A method for predicting creep life-wall thickness relationship reflecting cross-sectional size effect
Through the creep failure criterion and linear damage accumulation theory based on regional division, combined with the test life of minimum wall thickness and maximum wall thickness standard parts, the test volume of the prediction method for the creep life-wall thickness relationship of nickel-based superalloys in the existing technology is solved. Yamato solves the problem of many parameters, achieves accurate prediction of creep life within the wall thickness range, and simplifies the life design of nickel-based high-temperature alloy turbine blades.
Patent Information
- Application Number
- CN202210177057.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-02-24
AI Technical Summary
The existing prediction method for the creep life-wall thickness relationship of nickel-based superalloys requires a large number of tests and multi-parameter fitting, which limits its engineering application.
Using the creep failure criterion based on area division, through the test life of the minimum wall thickness and maximum wall thickness standard parts, combined with the linear damage accumulation theory, without the need for fitting parameters, the creep life of the wall thickness between δmm and δ'mm can be achieved predict.
Without the need to conduct a large number of tests, the creep life-wall thickness relationship of standard parts with different wall thicknesses can be accurately predicted, simplifying the life design and evaluation of nickel-based high-temperature alloy turbine blades.
Smart Images

Figure CN114530219B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a creep life-wall thickness relationship prediction method reflecting the cross-sectional size effect, which is mainly used for predicting the creep life-wall thickness relationship of nickel-based high-temperature alloys, laying a foundation for the life design and evaluation of nickel-based high-temperature alloy components (such as nickel-based high-temperature alloy turbine blades), and belongs to the field of material high-temperature mechanical property evaluation and aero-engine technology. Background Art
[0002] Nickel-based superalloys have excellent high-temperature properties and are important materials for manufacturing advanced aero-engine turbine blades. As the temperature before the aero-engine turbine continues to increase, the turbine blades gradually evolve from solid structures to hollow thin-walled structures. The thin-walled area of the turbine blade is usually its weak link, and the mechanical properties of the hollow thin-walled structure are usually different from those of traditional solid standard parts. Therefore, it is necessary to establish a prediction method for the mechanical property-wall thickness relationship that reflects the cross-sectional size effect and accurately evaluate the mechanical properties of the hollow thin-walled structure.
[0003] For creep, an important failure mode of turbine blades, the commonly used life-wall thickness relationship prediction methods can be divided into two categories:
[0004] (1) The first method: The high-temperature creep fracture process of the specimen is closely related to the formation of the surface oxide layer. The formation of the oxide layer will reduce the effective bearing area of the specimen and increase the effective stress it bears. Surface oxidation usually has a greater impact on thinner specimens. By quantifying the influence of surface oxidation on standard parts with different wall thicknesses, establishing the relationship between effective stress and wall thickness, and bringing the effective stress into the traditional creep life model, the creep life-wall thickness relationship can be predicted (Zhang Li, Yu Huichen, Guo Guangping, et al. Endurance and fracture behavior of thin-walled specimens of
[001] oriented DD6 single crystal alloy [J]. Journal of Aerospace Power, 2019, 34: 122-129).
[0005] (2) The second method: directly establish a creep life model or creep damage model related to wall thickness, thereby realizing the prediction of the creep life-wall thickness relationship (Han Jianfeng. Research on size effect and rafting of nickel-based single crystal alloy creep specimens [D]. Northwestern Polytechnical University, 2011).
