Method for coating composite substrates
By depositing organic/inorganic hybrid sol-gel primer on organic matrix composites, the problems of substrate erosion and low adhesion caused by thermal spraying are solved, and better coating adhesion and mechanical properties are achieved. in a variety of composite materials.
Patent Information
- Application Number
- CN202080062808.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-27
- Filing Date
- 2020-08-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-08-27
AI Technical Summary
When used on organic matrix composite materials (OMC), existing thermal spraying methods are prone to cause substrate erosion and low adhesion, damage to surface lines and reinforcement fibers, and affect the adhesion of the coating.
Deposit an organic/inorganic hybrid sol-gel primer on the OMC substrate prior to thermal spraying, as a surface preparation or bonding layer, protecting the substrate from sprayed particles, improving the adhesion of the coating, and through appropriate The thermal expansion coefficient enhances the adhesion between the upper layer and the substrate.
Effectively protect OMC substrates from thermal spray damage, improve the adhesion and mechanical properties of the coating, suitable for not only organic matrix composite materials, but also ceramic and metal matrix composite materials, enhancing their adhesion in different types of coating deposition sex.
Smart Images

Figure HDA0003607638860000011 
Figure HDA0003607638860000012
Abstract
Description
[0001] The present invention relates to the field of wet surface treatment of composite substrates, in particular organic matrix composites (OMCs).
[0002] Currently, metal parts on OMC substrates are mainly manufactured by making bonded forged parts. However, this method has limitations and problems in bonding and matching parts.
[0003] To solve these problems, the literature describes the testing of deposits (mainly metals) by different thermal spraying methods such as cold spraying or suspension plasma spraying (SPS). In fact, thermal spraying is a common method on metallic aerospace parts to produce coatings, most often metallic. The principle of thermal spraying methods such as cold spraying or suspension plasma spraying (SPS) or air plasma spraying (APS) or flame spraying (high velocity oxygen fuel (HVOF)) consists in spraying particles heated to a high temperature (i.e., from 180°C to the melting temperature of the particles, depending on the method) at high speed.
[0004] However, in order not to alter the mechanical properties of OMCs, OMCs are subject to temperature and mechanical exposure limits during processing. Therefore, recent attempts published in the literature to deposit on organic matrix composite substrates by thermal spraying almost always result in erosion of the substrate, which may destroy the surface line or deposition of very low adhesion (i.e. <1 MPa). In fact, the use of these methods on OMC substrates mainly leads to damage due to heat and erosion as well as the dynamics of the spraying particles and the heat input. This damage of the first OMC layer is reflected in the exposure of the reinforcement fibers and the non-sticky coating.
[0005] The inventors surprisingly realized that organic matrix composites can be protected by using a sol-gel primer layer, particularly an organic / inorganic hybrid sol-gel, deposited prior to deposition by thermal spraying. This primer layer can be considered as a surface preparation layer or bonding layer before depositing subsequent coatings by thermal spraying.
[0006] This base coat therefore has three functions:
[0007] -1 Protect the OMC substrate from erosion by spraying particles;
[0008] -2 Increase the adhesion of the coating:
[0009] - Adhesion to the OMC substrate (interface 1), mainly due to chemical compatibility
[0010] - and adhesion to the deposits produced by thermal spraying (interface 2), mainly through mechanical anchoring resulting from surface roughness and possible formulation-related chemical interactions;
[0011] -3 Improved adhesion between the OMC substrate and the upper layer obtained by thermal spraying due to the appropriate thermal expansion coefficient.
[0012] The inventors have also realised that such primer coatings may also protect other types of composite materials, such as ceramic matrix composites (CMCs) or metal matrix composites (MMCs).
[0013] They also realized that this primer could improve the adhesion of composites during other types of coating deposition, such as dip coating.
