A hydrated salt thermochemical heat storage composite material and its preparation method and application
By using a composite material of a highly thermally conductive porous adsorption carrier and a hydrated salt heat storage material in the lithium-ion battery module, the problems of thermal runaway and thermal runaway spread of lithium-ion batteries are solved, and the efficient heat storage effect matching the thermal runaway temperature of the battery is achieved , and simplifies the modeling process of thermochemical thermal storage models.
Patent Information
- Application Number
- CN202210193382.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The prior art is difficult to effectively alleviate the thermal runaway and thermal runaway spread of lithium-ion batteries, especially because the heat release is huge during thermal runaway, and the phase change temperature of existing endothermic phase change materials does not match the starting temperature of thermal runaway, and thermochemistry is also used. The heat storage model is complex and cumbersome, and it is difficult to be suitable for rapid heating and decomposition scenarios.
Composite materials using high thermal conductivity porous adsorption carrier and hydrated salt heat storage materials, including hydrophilic modified expanded graphite, hydrated salt heat storage materials and reinforced materials, describe their thermal chemical heat storage process through a simple thermochemical heat storage model, using Fill in the battery module to alleviate thermal runaway and curb the spread of thermal runaway.
The prepared hydrated salt thermochemical heat storage composite has a high latent heat value between 34 and 60°C and a large decomposition enthalpy between 85 and 110°C. It matches the thermal runaway temperature of the battery and has good thermal conductivity and compressive strength. , can effectively alleviate the thermal runaway from the battery and accurately describe the heat storage, simplifying the model modeling process.
Smart Images

Figure CN114539983B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of thermochemical heat storage and battery thermal runaway, and relates to a hydrated salt thermochemical heat storage composite material and a preparation method and application thereof. The application relates to a thermochemical heat storage model and an establishment process thereof. Background Art
[0002] With the large-scale application of lithium-ion batteries and the continuous improvement of lithium-ion battery capacity, lithium-ion battery accidents continue to occur frequently, such as electric vehicle battery packs damaged and catching fire, and energy storage power station battery modules catching fire. When lithium-ion batteries are subjected to thermal abuse, electrical abuse, and mechanical abuse, the internal substances continue to decompose and generate heat, causing the battery temperature to continue to rise, thereby causing thermal runaway and the spread of thermal runaway. Some literature points out that the decomposition process of internal battery substances is mainly divided into four parts: SEI film decomposition occurs at 70-120°C, negative electrode decomposition occurs at 120-200°C, positive electrode decomposition occurs at 200-230°C, and electrolyte decomposition occurs at 230-243°C. After a series of reactions, the temperature of the battery can reach 700°C or above, which is seriously harmful (Qingsong Wang, et al. A review of lithium ion battery failure mechanisms and fire prevention strategies [J]. Progress in Energy and Combustion Science, 2019, 73: 95-131). Therefore, how to alleviate battery thermal runaway and curb the spread of battery thermal runaway is an important research area.
[0003] Current solutions can be divided into internal measures and external measures. Internal measures are to improve the stability of battery electrodes, electrolytes, and separators, thereby increasing the critical temperature point at which the battery undergoes irreversible thermal runaway, such as microencapsulation of electrode materials (Jinyun Liu, et al. A Polysulfides-Confined All-in-One Porous Microcapsule Lithium–Sulfur Battery Cathode [J]. Small, 2021, 17 (41), 2103051), adding flame retardants to electrolytes (L. Kong, et al. Li-ion battery fire hazards and safety strategies [J]. Energies, 2018, 11: 1-11), and selecting ceramic separators or multilayer separators (C. O. Rendorff, et al. The role of separators in lithium-ion cell safety [J]. Electrochem Soc Inter face, 2012, 12: 61-65), etc. However, the process is complex and costly, there are many types of batteries and no unified measurement standard, and the universality is poor. In addition, when the battery cell is subjected to mechanical abuse, the structure is damaged, and thermal runaway has occurred, the internal measures are not very effective in curbing the spread of thermal runaway. The external measures are to remove the large amount of heat generated by the thermal runaway of the single cell, and try not to affect the adjacent batteries to avoid the spread of thermal runaway. External measures can be roughly divided into the following two types: one is to set an insulation layer between battery cells, such as an aerogel layer, and use air cooling or liquid cooling to remove heat; however, air cooling can basically not curb the spread of thermal runaway, but will promote the spread of thermal runaway (Zhang Zhihong, Mou Junyan, Meng Yufa, Thermal runaway expansion characteristics of air-cooled cylindrical lithium-ion battery system [J]. Energy Storage Science and Technology, 2021, 10(02): 658-663); liquid cooling can alleviate thermal runaway and curb the spread of thermal runaway, but it has high requirements on the sealing performance of cooling components. In addition, due to the huge heat release of battery thermal runaway, the coolant flow, pump power, and pressure drop will increase rapidly, causing great loss to the liquid cooling components (Xu J, Lan C, et al. Prevent thermal runaway of lithium-ion batteries with minichannel cooling. Applied Thermal Engineering. 