PETG-PC alloy with high light transmittance and high toughness, preparation method and application thereof

By adding PC resin and additives to PETG resin and using a special process to prepare PETG-PC alloy, the problem of poor demolding properties of PETG material is solved, and the application of materials with high light transmittance and high toughness is realized.

CN114539740BActive Publication Date: 2024-11-26SUZHOU WODF NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210390911.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-11-26
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

PETG material has poor demolding properties when processing thick-walled, large-sized materials, which limits its application, and its light transmittance and toughness need to be improved.

Method used

PETG-PC alloys were prepared by adding PC resin and specific proportions of nucleating agents, antioxidants, plasticizers, lubricants, transesterification inhibitors and chain extenders to PETG resin and using a twin-screw extruder melt extrusion process, thus optimizing the material composition and processing technology.

Benefits of technology

A PETG-PC alloy material with high light transmittance, good mold release properties, and high toughness has been obtained, which is suitable for optical lighting devices, household cleaning appliances, and medical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003595495950000091
    Figure BDA0003595495950000091
Patent Text Reader

Abstract

The invention discloses a PETG-PC alloy with high light transmittance and high toughness, a preparation method and an application, and relates to the technical field of polymer composite materials. The raw materials of the PETG-PC alloy with high light transmittance and high toughness include: 40-85 parts of PETG resin, 20-50 parts of PC resin, 0.05-0.3 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-2 parts of lubricant, 0.05-0.3 parts of ester exchange inhibitor and 0.05-0.2 parts of chain extender. Utilizing PETG resin and PC resin as main raw materials, with nucleating agent, antioxidant, plasticizer, lubricant, ester exchange inhibitor and chain extender, under the premise of improving the demoulding performance of PETG resin, a composite alloy material with good light transmittance, high chemical resistance, high toughness and low water absorption can also be obtained, which has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, and in particular to a PETG-PC alloy with high light transmittance and high toughness, a preparation method and an application thereof. Background Art

[0002] PETG is a transparent, amorphous copolyester. The commonly used comonomer is 1,4-cyclohexanedimethylene (CHDM), the full name of which is polyethylene terephthalate-1,4-cyclohexanedimethylene ester. It is a product of terephthalic acid (PTA), ethylene glycol (EG) and 1,4-cyclohexanedimethanol (CHDM) by ester exchange. Compared with PET, it has more 1,4-cyclohexanedimethanol comonomer, and compared with PCT, it has more ethylene glycol comonomer. Therefore, the performance of PETG is very different from that of PET and PCT. PETG sheet has outstanding toughness and high impact strength. Its impact strength is 3-10 times that of modified polyacrylates. It has a wide processing range, high mechanical strength and excellent flexibility. Compared with PVC, it has high transparency, good gloss, and a transmittance of more than 90. It is easy to print and has environmental advantages. In addition, the cost of PETG is much lower than that of PCTG.

[0003] However, PETG and PCTG currently generally have the problem of poor demoulding properties, so the processing performance is poor, especially when processing large-sized materials with thick walls, their applications are limited.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a PETG-PC alloy with high light transmittance and high toughness and a preparation method thereof, aiming to obtain an alloy material with good demoulding properties while improving the light transmittance, chemical resistance and toughness of the material.

[0006] Another object of the present invention is to provide the use of the above PETG-PC alloy in the preparation of optical lighting devices, household cleaning appliances or medical devices.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a PETG-PC alloy with high light transmittance and high toughness, wherein the raw materials include: 40-85 parts of PETG resin, 20-50 parts of PC resin, 0.05-0.3 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-2 parts of lubricant, 0.05-0.3 parts of ester exchange inhibitor and 0.05-0.2 parts of chain extender.

[0009] In an optional embodiment, the raw materials include: 60-80 parts of PETG resin, 20-40 parts of PC resin, 0.05-0.1 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-1 parts of lubricant, 0.1-0.3 parts of ester exchange inhibitor and 0.05-0.1 parts of chain extender.

[0010] In an optional embodiment, the PC resin is a transparent PC resin having a melt index of 9-20 g / 10 min and a molecular weight of 22000-25000.

[0011] In an optional embodiment, the nucleating agent is an organic transparent nucleating agent;

[0012] Preferably, the nucleating agent is selected from at least one of sorbitols and metal phosphates.