[0006] Both of the above methods require conducting creep tests on standard parts with different wall thicknesses (usually no less than 3 types) under the same test conditions to obtain the creep test life of standard parts with different wall thicknesses, and obtain model parameters by fitting the test results. The above methods have a large number of tests and many parameters, which limits their engineering application. Summary of the invention
[0007] The technical solution of the present invention is a new method for predicting the creep life-wall thickness relationship that reflects the cross-sectional size effect. This method can accurately predict the creep life of standard parts with a wall thickness between δmm and δ'mm based on the creep test life of standard parts with a wall thickness of δmm and δ'mm (δ'>δ), without the need for a large number of tests. In addition, this method can be used in combination with the linear damage accumulation theory to accurately predict the creep life-wall thickness relationship of standard parts with different wall thicknesses without using any fitting parameters. The specific implementation steps are as follows:
[0008] In the first step, for standard parts with arbitrary wall thickness, in the creep life prediction process, the entire standard part is divided into two parts: region 1 (material surface area) and region 2 (material internal area). Among them, the thickness of region 1 is determined by the standard part with the smallest wall thickness, and the thickness of region 2 is the difference between the total thickness of the standard part and the thickness of region 1.
[0009] The second step is to carry out creep tests on standard parts with minimum wall thickness (usually not more than 0.5mm) and creep tests on standard parts with maximum wall thickness (usually not less than 2.5mm) to obtain the creep test life of standard parts with minimum wall thickness and the creep test life of standard parts with maximum wall thickness.
[0010] The third step is to determine whether the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part.
[0011] (1) If the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part, it means that the material has a thin wall effect (a cross-sectional size effect). In this case, the creep failure criterion 1 based on regional division is used to predict the creep life-wall thickness relationship. The creep failure criterion 1 based on regional division believes that for materials with thin wall effect, the damage D1 in region 1 is greater than the damage D2 in region 2, and the total damage rate of the entire standard part is the area average of the damage rate in region 1 and the damage rate in region 2, that is:
[0012]
[0013] Where D is the total damage of the entire standard component, S1, S2 and S are the total areas of region 1, region 2 and the entire standard component respectively, and t is time. When the damage D1 and D2 obey Miner's linear damage accumulation theory, then dD1 / dt=D1 / t=K1, dD2 / dt=D2 / t=K2, K1 and K2 are both constants, and the integral formula (6) can be obtained:
[0014]
[0015] At this time, the creep failure criterion 1 based on regional division can be expressed as:
[0016]
[0017] Among them, D cri is the critical damage of the entire standard part (when the total damage of the entire standard part reaches the critical damage, the standard part breaks). Usually, the material will break when the true stress it bears reaches the ultimate tensile strength. At this time, the critical damage D cri The relationship with the macro stress σ is as follows:
[0018]
[0019] Among them, σ b is the ultimate tensile strength. Based on formula (9), the critical damage D cri It can be expressed as:
[0020]
[0021] According to Miner's linear damage accumulation theory and formula (8), the relationship between D1, D2 and t can be expressed by the creep test life of the standard part with the smallest wall thickness and the standard part with the largest wall thickness, respectively:
[0022]
[0023]
[0024] in, and is the creep life of the standard part with the smallest wall thickness and the standard part with the largest wall thickness, and S st It is the total area of area 1 of the standard part with the largest wall thickness, area 2 of the standard part with the largest wall thickness and the standard part with the largest wall thickness. It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 1 based on regional division, but this does not mean that the creep failure criterion 1 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 1 based on regional division can also be established by using methods such as nonlinear accumulation theory.
[0025] (2) If the creep test life of the minimum wall thickness standard part is greater than the creep test life of the maximum wall thickness standard part, it means that the material has an abnormal thin wall effect (a cross-sectional size effect). In this case, the creep failure criterion 3 based on regional division is used to predict the creep life-wall thickness relationship. The creep failure criterion 3 based on regional division believes that for materials with abnormal thin wall effect, the damage D1 in region 1 is less than the damage D2 in region 2, and the total damage rate of the entire standard part is the area average of the damage rate in region 1 and the damage rate in region 2, that is:
[0026]
[0027] When the damage D1 and D2 obey Miner's linear damage accumulation theory, the integral formula (13) can be obtained:
[0028]
[0029] At this time, the creep failure criterion 3 based on regional division can be expressed as:
[0030]
[0031] At this time, the relationship between D1, D2 and t can still be described by formula (11) and formula (12). It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 3 based on regional division, but this does not mean that the creep failure criterion 3 based on regional division can only be established by Miner's linear damage accumulation theory. The creep failure criterion 3 based on regional division can also be established by using nonlinear accumulation theory and other methods.