[0014] Therefore, the present invention relates to a coating method for a composite substrate, characterized in that it comprises the following steps:
[0015] a- Preparation of the sol-gel composition by mixing in an aqueous medium, in particular in water or a water / alcohol mixture, more particularly acidified water, for example water acidified by acetic acid or nitric acid:
[0016] 1-at least one metal alkoxide M(OR 1 ) x ,in
[0017] R 1 is C1-C4 alkyl, in particular propyl or butyl,
[0018] M is a metal selected from the group consisting of transition metals, lanthanides, phosphorus, magnesium, tin, zinc, aluminium and antimony, advantageously selected from the group consisting of Cu, Mn, Sn, Fe, Mg, Zn, Al, P, Sb, Zr, Ti, Hf, Ce, Nb, V and Ta, more advantageously selected from the group consisting of Zr, Ti, Al and Sb, even more advantageously selected from the group consisting of Zr, Ti and Al, more particularly the same metal as that of the subsequent coating, in particular deposited by spraying (see step c) below), and
[0019] x is an integer representing the valence of the metal,
[0020] Advantageously, the stirring time is required to hydrolyze and concentrate the organic-inorganic hybrid network, in particular from several minutes to several hours, more particularly from 15 minutes to 5 hours;
[0021] 2- In at least one formula (II) R 3 m Si(OR 2 ) 4-m In the presence of an organoalkoxysilane,
[0022] R 2 represents C1-C4 alkyl, in particular methyl, ethyl or isopropyl,
[0023] m represents an integer selected between 1, 2 and 3, in particular 1,
[0024] And each R 3 Each independently represents a polydimethylsiloxane, C1-C 18 Alkyl, C2-C4 alkenyl, C2-C4 alkynyl, C6-C 10 Aryl, methacryl, methacryl (C1-C 10 alkyl) (e.g., methacryloylpropyl) or methacryloyloxy (C1-C 10 alkyl) (e.g., methacryloyloxypropyl), epoxyalkyl or epoxyalkoxyalkyl, wherein the alkyl is a linear, branched or cyclic C1-C 10 Alkyl and alkoxy are straight or branched C1-C 10 Alkoxy (such as glycidyl and glycidyloxy (C1-C 10 alkyl), especially glycidyloxypropyl), C2-C 10 Haloalkyl (e.g., 3-chloropropyl), C2-C 10 Perhaloalkyl (e.g. perfluoropropyl), C2-C 10 Mercaptoalkyl (e.g. mercaptopropyl), C2-C 10 Aminoalkyl (e.g. aminopropyl), (C2-C 10 aminoalkyl)amino(C2-C 10 alkyl) (e.g. 3-[(2-aminoethyl)amino]propyl), di(C2-C 10 Alkylene)triamino(C2-C 10 alkyl) (e.g. 3-[diethylenetriamino]propyl), imidazolyl-(C2-C 10 Alkyl) and C2-C 10 Iminoalkyl, especially each R 3 Each independently represents a non-hydrolyzable group selected from epoxyalkyl or epoxyalkoxyalkyl, wherein the alkyl is a linear, branched or cyclic C1-C 10 Alkyl and alkoxy are straight or branched C1-C 10 Alkoxy (such as glycidyl and glycidyloxy (C1-C 10 alkyl), especially glycidyloxypropyl) and C2-C 10 aminoalkyl (eg aminopropyl),
[0025] The organoalkoxysilane may advantageously be premixed with an aqueous medium, in particular with water or a water / alcohol mixture, more particularly acidified water, while stirring for the time required for the hydrolysis and condensation of the organic-inorganic hybrid network.
[0026] 3- and the presence of optional oxide or metal particles, such as SiO2, ZrO2, TiO2, Ag, Al, Ti and mixtures thereof, in particular from ZrO2 and TiO2;
[0027] 4- by mixing the composition, in particular for a period of several minutes to several hours, more particularly under stirring, to allow condensation of the organic-inorganic hybrid network;
[0028] b- depositing at least one primer layer on the composite substrate from the sol-gel composition obtained in step a);
[0029] c- and depositing at least one subsequent coating, in particular by spraying, on the composite substrate coated with the base coating obtained in step b).
[0030] The method according to the invention may also comprise a step d) of recovering the coated composite substrate obtained in step c).
[0031] In one embodiment of the present invention, the metal alkoxide of formula (I) according to the present invention is reacted beforehand with an aqueous medium before being brought into the presence of the organoalkoxysilane of formula (II) according to the present invention, the reaction time being in particular the time required for the condensation of the organic-inorganic hybrid network.