[0013] In an optional embodiment, the antioxidant is selected from at least one of antioxidant 1076, antioxidant 168, antioxidant 626 and antioxidant 9228.

[0014] In an optional embodiment, the plasticizer is a synthetic ether ester plasticizer;

[0015] Preferably, the plasticizer is selected from at least one of RS-107 plasticizer, RS-700 plasticizer and RS-705 plasticizer.

[0016] In an optional embodiment, the lubricant is selected from at least one of ethylene bisstearamide and pentaerythritol stearate.

[0017] In an optional embodiment, the transesterification inhibitor is at least one of sodium dihydrogen phosphate and phosphate esters;

[0018] Preferably, the chain extender is selected from at least one of bifunctional acid derivatives, isocyanate compounds, anhydride compounds and epoxides.

[0019] In a second aspect, the present invention provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, which is prepared using the raw material of the PETG-PC alloy of any one of the aforementioned embodiments;

[0020] Preferably, the preparation method comprises: uniformly mixing the raw materials, granulating and drying the raw materials after melt extrusion;

[0021] Preferably, the PETG resin is first mixed with a plasticizer, and then mixed evenly with other raw materials, and melt-extruded using a twin-screw extruder;

[0022] Preferably, the twin-screw extrusion temperature is 150-235°C, and the main engine speed is 200-400rpm.

[0023] In a third aspect, the present invention provides the use of the PETG-PC alloy of any one of the aforementioned embodiments or the PETG-PC alloy prepared by the preparation method of the aforementioned embodiment in the preparation of optical lighting devices, household cleaning appliances and medical devices.

[0024] The invention has the following beneficial effects: PETG resin and PC resin are used as main raw materials, and a nucleating agent, an antioxidant, a plasticizer, a lubricant, an ester exchange inhibitor and a chain extender are added. On the premise of improving the demoulding performance of the PETG resin, a composite alloy material with good light transmittance, high chemical resistance, high toughness and low water absorption can be obtained, and the composite alloy material has broad application prospects. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] The embodiment of the present invention provides a PETG-PC alloy with high light transmittance and high toughness. The raw materials of the alloy include: 40-85 parts of PETG resin, 20-50 parts of PC resin, 0.05-0.3 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-2 parts of lubricant, 0.05-0.3 parts of ester exchange inhibitor and 0.05-0.2 parts of chain extender.

[0027] Specifically, PC resin (polycarbonate) is an amorphous polymer that becomes a transparent glass after melting and cooling, and has excellent optical and mechanical properties. It has a high melting point, is also resistant to low temperatures, has low water absorption, has good impact resistance, insulation and aging resistance, and can withstand inorganic and organic dilute acids. In addition, PC has good processing performance and high light transmittance.

[0028] It should be noted that the inventors added a specific proportion of PC resin to the PETG resin and combined it with other additives to improve the demoulding property of PETG without reducing the impact performance and at the same time without affecting the light transmittance. The light transmittance of the PETG / PC alloy prepared by the embodiment of the present invention can reach more than 85%, which is equivalent to the transparent ABS pure raw material. The composite material prepared by the embodiment of the present invention can be used in the fields of preparing optical lighting devices, household cleaning appliances and medical devices.

[0029] It is particularly pointed out that if PETG resin and PC resin are directly blended, transparent materials cannot be made, and are usually milky white and translucent, and cannot be used. The embodiment of the present invention adds additives and special processes to make the transparency of the prepared alloy material reach more than 85%, and the processing and forming performance is very excellent.

[0030] In a preferred embodiment, the raw materials of the PETG-PC alloy include: 60-80 parts of PETG resin, 20-40 parts of PC resin, 0.05-0.1 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-1 parts of lubricant, 0.1-0.3 parts of transesterification inhibitor and 0.05-0.1 parts of chain extender. By optimizing the amount of each raw material, the light transmittance and toughness of the composite material can be further improved.

[0031] Specifically, the PETG resin is polyethylene terephthalate-1,4-cyclohexanedimethanol, and the specific brands may be S2008, K2012, PN-100, and P-SF of South Korea's SK.