[0032] The fourth step is to determine whether the damage in area 1 and area 2 reaches 1.
[0033] (1) If the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step, calculate whether the damage of region 1 of the different wall thickness standard parts reaches 1. If the damage of region 1 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step are the final prediction results; if the damage of region 1 reaches 1, the creep failure criterion 2 based on regional division should be used to update the prediction results in the third step, and the updated prediction results are the final prediction results. The creep failure criterion 2 based on regional division believes that: for materials with thin wall effect, the damage D1 of region 1 is greater than the damage D2 of region 2, and the damage process of the entire standard part includes two stages: in the first stage, the total damage rate of the entire standard part is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard part is equal to the product of the damage rate of region 2 and the area ratio S2 / S occupied by region 2, that is:
[0034]
[0035] Among them, D I is the total damage in the first stage, D II is the total damage in the second stage. When the damage D1 and D2 obey Miner's linear damage accumulation theory, the total damage D in the second stage II It can be expressed as:
[0036]
[0037] At this time, the creep failure criterion 2 based on regional division can be expressed as:
[0038]
[0039] According to Miner's linear damage accumulation theory and formula (18), D2 can be expressed as:
[0040]
[0041] It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 2 based on regional division. However, this does not mean that the creep failure criterion 2 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 2 based on regional division can also be established by using methods such as nonlinear accumulation theory.
[0042] (2) If the creep test life of the minimum wall thickness standard part is greater than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step, calculate whether the damage of region 2 of the different wall thickness standard parts reaches 1. If the damage of region 2 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step are the final prediction results; if the damage of region 2 reaches 1, the creep failure criterion 4 based on regional division should be used to update the prediction results in the third step, and the updated prediction results are the final prediction results. The creep failure criterion 4 based on regional division believes that: for materials with abnormal thin wall effect, the damage D1 of region 1 is less than the damage D2 of region 2, and the damage process of the entire standard part includes two stages: in the first stage, the total damage rate of the entire standard part is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard part is equal to the product of the damage rate of region 1 and the area ratio S1 / S occupied by region 1, that is:
[0043]
[0044] When damage D1 and D2 obey Miner's linear damage accumulation theory, the total damage D in the second stage II It can be expressed as:
[0045]
[0046] At this time, the creep failure criterion 4 based on regional division can be expressed as:
[0047]
[0048] At this time, the relationship between D1 and t can still be described by formula (11). It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 4 based on regional division, but this does not mean that the creep failure criterion 4 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 4 based on regional division can also be established by using nonlinear accumulation theory and other methods.
[0049] The advantages of the present invention over the prior art are as follows: the core of the present invention is the creep failure criterion based on regional division. Based on this method, when the creep test life of standard parts with a wall thickness of δmm and the creep test life of standard parts with a wall thickness of δ'mm (δ'>δ) are known, the creep life of standard parts with a wall thickness between δmm and δ'mm can be accurately predicted without conducting a large number of tests; in addition, this method can be used in combination with the linear damage accumulation theory, and the creep life-wall thickness relationship can be accurately predicted without fitting any parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 The implementation process of the method of the present invention;
[0051] Figure 2 This is a schematic diagram of the standard parts area division;
[0052] Figure 3 This is the damage-time relationship diagram of the material with thin-wall effect (based on Miner's linear damage accumulation theory, the cumulative damage of area 1 and area 2 does not reach 1);
[0053] Figure 4 This is the damage-time relationship diagram of the material with abnormal thin-wall effect (based on Miner's linear damage accumulation theory, the cumulative damage of area 1 and area 2 does not reach 1);
[0054] Figure 5 This is the damage-time relationship diagram of the material with thin-wall effect (based on Miner's linear damage accumulation theory, the cumulative damage in area 1 reaches 1);
[0055] Figure 6 This is the damage-time relationship diagram of the material with abnormal thin-wall effect (based on Miner's linear damage accumulation theory, the cumulative damage in area 2 reaches 1);
[0056] Figure 7 The creep life-wall thickness relationship prediction results of the standard nickel-based single crystal superalloy PWA1484 with thin wall effect;
[0057] Figure 8 The predicted results of creep life-wall thickness relationship of standard nickel-based single crystal superalloy DD6 parts with thin wall effect;
[0058] Fig. 9 The creep life-wall thickness relationship prediction results of the standard nickel-based single crystal high-temperature alloy DD6 with anomalous thin-wall effect. DETAILED DESCRIPTION
[0059] The following is a further explanation of the technical solution of a creep life-wall thickness relationship prediction method reflecting the cross-sectional size effect proposed by the present invention by way of example in conjunction with the accompanying drawings. The pre-study materials of this example are nickel-based single crystal high-temperature alloy PWA1484 and nickel-based single crystal high-temperature alloy DD6.