[0032] Within the meaning of the present invention, "C1-C4 alkyl" refers to any straight-chain or branched alkyl group containing 1 to 4 carbon atoms. It can thus be methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl or tert-butyl, preferably methyl, ethyl or isopropyl, in particular ethyl or methyl.
[0033] Within the meaning of the present invention, "C1-C 18 "Alkyl" means any straight-chain or branched alkyl group containing 1 to 18 carbon atoms. It can thus be methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl or octadecyl, preferably methyl, ethyl or isopropyl, in particular ethyl or methyl.
[0034] Within the meaning of the present invention, "C1-C 10 "Alkyl" means any straight-chain or branched alkyl group containing 1 to 10 carbon atoms. It can thus be methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, heptyl, octyl, nonyl or decyl, preferably methyl, ethyl or propyl, in particular ethyl or propyl.
[0035] Within the meaning of the present invention, "C2-C4alkenyl" refers to any alkenyl group having 2 to 4 carbon atoms, linear or branched, in particular vinyl, allyl, 1-propenyl, 2-propenyl and butenyl.
[0036] Within the meaning of the present invention, "C2-C4alkynyl" refers to any alkynyl group having 2 to 4 carbon atoms, straight or branched, in particular ethynyl, ethynyl or propargyl.
[0037] In the meaning of the present invention, "non-hydrolyzable group" refers to any group that can not react with water to produce-OH group. The presence of this non-hydrolyzable group in the organoalkoxysilane of formula II makes it possible to introduce organic functions in the Si-OM, Si-O-Si or MOM oxide bond network of the sol-gel material (sol-gel primer), and this organic function is non-reactive (such as alkyl), or reactive and polymerizable (methacryloyloxy, epoxy resin, etc.), which will cause some parts of the material to be fully organic. The sol-gel material (sol-gel primer) thus obtained is so-called "organic / inorganic hybrid sol-gel". Therefore, these functions can regulate the mechanical and thermal properties (more non-damageable and non-fragile than simple Si-OM, Si-O-Si or MOM groups) of the final sol-gel material (sol-gel primer), and can also control the thickness of the layer. In addition, it is ensured that the non-hydrolyzable group of the chemical bond between the sol-gel primer and the composite resin, particularly the OMC, also ensures the adhesion with the substrate, particularly the OMC.
[0038] Within the meaning of the present invention, "C6-C 10 "Aryl" refers to one or more aromatic rings having 6 to 10 carbon atoms, which may be linked or fused. In particular, the aryl group may be a monocyclic or bicyclic group, preferably phenyl or naphthyl.
[0039] Within the meaning of the present invention, the term "condensed organic-inorganic hybrid network" means that each metal alkoxide is polymerized together, each organoalkoxysilane is polymerized together and / or each metal alkoxide is polymerized with each organoalkoxysilane, i.e., forming oxo bridges, such as Si-OM or Si-O-Si or MOM.
[0040] In an advantageous embodiment, the Si / M molar ratio in the sol-gel composition obtained in step a) is between 0.1 and 0.5, advantageously between 0.2 and 0.5, in particular 0.3≤Si / M≤0.5.
[0041] In another advantageous embodiment, the metal alkoxide of formula (I) is selected from aluminum (III) isopropoxide, titanium (IV) butoxide and zirconium (IV) propoxide.
[0042] In another advantageous embodiment, the organoalkoxysilane of formula (II) is selected from 3-aminopropyltrialkoxysilane (R 2 O)3Si-(CH2)3-NH2, 3-(2-aminoethyl)aminopropyltrialkoxysilane (R 2 O)3Si-(CH2)3-NH-(CH2)2-NH2,3-(Trialkoxysilyl)propyldiethylenetriamine (R 2 O)3Si-(CH2)3-NH-(CH2)2-NH-(CH2)2-NH2, 3-chloropropyltrialkoxysilane (R 2 O)3Si-(CH2)3Cl, 3-mercaptopropyltrialkoxysilane (R 2 O)3Si-(CH2)3SH, (3-glycidoxypropyl)trialkoxysilane, (trialkoxysilyl)propyl methacrylate, aminopropyltrialkoxysilane; N-(3-trialkoxysilylpropyl)-4,5-dihydroimidazole organosilylazole and mixtures thereof, R 2 has the same meaning as above. In particular, it is selected from (3-glycidoxypropyl)trimethoxysilane, (trimethoxysilyl)propyl methacrylate, aminopropyltriethoxysilane and mixtures thereof.
