soft-pack battery.