[0060] like Figure 1 As shown, the specific implementation process of the present invention is as follows:
[0061] In the first step, for standard parts with arbitrary wall thickness, in the creep life prediction process, according to Figure 2 As shown in the figure, the entire standard part is divided into two parts: Area 1 (material surface area) and Area 2 (material internal area). The thickness of Area 1 is determined by the standard part with the smallest wall thickness, and the thickness of Area 2 is the difference between the total thickness of the standard part and the thickness of Area 1. Figure 2 As shown, when the minimum wall thickness of the standard part is δ, for the standard parts with wall thicknesses of δ, 2δ, and 4δ, the thicknesses of region 1 are δ, δ, and δ respectively, and the thicknesses of region 2 are 0, δ, and 3δ respectively.
[0062] The second step is to carry out creep tests on standard parts with minimum wall thickness (usually not more than 0.5mm) and creep tests on standard parts with maximum wall thickness (usually not less than 2.5mm) to obtain the creep test life of standard parts with minimum wall thickness and the creep test life of standard parts with maximum wall thickness.
[0063] The third step is to determine whether the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part.
[0064] (1) If the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part, it means that the material has a thin wall effect (a cross-sectional size effect). In this case, the creep failure criterion 1 based on regional division is used to predict the creep life-wall thickness relationship. The creep failure criterion 1 based on regional division believes that: for materials with thin wall effect, the damage-time relationship is as follows: Figure 3 As shown in Figure 1 (based on Miner's linear damage accumulation theory, the cumulative damage of area 1 and area 2 does not reach 1), the damage D1 of area 1 is greater than the damage D2 of area 2, and the total damage rate of the entire standard part is the area average of the damage rate of area 1 and the damage rate of area 2, that is:
[0065]
[0066] Where D is the total damage of the entire standard component, S1, S2 and S are the total areas of region 1, region 2 and the entire standard component respectively, and t is time. When the total damage D of the entire standard component reaches the critical damage, the standard component fails. When the damage D1 and D2 obey Miner's linear damage accumulation theory, then dD1 / dt=D1 / t=K1, dD2 / dt=D2 / t=K2, K1 and K2 are both constants, and the integral formula (23) can be obtained:
[0067]
[0068] At this time, the creep failure criterion 1 based on regional division can be expressed as:
[0069]
[0070] Among them, D cri is the critical damage of the entire standard part (when the total damage of the entire standard part reaches the critical damage, the standard part breaks). Usually, the material will break when the true stress it bears reaches the ultimate tensile strength. At this time, the critical damage D cri The relationship with the macro stress σ is as follows:
[0071]
[0072] Among them, σ b is the ultimate tensile strength. Based on formula (26), the critical damage D cri It can be expressed as:
[0073]
[0074] According to Miner's linear damage accumulation theory and formula (25), the relationship between D1, D2 and t can be expressed by the creep test life of the standard part with the smallest wall thickness and the standard part with the largest wall thickness, respectively:
[0075]
[0076]
[0077] in, and It is the creep life of the standard part with the smallest wall thickness and the standard part with the largest wall thickness. and S stIt is the total area of area 1 of the standard part with the largest wall thickness, area 2 of the standard part with the largest wall thickness and the standard part with the largest wall thickness. It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 1 based on regional division, but this does not mean that the creep failure criterion 1 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 1 based on regional division can also be established by using methods such as nonlinear accumulation theory.