2017, 110: 883-90); in addition, battery thermal runaway is accompanied by gas injection, which can easily damage the liquid cooling components and cause coolant leakage.The second is to fill low thermal conductivity endothermic phase change materials or high thermal conductivity endothermic phase change materials between battery cells to alleviate thermal runaway and thermal runaway propagation through the heat storage process of the material itself. Basically, it is a composite material of fumed silica or expanded graphite and paraffin phase change materials (Wilke S, Schweitzer B, et al. Preventing thermal runaway propagation in lithium ion battery packs using a phase change composite material: An experimental study. Journal of Power Sources. 2017; 340: 51-9). Its solid-liquid phase transition temperature is lower than 50°C, which is much lower than the thermal runaway starting temperature of the battery (120°C). Its phase change latent heat value is 150J / g, which is much lower than the heat released when the battery thermally runs away (~880J / g). Therefore, the effect of alleviating the spread of thermal runaway is general. Compared with air cooling and liquid cooling, filling endothermic phase change materials does not require an additional power source between batteries and is more convenient in structure, but it is necessary to find a material with a phase change temperature that matches the starting temperature of thermal runaway and a large phase change enthalpy value.
[0004] Hydrated salt materials will undergo thermal decomposition at high temperatures (around 100°C), and their crystal water will evaporate and escape, taking away a large amount of heat. Common hydrated salt thermochemical heat storage models are all kinetic models, and their modeling methods are to test the heating decomposition of materials at different temperature rise rates (such as 5K / min, 10K / min, 15K / min, etc.), and then calculate its activation energy, pre-exponential factor and other parameters through the Arrhenius formula. The obtained model parameters are extremely dependent on the material test conditions, and the calculation is cumbersome. In addition, the heat released during thermal runaway of the battery is huge, and the material is heated quickly. The test heating rate is difficult to match the actual application scenario, and the obtained thermochemical heat storage model may not be applicable to the actual situation where the material is rapidly heated and decomposed. Therefore, a simpler and more effective thermochemical heat storage model is needed to describe the thermochemical heat storage process of hydrated salts. Summary of the invention
[0005] The present invention aims to provide a hydrated salt thermochemical heat storage composite material and a preparation method thereof, whose decomposition temperature is relatively matched with the starting temperature of battery thermal runaway and whose decomposition enthalpy value is relatively large, and fill it between battery modules to alleviate battery thermal runaway and curb the spread of thermal runaway.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] The invention provides a hydrated salt thermochemical heat storage composite material. The composite material comprises a high thermal conductivity porous adsorption carrier, a hydrated salt heat storage material and a reinforcing material.
[0008] The highly thermally conductive porous adsorption carrier serves as the basic supporting skeleton, which not only provides a thermal conductive path but also prevents the leakage of hydrated salts.
[0009] Preferably, the high thermal conductivity porous adsorption carrier is one of hydrophilic modified expanded graphite, hydrophilic modified silicon nitride and hydrophilic modified silicon carbide, accounting for 10% to 20% of the total amount.
[0010] The hydrated salt heat storage material is filled in the carrier to play a role in thermochemical heat storage.
[0011] Preferably, the hydrated salt heat storage material is a mixed salt of disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate, the mass proportion of disodium hydrogen phosphate dodecahydrate is 90% to 98%, the mass proportion of sodium acetate trihydrate is 2% to 10%; the mixed salt accounts for 70% to 80% of the total amount.
[0012] The reinforcement material is used to enhance the thermal conductivity path and the mechanical properties of the enhanced material after pressing and forming.
[0013] Preferably, the reinforcing material is one or more of alumina fiber, aluminum nitride fiber, carbon fiber, alumina particles, and fine graphite powder, accounting for 5-10% of the total amount.
[0014] The present invention provides a method for preparing the above-mentioned hydrated salt thermochemical heat storage composite material, comprising the following steps:
[0015] (1) drying one of expanded graphite, silicon nitride powder, and silicon carbide powder and mixing it with a surfactant, sealing, heating, and stirring, and then drying to obtain a high thermal conductivity porous adsorption carrier material for standby use;
[0016] (2) dissolving disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate in water respectively, blending and completely melting them to obtain a hydrated salt heat storage material for standby use;
[0017] (3) Drying the reinforcement material for later use;
[0018] (4) The high thermal conductivity porous adsorption carrier material, the hydrated salt heat storage material, and the reinforcing material are sealed together, heated, and stirred, and then cooled and stirred to obtain the hydrated salt thermochemical heat storage composite material.