[0043] The sol-gel composition according to the present invention may or may not contain oxides or metal particles. In another advantageous embodiment, the content of oxides or metal particles in the sol-gel composition obtained in step a) is 0-50% relative to the total mass of the composition, in particular 3-40% relative to the total mass of the composition, advantageously 5-30% relative to the total mass of the composition, more advantageously 5-15% relative to the total mass of the composition. Therefore, advantageously, the sol-gel composition contains oxides or metal particles.
[0044] The particles may have a size, in particular a diameter, of 2 nm to 80 μm, in particular 2 to 100 nm, advantageously they are nanoparticles, more advantageously having a size, in particular a diameter, of 10 to 60 nm, more preferably 20 to 50 nm. The diameter of these particles may be measured by transmission electron microscopy (TEM), X-ray diffraction and small angle X-ray scattering or light scattering.
[0045] Advantageously, the metal M of the metal alkoxide and / or of the particles is of the same nature as that contained in the deposition of the subsequent coating, in particular in spray deposition, in step c) of the method according to the invention.
[0046] The substrate according to the present invention is a composite material. It can advantageously be an organic matrix composite material (OMC), a ceramic matrix composite material (CMC) or a metal matrix composite material (MMC). In particular, the substrate is an organic matrix composite. In fact, due to the presence of the non-hydrolyzable group R in the organoalkoxysilane of formula II 3 , resulting in the presence of some portion of all-organic material in the sol-gel undercoat, so the adhesion of the sol-gel layer is enhanced on this type of substrate.
[0047] Organic matrix composite substrates are well known to those skilled in the art. They are usually composed of fiber reinforcements densified by an organic matrix, such as thermosetting or thermoplastic resins, in particular selected from epoxy resins, polyimides and polyurethanes (thermosetting resins) or polyetheretherketone (PEEK) resins, polyetherketoneketone (PEKK) resins, polyetherimides, polycarbonates, polyolefins (polyethylene or polypropylene), polyvinyl chloride (PVC) and polystyrene (thermoplastic resins), or bismaleimide or cyanate resins, more particularly epoxy resins. They are mainly organic.
[0048] The manufacture of these substrates is well known and consists first of all in manufacturing a fiber structure which can be in different forms, for example: - a two-dimensional (2D) fabric, - a three-dimensional (3D) fabric obtained by 3D or multilayer weaving, - a braid, - a knit, - a felt, - a unidirectional (UD) web of yarns or cables, or a multidirectional (nD) web obtained by superimposing a plurality of UD webs in different directions and bonding the UD webs together, for example by sewing, by chemical adhesives or by knitting. It is also possible to use a fiber structure formed by several superimposed layers of a fabric, a braid, a knit, a felt, a web or other, the layers being bonded together, for example, by sewing, by the implantation of yarns or stiffening elements or by knitting. The fibers constituting the fiber structure are in particular refractory fibers, i.e. generally carbon fibers, polymer fibers or glass fibers, in particular carbon fibers.
[0049] After optional shaping and consolidation, the fiber structure is then densified. Densification of the fiber structure includes filling the pores of the structure in all or part of its volume with the material constituting the matrix. The composite matrix is obtained in a manner known per se, for example by following a liquid method. The liquid method includes impregnating the fiber structure with a liquid resin containing a precursor of the matrix material. The precursor is usually present in the form of a polymer optionally diluted in a solvent. The fiber structure is placed in a mold, which can be tightly closed with a groove having the shape of the final molded part. Next, the mold is closed and the resin is injected into the entire groove to impregnate the fiber structure. The conversion of the precursor to the matrix, i.e. its polymerization, is carried out by thermal treatment, usually by heating the mold, and after eliminating any solvent and crosslinking the polymer, the preform remains in the mold. The matrix is an organic matrix, such as a thermoplastic or thermosetting resin. The organic matrix can be obtained in particular from an epoxy resin, such as a high-performance epoxy resin sold by the company CYTEC under the reference number PR 520.