[0078] (2) If the creep test life of the minimum wall thickness standard part is greater than the creep test life of the maximum wall thickness standard part, it means that the material has an abnormal thin wall effect (a cross-sectional size effect). In this case, the creep failure criterion 3 based on regional division is used to predict the creep life-wall thickness relationship. The creep failure criterion 3 based on regional division believes that: for materials with abnormal thin wall effect, the damage-time relationship is as follows: Figure 4 As shown in Figure 1 (based on Miner's linear damage accumulation theory, the cumulative damage of area 1 and area 2 does not reach 1), the damage D1 of area 1 is less than the damage D2 of area 2, and the total damage rate of the entire standard part is the area average of the damage rate of area 1 and the damage rate of area 2, that is:
[0079]
[0080] When the total damage D of the entire standard component reaches the critical damage, the standard component fails. When the damage D1 and D2 obey Miner's linear damage accumulation theory, the integral formula (30) can be obtained:
[0081]
[0082] At this time, the creep failure criterion 3 based on regional division can be expressed as:
[0083]
[0084] At this time, the relationship between D1, D2 and t can still be described by formula (28) and formula (29). It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 3 based on regional division, but this does not mean that the creep failure criterion 3 based on regional division can only be established by Miner's linear damage accumulation theory. The creep failure criterion 3 based on regional division can also be established by using nonlinear accumulation theory and other methods.
[0085] The fourth step is to determine whether the damage in area 1 and area 2 reaches 1.
[0086] (1) If the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step, calculate separately whether the damage of region 1 of the different wall thickness standard parts reaches 1. If the damage of region 1 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step are the final prediction results; if the damage of region 1 reaches 1, the creep failure criterion 2 based on regional division should be used to update the prediction results in the third step, and the updated prediction results are the final prediction results. The creep failure criterion 2 based on regional division believes that: for materials with thin-wall effect, its damage-time relationship is as follows: Figure 5 As shown in Figure 1 (based on Miner's linear damage accumulation theory, the cumulative damage of region 1 reaches 1), the damage D1 of region 1 is greater than the damage D2 of region 2. The damage process of the entire standard component includes two stages: in the first stage, the total damage rate of the entire standard component is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard component is equal to the product of the damage rate of region 2 and the area ratio S2 / S occupied by region 2, that is:
[0087]
[0088] Among them, D I is the total damage in the first stage, D II is the total damage in the second stage. When the total damage of the entire standard component reaches the critical damage, the standard component fails. When the damage D1 and D2 obey Miner's linear damage accumulation theory, the total damage D in the second stage II It can be expressed as:
[0089]
[0090] At this time, the creep failure criterion 2 based on regional division can be expressed as:
[0091]
[0092] According to Miner's linear damage accumulation theory and formula (35), D2 can be expressed as:
[0093]
[0094] It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 2 based on regional division. However, this does not mean that the creep failure criterion 2 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 2 based on regional division can also be established by using methods such as nonlinear accumulation theory.