[0019] Preferably, the drying temperature in step (1) is 100-120° C., and the drying time is 24-48 hours.
[0020] Preferably, the surfactant in step (1) is Tween 60 or octylphenyl polyoxyethylene ether.
[0021] Preferably, the heating and stirring temperature in step (1) is 60 to 70° C., and the heating and stirring time is 1 to 3 hours.
[0022] Preferably, the melting temperature in step (2) is 60-70°C.
[0023] Preferably, the drying temperature in step (3) is 100-120° C., and the drying time is 24-48 hours.
[0024] Preferably, the heating and stirring temperature in step (4) is 60-70° C., and the heating and stirring time is 4-6 hours; the cooling temperature in step (4) is 10-20° C., and the stirring time is 1-2 hours.
[0025] The present invention also provides application of the above-mentioned hydrated salt thermochemical heat storage composite material in battery thermal runaway protection.
[0026] In addition, the present invention also provides a simple and effective hydrated salt thermochemical heat storage model, which is used to describe the thermochemical heat storage process of the hydrated salt thermochemical heat storage composite material by constructing the hydrated salt thermochemical heat storage model, so as to optimize the usage of the hydrated salt thermochemical heat storage composite material in the module and estimate the temperature in the case of thermal runaway of the battery.
[0027] The hydrated salt thermochemical heat storage model is a lumped model, which combines the sensible heat and latent heat of the material into apparent specific heat capacity, and regards the thermochemical heat storage process as a quasi-linear process related to the thermochemical decomposition starting temperature, end temperature, decomposition enthalpy, and real-time temperature.
[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0029] (1) The hydrated salt thermochemical heat storage composite material prepared by the present invention has a latent heat value of 110 to 150 J / g at 34 to 60°C and a decomposition enthalpy of 1100 to 1300 J / g at 85 to 110°C; its decomposition temperature and decomposition enthalpy are relatively consistent with the starting temperature of battery thermal runaway and the unit heat release during runaway.
[0030] (2) The hydrated salt thermochemical heat storage composite material prepared by the present invention can be filled in a battery module. When the battery is subjected to electrical abuse, mechanical abuse, or thermal abuse and thermal runaway occurs, the thermal runaway of the battery can be effectively alleviated and the spread of the thermal runaway can be curbed.
[0031] (3) The hydrated salt thermochemical heat storage composite material prepared by the present invention has good thermal conductivity (density of 600-1000 kg / m 3 When the thermal conductivity is 6.26~14.56W / (m·K)) and compressive strength.
[0032] (4) The relative error between the simulation results of the hydrated salt thermochemical heat storage model proposed in the present invention and the experimental results does not exceed 5%. The model can accurately describe the heat storage capacity of the material and is simpler and more effective than the commonly used complicated kinetic models that describe thermochemical processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The DSC-TG graph of the hydrated salt thermochemical heat storage composite material obtained in Example 1;
[0034] Figure 2 The thermal conductivity diagram of the hydrated salt thermochemical heat storage composite material obtained in Example 1 at different densities;
[0035] Figure 3 This is a diagram of the compressive strength of the hydrated salt thermochemical heat storage composite material obtained in Example 1;
[0036] Figure 4 This is a diagram of the modeling process of the hydrated salt thermochemical heat storage model;
[0037] Figure 5 The actual temperature curve of the hydrated salt thermochemical heat storage composite material obtained in Example 1 in the battery module and the simulated temperature curve predicted by the model in the hydrated salt thermochemical heat storage model. DETAILED DESCRIPTION
[0038] Example 1
[0039] (1) Select 100 mesh expanded graphite and place it in a 120°C oven for 24 hours to remove the moisture adsorbed from the air. Mix the expanded graphite and Tween 60 in a sealed stirring tank at a mass ratio of 96:4 and stir at 60°C for 3 hours, wherein Tween 60 must first be dissolved in pure water and ensure that the Tween 60 aqueous solution completely wets the expanded graphite. Then, dry the modified expanded graphite in a 120°C oven for 24 hours to remove the modifier, thereby obtaining hydrophilic modified expanded graphite.
[0040] (2) Disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate were mixed in a mass ratio of 97:3 and completely melted in an oven at 65° C.; and the alumina fibers cut into small pieces were dried in an oven at 120° C. for 24 hours.