[0050] According to one aspect of the invention, the fiber preform can be densified by the known method of resin transfer molding (RTM). According to the RTM method, the fiber preform is placed in a mold having the outer shape of the part to be manufactured. A thermosetting resin is injected into the inner space of the mold including the fiber preform. A pressure gradient is usually established in this inner space between the location where the resin is injected and its discharge hole to control and optimize the impregnation of the preform with the resin.
[0051] The fiber preform can also be densified in a known manner by chemical vapor infiltration (CVI). The fiber preform corresponding to the fiber reinforcement of the substrate to be produced is placed in an oven that allows the entry of a reactive gas phase. The pressure and temperature in the oven and the composition of the gas phase are selected to allow the gas phase to diffuse within the pores of the preform and thus form a matrix by deposition in the core of the material in contact with the fibers, unlike the pressure and temperature conditions characteristic of chemical vapor deposition (CVD) methods, which only form deposits on the surface of the material, while the decomposition of the gas phase components or the reaction between several components produces a solid material.
[0052] Ceramic matrix composite substrates are well known to those skilled in the art. They usually consist of a fiber reinforcement, usually based on carbon fibers or silicon carbide fibers, sometimes aluminum oxide or aluminum oxide fibers (Al2O3), or a mixed crystal of aluminum oxide and silicon oxide (SiO2) called mullite (3Al2O3, 2SiO2), densified by a ceramic matrix, for example a matrix based on aluminum oxide, mullite, carbon or silicon carbide.
[0053] Fibrous structures can be produced and densified as noted above for organic matrix composites.
[0054] Metal matrix composite substrates are also well known to those skilled in the art. They are usually composed of a fiber reinforcement, usually based on ceramic fibers (e.g. silicon carbide) or metal fibers (e.g. stainless steel wires), densified by a light metal matrix (e.g. based on aluminum, magnesium, zinc or titanium).
[0055] Fibrous structures can be produced and densified as noted above for organic matrix composites.
[0056] In an advantageous embodiment of the invention, the composite substrate is a component for aviation, in particular an engine or nacelle component, more particularly a reactor or turbine engine component, advantageously a fan blade, a fan casing or an outlet guide vane (OGV).
[0057] The sol-gel basecoat of step b) is deposited by methods well known to those skilled in the art, such as dipping, spraying, spin coating, spatula, film drawing or brushing, in particular by dipping or spraying.
[0058] In an advantageous embodiment of the invention, the thickness of the sol-gel primer obtained in step b) is at least 5 μm, in particular between 5 μm and 200 μm (inclusive), more particularly between 10 μm and 200 μm. This thickness depends on the nature of the deposit of the subsequent coating of step c) to meet the functional requirements (protection against erosion, frost, ice, lightning, fire, etc.).
[0059] The step c) of depositing the subsequent coating according to the method of the invention can be implemented by methods well known to those skilled in the art. It can therefore be a step of dipping or spraying. Advantageously, it is a thermal spraying step, such as cold spraying or suspension plasma spraying (SPS) or air plasma spraying (APS) or flame spraying (e.g. high velocity oxygen fuel (HVOF)). It can also be a compression heat treatment. It can advantageously be cold spraying, particularly at low pressure. These methods are well known to those skilled in the art.
[0060] Advantageously, the subsequent coating of step c) is a metal layer (pure metal or metal alloy), a ceramic, a cermet or a reinforced or unreinforced polymer or a mixture, advantageously it is a metal layer (pure metal or metal alloy), in particular titanium, aluminum or copper or a mixture of metals, for example a mixture of tin and copper. The particles deposited, in particular sprayed, during step c) of the method according to the invention are therefore advantageously metal particles (pure metal or metal alloy), ceramic particles, cermet particles, reinforced or unreinforced polymer particles or mixture particles, in particular metals, for example titanium, aluminum or copper or a mixture of metals, for example a mixture of tin and copper. The subsequent cermet layer according to the invention can be a highly filled cermet layer (preferably above 12 wt %) and metal elements, for example Co, Ni, Cu, Al or alloys of these elements, for example WC12Co, WC17Co. The subsequent metal coating according to the invention can be Ni, Al or Ti, or a Ni, Co, Al or Ti based alloy. For example, it can be:
[0061] - Ni-based alloys of the NiAl, NiCrAl or NiCrAlY type, in particular Ni-based alloys containing 5 to 20% by weight of Al, for example Ni5Al, NiCr-6Al;
[0062] - an aluminum alloy containing up to 12% by weight of Si;
[0063] - metal alloys based on nickel or cobalt (called “resistance”), highly filled with additional metal elements, for example CoMoCrSi, CoNiCrAIY;
[0064] - Weakly alloyed titanium alloys, such as TA6V, Ti6242 or Tiβ21s.