[0032] Specifically, the PC resin is a highly transparent PC resin with a melt index of 9-20 g / 10 min and a molecular weight of 22000-25000, and a light transmittance of 88-90%.

[0033] Furthermore, the nucleating agent is an organic transparent nucleating agent, which can change the crystallization behavior of the resin, accelerate the crystallization rate, increase the crystal density and promote the miniaturization of the grain size, thereby achieving the purpose of shortening the molding cycle and improving the transparency of the product. Specifically, the nucleating agent is selected from at least one of sorbitols and phosphate metal salts, and can be one or more. Specifically, the sorbitol can be general sorbitol, and the organic phosphate can be sodium organic phosphate, etc.

[0034] Further, the antioxidant is selected from at least one of antioxidant 1076, antioxidant 168, antioxidant 626 and antioxidant 9228. The addition of the antioxidant can significantly improve the chemical resistance of the composite material, and obtain a composite material with high chemical resistance. The above several types of antioxidants are suitable for the formulation system of the embodiment of the present invention, which is conducive to obtaining a composite material with high chemical resistance. The type of antioxidant can be one or more.

[0035] Furthermore, the plasticizer is a synthetic ether ester plasticizer. General synthetic ether ester plasticizers are suitable for the embodiments of the present invention. The addition of the plasticizer can improve the flexibility of the material and make the material easy to process. Specifically, the plasticizer is selected from at least one of RS-107 plasticizer, RS-700 plasticizer and RS-705 plasticizer, and can be one or more. The above types of plasticizers can all be purchased from Aidico.

[0036] Furthermore, the lubricant is selected from at least one of ethylene bis stearamide (EBS) and pentaerythritol stearate (PETS), and may be one or more. The addition of the lubricant is beneficial to improving the extrusion and demoulding performance of the material, avoiding the material from being decomposed by friction and shearing with the twin screw during the extrusion process, and the lubricant also has the effect of assisting demoulding.

[0037] Furthermore, the transesterification inhibitor is at least one of sodium dihydrogen phosphate and phosphate esters, and may be one or more. The addition of the transesterification inhibitor can inhibit the transesterification reaction between PETG and PC during melt extrusion, thereby affecting the light transmittance and other properties of the composite material.

[0038] Further, the chain extender is selected from at least one of bifunctional acid derivatives, isocyanate compounds, anhydride compounds and epoxides, and may be one or more, specifically BASF chain extenders Joncryl ADR4400, ADR4468, etc. Specifically, the bifunctional compound of the chain extender contains functional groups that are easily reactive with carboxyl, hydroxyl and amino groups, etc., and can directly react with low molecular weight oligomers to form a "bridge" between two polymer chains, significantly increase the molecular weight, improve the viscosity of the system, and reduce the end group content of the copolyester.

[0039] The embodiment of the present invention also provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, which is prepared by using the raw materials of the above-mentioned PETG-PC alloy and a composite material with high light transmittance and good toughness can be obtained through a conventional extrusion process.

[0040] In some embodiments, the preparation method includes: mixing the raw materials uniformly, granulating and drying after melt extrusion to obtain a composite material that meets the particle size requirements.

[0041] In actual operation, PETG resin can be added to the mixer first, and then the plasticizer can be added and mixed at medium speed for about 2 minutes, and then mixed with other raw materials at medium speed for about 2 minutes, so as to achieve the purpose of mixing the raw materials evenly. Then, the evenly mixed raw materials are melt-extruded by a twin-screw extruder; the twin-screw extrusion temperature is 150-235℃, and the main engine speed is 200-400rpm.

[0042] Specifically, the twin-screw extrusion temperature can be 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, etc., or any value between the above adjacent temperature values. The main engine speed can be 200rpm, 250rpm, 300rpm, 350rpm, 400rpm, etc., or any value between the above adjacent speed values.

[0043] The present invention implements PETG-PC alloy

[0044] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0045] Example 1

[0046] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, and the specific steps are as follows:

[0047] Ingredients: 70 parts of PETG resin, 28 parts of PC resin, 0.1 parts of nucleating agent (sorbitol), 0.2 parts of antioxidant 1076, 0.2 parts of antioxidant 168, 1 part of plasticizer (RS-107 from Aidico), 0.3 parts of lubricant PETS, 0.15 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.05 parts of chain extender (Joncryl ADR4400).