[0095] (2) If the creep test life of the minimum wall thickness standard part is greater than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step, calculate separately whether the damage of region 2 of the different wall thickness standard parts reaches 1. If the damage of region 2 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in the third step are the final prediction results; if the damage of region 2 reaches 1, the creep failure criterion 4 based on regional division should be used to update the prediction results in the third step, and the updated prediction results are the final prediction results. The creep failure criterion 4 based on regional division believes that: for materials with abnormal thin-wall effect, its damage-time relationship is as follows: Figure 6 As shown in Figure 1 (based on Miner's linear damage accumulation theory, the cumulative damage of region 2 reaches 1), the damage D1 of region 1 is less than the damage D2 of region 2. The damage process of the entire standard component includes two stages: in the first stage, the total damage rate of the entire standard component is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard component is equal to the product of the damage rate of region 1 and the area ratio S1 / S occupied by region 1, that is:
[0096]
[0097] Among them, D I is the total damage in the first stage, D II is the total damage in the second stage. When the total damage of the entire standard component reaches the critical damage, the standard component fails. When the damage D1 and D2 obey Miner's linear damage accumulation theory, the total damage D in the second stage II It can be expressed as:
[0098]
[0099] At this time, the creep failure criterion 4 based on regional division can be expressed as:
[0100]
[0101] At this time, the relationship between D1 and t can still be described by formula (28). It should be pointed out that this example uses Miner's linear damage accumulation theory to describe the creep failure criterion 4 based on regional division, but this does not mean that the creep failure criterion 4 based on regional division can only be established through Miner's linear damage accumulation theory. The creep failure criterion 4 based on regional division can also be established by using nonlinear accumulation theory and other methods.
[0102] In order to verify the accuracy of the creep life-wall thickness relationship prediction method reflecting the cross-sectional size effect proposed in the present invention, combined with Miner's linear damage accumulation theory, the creep life-wall thickness relationship of the nickel-based single crystal superalloy PWA1484 standard parts with different wall thicknesses in the reference (Seetharaman V, Cetel AD. Thickness debit in creep properties of PWA1484 [J]. Proceedings of the International Symposium on Superalloys, 2004, 207-214.) and the nickel-based single crystal superalloy DD6 standard parts with different wall thicknesses in the reference (Wen Z, Pei H, Li D, et al. Thickness influence on the creep response of DD6 Ni-Based single-crystal superalloy [J]. High Temperature Material Processes, 2016, 35 (9): 871-880.) are predicted. The creep life-wall thickness relationship prediction results of the nickel-based single crystal superalloy PWA1484 standard parts with thin wall effect are as follows: Figure 7 As shown in Figure 2, the prediction results under the conditions of 871℃ / 413MPa, 982℃ / 207MPa, 760℃ / 758MPa, and 982℃ / 248MPa are in good agreement with the test results; the prediction results of the creep life-wall thickness relationship of the standard nickel-based single crystal high-temperature alloy DD6 with thin-wall effect are as follows Figure 8 As shown in Figure 2, the prediction results under the conditions of 980℃ / 320MPa, 980℃ / 360MPa, 980℃ / 400MPa, 760℃ / 830MPa, 760℃ / 850MPa, and 760℃ / 900MPa are in good agreement with the test results; the prediction results of the creep life-wall thickness relationship of the standard nickel-based single crystal high-temperature alloy DD6 with abnormal thin-wall effect are as follows Fig. 9 As shown, the prediction results under the conditions of 1100℃ / 170MPa, 1100℃ / 200MPa, and 1100℃ / 225MPa are in good agreement with the test results. It can be seen that the creep life-wall thickness relationship prediction law of nickel-based single crystal high-temperature alloy PWA1484 standard parts with different wall thicknesses and nickel-based single crystal high-temperature alloy DD6 standard parts with different wall thicknesses are in good agreement with the test results. The above results show that the creep life-wall thickness relationship prediction method reflecting the cross-sectional size effect proposed in the present invention can better quantify and characterize the cross-sectional size effect (including thin-wall effect and abnormal thin-wall effect) in the creep process.
[0103] The above embodiments are provided only for the purpose of describing the present invention, and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. Various equivalent substitutions and modifications made without departing from the spirit and principles of the present invention should all be included within the scope of the present invention.