[0065] Such metals or alloys have good mechanical properties, especially interesting ductility and therefore good shock absorption, which makes them useful as, for example, protective reinforcements for substrates, especially OMCs, more particularly when the substrate is the leading edge of a blade, such as a fan or stator blade. Aluminum, copper and zinc as well as Sn-Zn and Sn-Cu alloys and aluminum alloys can be used to form a lightning protection layer. TiO2 and SiO2 can be used to form an anti-icing layer (anti-icing). Ti and TiN can be used to form an erosion protection layer.
[0066] The thickness of the subsequent coating depends on its nature and function (protection against corrosion, ice, lightning, fire, etc.). It can vary, for example, between 50 μm and 200 μm, or even up to several millimeters, for example between 0.5 mm and 20 mm.
[0067] In an advantageous embodiment, the method according to the invention comprises a prior step α) of preparing the surface of the composite substrate, advantageously by degreasing and then sandblasting or sanding, before step b) of depositing the sol-gel primer. This step improves the adhesion of the primer of step b) on the substrate. Step b) is thus carried out on the composite substrate thus prepared, i.e. obtained at the end of this step.
[0068] In another advantageous embodiment, the method according to the invention comprises an intermediate step b1) of heat treatment. This intermediate step b1) is located between steps b) and c) and is a step of heat treatment of the coated composite substrate obtained in step b) at a maximum temperature of 200° C., in particular at a temperature of 110° C., advantageously for 2 hours, in particular for 1 hour, whereby step c is carried out on the substrate obtained in step b1). This heat treatment step is therefore optional and, if desired, makes it possible to accelerate the polymerization of the sol-gel undercoat.
[0069] In another advantageous embodiment, the method according to the invention comprises an additional finishing step e) after step c) or after optional step d). This is a mechanical or chemical surface finishing step which leads to the final surface state required to ensure the desired functionality. It can be carried out in particular by methods well known to those skilled in the art, such as sandblasting, shot peening, laser texturing, pressing, stamping, abrasion (paper or grindstone), machining, chemical etching or water jetting.
[0070] In a variant of one embodiment, the method according to the invention comprises an intermediate step b2). This intermediate step b2) between steps b) and c) or between optional steps b1) and c) is a step of increasing the surface roughness of the coated composite substrate obtained in step b) or step b1), so that step c) is implemented on the substrate obtained in step b2). This step b2) can be implemented in particular by methods well known to those skilled in the art, such as sandblasting, laser texturing, pressing, stamping, grinding (paper or grindstone), machining, chemical etching or water jetting. It improves the adhesion of the subsequent coating of step c) on the sol-gel primer according to the invention. Therefore, this variant of the method according to the invention comprises steps a), α), b), b1), b2), c), d) and e) as described above, steps α), b1), d) and e) being optional.
[0071] In another embodiment variant, fusible particles, i.e. particles whose particle imprint can be removed by heating or chemical treatment, for example polystyrene particles, are added to the sol-gel composition of step a), and the method according to the invention comprises an intermediate step b3). This intermediate step b3) is located between steps b) and c) and is a heat treatment step (for example, polystyrene particles at 170° C., in particular for 30 minutes) or chemical etching, in order to remove the porosity of the substrate obtained in step b), step c) is therefore carried out on the substrate obtained in step b3). Thus, this variant of the method according to the invention comprises steps a), α), b), b3), c), d) and e) as described above, steps α), d) and e) being optional.