[0048] Mixing: After adding PETG resin into the mixer, add the plasticizer in the above proportion, stir at 60r / min for 2 minutes, then add PC resin and other additives mentioned above, stir at 60r / min for 2 minutes, and discharge the material.

[0049] Extrusion: twin-screw extrusion is adopted, extrusion temperature: zones 1-10 are set to 150℃ / 220℃ / 220℃ / 220℃ / 225℃ / 235℃ / 235℃ / 235℃ / 230℃ / die: 235℃, and the main engine speed is 240rpm.

[0050] Example 2

[0051] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, and the specific steps are as follows:

[0052] Ingredients: 70 parts of PETG resin, 28 parts of PC resin, 0.05 parts of nucleating agent (sorbitol), 0.2 parts of antioxidant 1076, 0.2 parts of antioxidant 168, 1 part of plasticizer (RS-107 from Aidico), 0.3 parts of lubricant PETS, 0.15 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.05 parts of chain extender (Joncryl ADR4400).

[0053] Mixing: The steps and parameters are the same as those in Example 1.

[0054] Extrusion: Same parameters as in Example 1.

[0055] Example 3

[0056] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, and the specific steps are as follows:

[0057] Ingredients: 63 parts of PETG resin, 35 parts of PC resin, 0.05 parts of nucleating agent (sorbitol), 0.2 parts of antioxidant 1076, 0.2 parts of antioxidant 168, 1 part of plasticizer (RS-107 from Aidico), 0.3 parts of lubricant PETS, 0.15 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.05 parts of chain extender (Joncryl ADR4400).

[0058] Mixing: The steps and parameters are the same as those in Example 1.

[0059] Extrusion: twin-screw extrusion, extrusion temperature: 180℃ / 230℃ / 230℃ / 230℃ / 235℃ / 240℃ / 240℃ / 240℃ / 240℃ / 240℃ / die: 245℃, main engine speed: 280rpm.

[0060] Example 4

[0061] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, and the specific steps are as follows:

[0062] Ingredients: 78 parts of PETG resin, 20 parts of PC resin, 0.05 parts of nucleating agent (sorbitol), 0.2 parts of antioxidant 1076, 0.2 parts of antioxidant 168, 1 part of plasticizer (RS-107 from Aidico), 0.3 parts of lubricant PETS, 0.3 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.05 parts of chain extender (Joncryl ADR4400).

[0063] Mixing: The steps and parameters are the same as those in Example 1.

[0064] Extrusion: Same parameters as in Example 1.

[0065] Example 5

[0066] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, which is different from the embodiment 1 only in the batching steps, which are as follows:

[0067] 40 parts of PETG resin, 20 parts of PC resin, 0.05 parts of nucleating agent (sorbitol), 0.1 parts of antioxidant 1076, 1 part of plasticizer (RS-107 from Aidico), 0.3 parts of lubricant PETS, 0.05 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.05 parts of chain extender (Joncryl ADR4400).

[0068] Example 6

[0069] This embodiment provides a method for preparing a PETG-PC alloy with high light transmittance and high toughness, which is different from the embodiment 1 only in the batching steps, which are as follows:

[0070] 85 parts of PETG resin, 50 parts of PC resin, 0.3 parts of nucleating agent (sorbitol), 0.4 parts of antioxidant 1076, 3 parts of plasticizer (RS-107 of Aidico), 2 parts of lubricant PETS, 0.3 parts of ester exchange inhibitor (sodium dihydrogen phosphate), and 0.2 parts of chain extender (Joncryl ADR4400).

[0071] Comparative Example 1

[0072] The only difference from Example 1 is that no nucleating agent, plasticizer, transesterification inhibitor and chain extender are added.

[0073] Comparative Example 2

[0074] The only difference from Example 1 is that no transesterification inhibitor and chain extender are added.

[0075] Comparative Example 3

[0076] The only difference from Example 1 is that the amount of the transesterification inhibitor used is 0.005 parts.

[0077] Comparative Example 4

[0078] The only difference from Example 1 is that the amount of the transesterification inhibitor used is 0.5 parts.