[0041] (3) The hydrophilic modified expanded graphite, the blended salt, and the alumina fiber were mixed in a sealed stirring kettle in a ratio of 20:70:10, and stirred at 70° C. for 4 h; and then stirred at 10° C. for 1 h. Thus, the hydrated salt thermochemical heat storage composite material was obtained.
[0042] Figure 1This is the DSC-TG graph of the hydrated salt thermochemical heat storage composite material obtained in Example 1. The thermochemical heat storage composite material has a latent heat value of 116 J / g at 34-60°C and a decomposition enthalpy of 1100 J / g at 85-110°C. Figure 2 The thermal conductivity diagram of the hydrated salt thermochemical heat storage composite material obtained in Example 1 is as follows: Figure 2 As shown, the thermochemical heat storage composite material has a density of 600 kg / m 3 , 700kg / m 3 , 800kg / m 3 , 900kg / m 3 , 1000kg / m 3 The thermal conductivity is 6.26W / (m·K), 9.21W / (m·K), 10.97W / (m·K), 12.71W / (m·K), and 14.56W / (m·K), respectively, which can quickly guide the heat to the entire module to avoid heat accumulation. Figure 3 The compressive strength diagram of the hydrated salt thermochemical heat storage composite material obtained in Example 1 is shown in FIG. Figure 3 It can be seen that compared with paraffin-based endothermic materials, hydrated salt thermochemical heat storage composite materials have better compressive resistance, which can effectively resist the pressure shock caused by battery out of control and avoid serious damage to the entire material.
[0043] Example 2
[0044] (1) Select 50 mesh expanded graphite and place the expanded graphite in a 100°C oven for 48 hours to remove the moisture adsorbed from the air. Mix the expanded graphite and octylphenyl polyoxyethylene ether in a sealed stirring tank at a mass ratio of 96:4 and stir at 65°C for 2 hours, wherein the octylphenyl polyoxyethylene ether must be dissolved in pure water first, and ensure that the aqueous solution of octylphenyl polyoxyethylene ether completely wets the expanded graphite. Subsequently, the modified expanded graphite is dried in a 110°C oven for 36 hours to remove the modifier, thereby obtaining hydrophilic modified expanded graphite.
[0045] (2) Disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate were mixed in a mass ratio of 90:10 and completely melted in an oven at 70° C.; aluminum nitride fibers cut into small pieces were dried in an oven at 110° C. for 36 hours.
[0046] (3) The hydrophilic modified expanded graphite, the blended salt, and the aluminum nitride fiber were mixed in a sealed stirring kettle in a ratio of 10:80:10, and stirred at 65° C. for 5 h; and then stirred at 15° C. for 1.5 h. Thus, the hydrated salt thermochemical heat storage composite material was obtained.
[0047] The thermochemical heat storage composite material obtained in this example has a latent heat value of 132 J / g at 34-60°C and a decomposition enthalpy of 1250 J / g at 85-110°C; its DSC-TG graph is Figure 1 Similar; its thermal conductivity is similar to that of Example 1.
[0048] Example 3
[0049] (1) Select silicon carbide powder and place it in a 110°C oven for 36 hours to remove the moisture adsorbed from the air. Mix silicon carbide and Tween 60 in a sealed stirring vessel at a mass ratio of 96:4 and stir at 70°C for 1 hour. Tween 60 must first be dissolved in pure water and ensure that the Tween 60 aqueous solution completely wets the silicon carbide powder. Then, dry the modified silicon carbide in a 100°C oven for 48 hours to remove the modifier, thereby obtaining hydrophilic modified silicon carbide.
[0050] (2) Disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate were mixed in a mass ratio of 98:2 and completely melted in an oven at 60° C.; and the alumina fibers cut into small pieces were dried in an oven at 100° C. for 48 hours.
[0051] (3) The hydrophilic modified silicon carbide, the blended salt, and the alumina fiber were mixed in a sealed stirring kettle in a ratio of 15:80:5, and stirred at 60° C. for 6 hours; and then stirred at 20° C. for 2 hours. Thus, the hydrated salt thermochemical heat storage composite material was obtained.
[0052] The thermochemical heat storage composite material obtained in this example has a latent heat value of 130 J / g at 34-60°C and a decomposition enthalpy of 1230 J / g at 85-100°C; its DSC-TG graph is Figure 1 Similar; its thermal conductivity is similar to that of Example 1.