[0072] In another embodiment variant, the sol-gel composition obtained in step a) has a controlled gel state, i.e. the final polymerized state of the organic-inorganic network, making it possible for the layer to be deformable, allowing the deposited, in particular sprayed particles to be embedded (so that the polymerization is not completed), and the deposited, in particular sprayed particles to penetrate into the sol-gel base layer in step c), thereby forming a concentration gradient of particles embedded in the base layer. In fact, in this variant, the sol-gel base layer will have a good ability to deform under the impact of the deposited, in particular sprayed particles during step c). For this reason, the chemical composition of the sol-gel composition of step a) and its drying parameters are specifically selected to allow the deposited, in particular sprayed particles to penetrate. In particular, the chemical precursors (metal alkoxide of formula (I) and organoalkoxysilane of formula (II) of the sol-gel composition), their proportions and their hydrolyzable functions, as well as the particle size of the composition, can be specifically selected. This state of the base layer will allow:
[0073] - embedding deposited, in particular sprayed, particles and obtaining a thermal expansion coefficient gradient;
[0074] - Increase the roughness of the surface state of the base coating, thereby improving the adhesion of the deposited layer, especially the sprayed layer, more especially the thermal sprayed layer;
[0075] - protecting the composition substrate from deposited, especially sprayed, particles;
[0076] The polymerization rate of the sol-gel basecoat is controlled by the contribution of the calories input by the particles deposited, in particular sprayed, during the spraying step.
[0077] This particle embedding gradient also allows for control of the difference in coefficient of thermal expansion between the substrate and the final coating when the part is in use.
[0078] In another embodiment variant, the method according to the invention comprises an intermediate step b4). This intermediate step, located between steps b) and c) or between optional steps b1) and c), is a step of coating the composite substrate obtained in step b) or in optional step b1) by mixing in an aqueous medium an additional primer layer of the sol-gel composition obtained:
[0079] 1-at least one metal alkoxide M(OR 1 ) x ,in
[0080] R 1 represents a C1-C4 alkyl group,
[0081] M represents a metal selected from the group consisting of transition metals, lanthanides, phosphorus, magnesium, tin, zinc, aluminum and antimony,
[0082] x is an integer representing the valence of the metal,
[0083] In particular, as defined above,
[0084] 2- In at least one formula (II) R 3 m Si(OR 2 ) 4-m In the presence of an organoalkoxysilane,
[0085] R 2 represents a C1-C4 alkyl group,
[0086] m represents an integer selected between 1, 2 and 3,
[0087] And each R 3 Each independently represents a non-hydrolyzable group selected from polydimethylsiloxane, C1-C 18 Alkyl, C2-C4 alkenyl, C2-C4 alkynyl, C6-C 10 Aryl, methacryl, methacryl (C1-C 10 Alkyl) or methacryloyloxy (C1-C 10 alkyl), epoxyalkyl or epoxyalkyloxyalkyl, wherein the alkyl is a linear, branched or cyclic C1-C 10 Alkyl, and alkoxy is C1-C 10 Alkoxy, C2-C 10 Halogenated alkyl, C2-C 10 Perhaloalkyl, C2-C 10 Mercaptoalkyl, C2-C 10 Aminoalkyl (C2-C 10 aminoalkyl)amino(C2-C 10 Alkyl), di(C2-C 10Alkylene)triamino(C2-C 10 alkyl), imidazolyl-(C2-C 10 Alkyl) and C2-C 10 Iminoalkyl, in particular as defined above,
[0088] The organoalkoxysilane may advantageously be premixed with acidified water while stirring for the time required to hydrolyze and condense the organic-inorganic hybrid network.
[0089] 3- and in the presence of optionally oxide or metal particles, in particular as defined above,
[0090] 4- by mixing the composition to condense the organic-inorganic hybrid network, the method being advantageously as described above;
[0091] And the sol-gel composition has a controlled gelation state, so that step c) is implemented on the substrate obtained in step b4), so that the particles deposited during step c), in particular sprayed, penetrate into the additional sol-gel primer layer, thereby generating a concentration gradient of particles embedded in the additional primer layer. In this variant, the optional step b1) can be implemented after step b) and / or after step b4). Therefore, this variant of the method according to the invention comprises steps a), α), b), b1), b4), b1) c), d) and e) as described above, steps α), b), b1), d) and e) being optional. Therefore, the first primer layer (step b) mainly ensures chemical adhesion to the substrate and protects the substrate from corrosion, while the second primer layer (step b4) can obtain a thermal expansion coefficient gradient and the roughness required for adhesion of the subsequent coating deposited, in particular by spraying (step c). The composition of the sol-gel mixture of the first and second primer layers can be the same or different; advantageously, they are different.