[0079] Test Example 1

[0080] The tensile strength, impact strength, flexural strength, flexural modulus, water absorption, molding shrinkage, melt index and light transmittance of the composite materials prepared in the test examples and comparative examples are shown in Table 1. The test methods refer to ISO international standards.

[0081] Table 1 Performance test results of composite materials

[0082]

[0083] In summary, the present invention provides a PETG-PC alloy with high light transmittance and high toughness, as well as a preparation method and application. PC is added to the PETG system, and the transparency of the alloy material prepared by adding additives and special processes can reach more than 85%, and the light transmittance is basically equivalent to that of the raw materials, and the processing and molding demolding performance of the material is improved. PC can improve the tensile strength and impact strength of PETG, and PETG can improve the solvent resistance and processing fluidity of PC; PC and PETG are blended to obtain a high-transparency alloy with excellent mechanical properties, processing properties and solvent resistance.

[0084] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A PETG-PC alloy with high light transmittance and high toughness, characterized in that: The raw materials include: 40-85 parts of PETG resin, 20-50 parts of PC resin, 0.05-0.3 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-2 parts of lubricant, 0.05-0.3 parts of ester exchange inhibitor and 0.05-0.2 parts of chain extender; The nucleating agent is an organic transparent nucleating agent; The plasticizer is a synthetic ether ester plasticizer; The transesterification inhibitor is at least one of sodium dihydrogen phosphate and phosphate esters; The chain extender is selected from at least one of bifunctional acid derivatives, isocyanate compounds, anhydride compounds and epoxides.

2. The PETG-PC alloy according to claim 1, characterized in that The raw materials include: 60-80 parts of PETG resin, 20-40 parts of PC resin, 0.05-0.1 parts of nucleating agent, 0.1-0.4 parts of antioxidant, 1-3 parts of plasticizer, 0.3-1 parts of lubricant, 0.1-0.3 parts of ester exchange inhibitor and 0.05-0.1 parts of chain extender.

3. The PETG-PC alloy according to claim 1 or 2, characterized in that The PC resin is a transparent PC resin with a melt index of 9-20 g / 10 min and a molecular weight of 22000-25000.

4. The PETG-PC alloy according to claim 1 or 2, characterized in that The nucleating agent is selected from at least one of sorbitols and metal phosphates.

5. The PETG-PC alloy according to claim 1 or 2, characterized in that The antioxidant is selected from at least one of antioxidant 1076, antioxidant 168, antioxidant 626 and antioxidant 9228.

6. The PETG-PC alloy according to claim 1 or 2, characterized in that The plasticizer is selected from at least one of RS-107 plasticizer, RS-700 plasticizer and RS-705 plasticizer.

7. The PETG-PC alloy according to claim 1 or 2, characterized in that The lubricant is selected from at least one of ethylene bisstearamide and pentaerythritol stearate.

8. A method for preparing a PETG-PC alloy with high light transmittance and high toughness, characterized in that: The method is prepared by using the raw material of the PETG-PC alloy described in any one of claims 1 to 7.

9. The preparation method according to claim 8, characterized in that: The preparation method comprises: uniformly mixing various raw materials, melting and extruding, and then granulating and drying.

10. The preparation method according to claim 9, characterized in that: First, mix the PETG resin with the plasticizer, then mix it evenly with other raw materials, and use a twin-screw extruder for melt extrusion.

11. The preparation method according to claim 10, characterized in that: The twin-screw extrusion temperature is 150-235°C and the main engine speed is 200-400rpm.

12. Use of the PETG-PC alloy according to any one of claims 1 to 7 or the PETG-PC alloy prepared by the preparation method according to any one of claims 8 to 11 in the preparation of optical lighting devices, household cleaning appliances and medical devices.

Citation Information

Patent Citations

  • PC / PETG alloy material and preparation method thereof

    CN104672880A

  • 3D-printing PC / PETG special material and preparation method thereof

    CN107383830A

  • Flame-retardant photodiffusion polyester material and preparation method and application thereof

    CN109438930A

  • Transparent PC / polyester alloy capable of being subjected to low-temperature injection molding and preparation method thereof

    CN111849141A

  • Polycarbonate / polyester alloy as well as preparation method and application thereof

    CN112226061A