Claims
1. A method for predicting creep life-wall thickness relationship reflecting cross-sectional size effect, characterized in that: The steps include: Step 1): For standard parts with arbitrary wall thickness, in the creep life prediction process, the entire standard part is divided into two parts: Region 1, i.e., the surface area of the material, and Region 2, i.e., the internal area of the material. The thickness of Region 1 is determined by the standard part with the smallest wall thickness, and the thickness of Region 2 is the difference between the total thickness of the standard part and the thickness of Region 1. Step 2): Conduct creep tests on standard parts with minimum wall thickness and standard parts with maximum wall thickness to obtain creep test life of standard parts with minimum wall thickness and creep test life of standard parts with maximum wall thickness; the minimum wall thickness is not greater than 0.5 mm, and the maximum wall thickness is not less than 2.5 mm; Step 3): Determine whether the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part; (1) If the creep test life of the standard part with the smallest wall thickness is less than that of the standard part with the largest wall thickness, it means that the material has a thin-wall effect, which belongs to the cross-sectional size effect. In this case, the creep failure criterion 1 based on regional division is used to predict the creep life-wall thickness relationship; (2) If the creep test life of the standard part with the smallest wall thickness is greater than that of the standard part with the largest wall thickness, it means that the material has an abnormal thin-wall effect, which belongs to the cross-sectional size effect. In this case, the creep failure criterion 3 based on regional division is used to predict the creep life-wall thickness relationship; Step 4): Determine whether the damage of area 1 and area 2 reaches 1; (1) If the creep test life of the minimum wall thickness standard part is less than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in step 3), calculate separately whether the damage of region 1 of the different wall thickness standard parts reaches 1; if the damage of region 1 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in step 3) are the final prediction results; if the damage of region 1 reaches 1, the creep failure criterion 2 based on regional division should be used to update the creep life-wall thickness relationship prediction results in step 3), and the updated prediction results are the final prediction results; (2) If the creep test life of the minimum wall thickness standard part is greater than the creep test life of the maximum wall thickness standard part, based on the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in step 3), calculate separately whether the damage of region 2 of the different wall thickness standard parts reaches 1; if the damage of region 2 does not reach 1, the creep life-wall thickness relationship prediction results of the different wall thickness standard parts in step 3) are the final prediction results; if the damage of region 2 reaches 1, the creep failure criterion 4 based on regional division should be used to update the creep life-wall thickness relationship prediction results in step 3), and the updated prediction results are the final prediction results; In step 3), the creep failure criterion 1 based on regional division is: for materials with thin-wall effect, region 1 is damaged Greater than zone 2 damage , the total damage rate of the entire standard part is the area average of the damage rate in area 1 and the damage rate in area 2, that is: (1) Where D is the total damage of the entire standard component, S1, S2 and S are the total areas of region 1, region 2 and the entire standard component respectively, and t is the time; when the total damage of the entire standard component reaches the critical damage D cri When the standard part breaks, the critical damage D cri It is expressed as: (2) Among them, σ is the macro stress, σ b is the ultimate tensile strength; Creep failure criterion 3 based on regional division is: materials with abnormal thin wall effect, damage in region 1 Less damage than zone 2 , the total damage rate of the entire standard part is the area average of the damage rate in area 1 and the damage rate in area 2, that is: (3) When the total damage of the entire standard component reaches the critical damage D cri When , the standard part breaks; In step 4), the creep failure criterion 2 based on regional division is: for materials with thin-wall effect, region 1 is damaged Greater than zone 2 damage , the damage process of the entire standard part includes two stages: in the first stage, the total damage rate of the entire standard part is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard part is equal to the product of the damage rate of region 2 and the area ratio S2 / S of region 2, that is: (4) Among them, D I is the total damage in the first stage, D II is the total damage in the second stage; Creep failure criterion 4 based on regional division is: materials with abnormal thin wall effect, damage in region 1 Less damage than zone 2 , the damage process of the entire standard part includes two stages: in the first stage, the total damage rate of the entire standard part is the area average of the damage rate of region 1 and the damage rate of region 2; in the second stage, the total damage rate of the entire standard part is equal to the product of the damage rate of region 1 and the area ratio S1 / S of region 1, that is: (5)。