[0053] Example 4
[0054] The hydrated salt thermochemical heat storage material obtained in Example 1 was heated at 600 kg / m 3 The density is pressed into a block with a length, width and height of 125mm*110mm*57mm. There are 20 4*5 holes with a diameter of 18mm in total, and the hole spacing is 7mm. 18650 batteries with a diameter of 18mm and a height of 65mm are placed in each hole. The battery is triggered to have thermal runaway, such as Figure 5 As shown, its maximum temperature is about 130°C, far below 700°C, and the temperatures of adjacent batteries (adjacent electric heating rods) are all below 100°C, indicating that the hydrated salt thermochemical heat storage composite material can effectively alleviate battery thermal runaway and inhibit the spread of thermal runaway.
[0055] Figure 4This is a modeling process diagram of the hydrated salt thermochemical heat storage model. The total heat storage consists of sensible heat storage, latent heat storage and thermochemical heat storage. The thermochemical heat storage process is regarded as a quasi-linear process, which is only related to the decomposition starting temperature, end temperature, decomposition enthalpy and real-time temperature. The latent heat storage and sensible heat storage are combined into apparent specific heat capacity. The hydrated salt thermochemical heat storage composite material obtained in Example 1 was subjected to TG-DSC test, and the decomposition starting temperature was 85°C, the decomposition end temperature was 110°C, and the decomposition enthalpy was 1100 J / g; according to Figure 4 The modeling process diagram of the thermochemical decomposition process is Where T is the real-time temperature of the material; the temperature curve predicted by the model is as follows Figure 5 As shown, the degree of agreement with the actual temperature curve is very high, indicating that the modeling method can effectively predict the temperature changes of batteries and materials, and is reliable and simple.
[0056] pass Figure 4 The established model optimizes the block of the hydrated salt thermochemical heat storage composite material obtained in Example 1. At a compaction density of 600kg / m3, a module of 100 18650 batteries is placed, and the hydrated salt thermochemical heat storage composite material is filled between the batteries, shortening the battery spacing to 3mm. By optimizing the amount of hydrated salt thermochemical heat storage composite material in the module through this model, it can still ensure that the thermal runaway triggering battery temperature is around 140°C and the surrounding battery temperature is not lower than 100°C.
[0057] The above embodiments are used to illustrate the present invention, and the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a hydrated salt thermochemical heat storage composite material, characterized in that: The steps include: (1) drying one of silicon nitride powder and silicon carbide powder and mixing it with a surfactant, sealing, heating and stirring, and then drying to obtain a high thermal conductivity porous adsorption carrier material for standby use; (2) dissolving disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate in water respectively, blending and completely melting them to obtain a hydrated salt heat storage material for standby use; (3) Drying the reinforcement material for later use; (4) sealing the high thermal conductivity porous adsorption carrier material, the hydrated salt heat storage material, and the reinforcing material together, heating and stirring, and then cooling and stirring to obtain the hydrated salt thermochemical heat storage composite material; The drying temperature in step (1) is 100-120° C., and the drying time is 24-48 hours; the surfactant in step (1) is Tween 60 or octylphenyl polyoxyethylene ether; the heating and stirring temperature in step (1) is 60-70° C., and the heating and stirring time is 1-3 hours; The melting temperature in step (2) is 60-70° C.; the drying temperature in step (3) is 100-120° C., and the drying time is 24-48 hours; The heating and stirring temperature in step (4) is 60-70° C., and the heating and stirring time is 4-6 hours; the cooling temperature in step (4) is 10-20° C., and the stirring time is 1-2 hours; The composite material comprises a high thermal conductivity porous adsorption carrier, a hydrated salt heat storage material and a reinforcing material; the high thermal conductivity porous adsorption carrier is one of hydrophilic modified silicon nitride and hydrophilic modified silicon carbide; the hydrated salt heat storage material is a mixed salt of disodium hydrogen phosphate dodecahydrate and sodium acetate trihydrate; the mass proportion of disodium hydrogen phosphate dodecahydrate is 90% to 98%, and the mass proportion of sodium acetate trihydrate is 2% to 10%; the reinforcing material is one or more of alumina fiber, aluminum nitride fiber and alumina particles.
2. An application of the hydrated salt thermochemical heat storage composite material as claimed in claim 1 in battery thermal runaway protection.
3. The use according to claim 2, characterized in that: A hydrated salt thermochemical heat storage model is constructed to describe the thermochemical heat storage process of a hydrated salt thermochemical heat storage composite material; the hydrated salt thermochemical heat storage model combines the sensible heat and latent heat of the material into an apparent specific heat capacity, and regards the thermochemical heat storage process as a quasi-linear process related to the thermochemical decomposition starting temperature, ending temperature, decomposition enthalpy, and real-time temperature.