[0092] The present invention also relates to a coated composite substrate, in particular a coated organic matrix composite material, obtainable by the process according to the invention, in particular as described above. It thus comprises a coating consisting of at least one sol-gel primer coating, in particular as described above, and a subsequent coating, in particular by spraying, in particular by thermal spraying, in particular as described above.
[0093] In an advantageous embodiment of the invention, the coated composite substrate is a component for aviation, in particular an engine or nacelle component, more particularly a reactor or turbine engine component, advantageously a fan blade, a fan casing or an outlet guide vane (OGV).
[0094] Advantageously, the thickness of the sol-gel primer layer is advantageously at least 5 μm, more advantageously between 5 μm and 200 μm, more particularly between 10 μm and 200 μm. This thickness depends on the nature of the subsequent coating deposited, in particular the thermal spray coating, which meets the functional requirements (protection against erosion, ice, lightning, fire, etc.).
[0095] Advantageously, the subsequent coating of the substrate is a metal layer (pure metal or metal alloy), a ceramic, a cermet or a reinforced or unreinforced polymer or a mixture thereof, advantageously it is a metal layer (pure metal or metal alloy), in particular titanium, aluminum or copper or a mixture of metals, such as a mixture of tin and copper. The subsequent cermet layer according to the invention can be a highly filled cermet layer (preferably above 12 wt. %) and a metallic element, such as Co, Ni, Cu, Al or an alloy of these elements, such as WC12Co, WC17Co. The subsequent metal coating according to the invention can be Ni, Al or Ti, or a Ni, Co, Al or Ti based alloy. For example, it can be:
[0096] - Ni-based alloys of the NiAl, NiCrAl or NiCrAlY type, in particular Ni-based alloys containing 5 to 20% by weight of Al, for example Ni5Al, NiCr-6Al;
[0097] - an aluminium alloy containing up to 12% by weight of Si;
[0098] - metal alloys based on nickel or cobalt (called “resistance”), highly filled with additional metal elements, for example CoMoCrSi, CoNiCrAIY;
[0099] - Weakly alloyed titanium alloys, such as TA6V, Ti6242 or Tiβ21s.
[0100] Such metals or alloys have good mechanical properties, especially interesting ductility and therefore good shock absorption, which makes them useful as protective reinforcements for substrates, in particular when the substrate is the leading edge of a blade, such as a fan or stator blade. Aluminum, copper and zinc as well as Sn-Zn and Sn-Cu alloys and aluminum alloys can be used to form lightning protection layers. TiO2 and SiO2 can be used to form anti-icing layers. Ti and TiN can be used to form erosion protection layers.
[0101] The thickness of the subsequent coating depends on its nature and function (protection against corrosion, ice, lightning, fire, etc.). It can vary, for example, between 50 μm and 200 μm, or even up to several millimeters, for example between 0.5 mm and 20 mm.
[0102] The invention also relates to the use of the sol-gel composition obtained by mixing in an aqueous medium:
[0103] 1-at least one metal alkoxide M(OR 1 ) x ,in
[0104] R 1 represents a C1-C4 alkyl group,
[0105] M represents a metal selected from the group consisting of transition metals, lanthanides, phosphorus, magnesium, tin, zinc, aluminum and antimony,
[0106] x is an integer representing the valence of the metal,
[0107] In particular, as defined above,
[0108] 2- In at least one formula (II) R 3 m Si(OR 2 ) 4-m In the presence of an organoalkoxysilane,
[0109] R 2 represents a C1-C4 alkyl group,
[0110] m represents an integer selected between 1, 2 and 3,
[0111] And each R 3 Each independently represents a non-hydrolyzable group selected from polydimethylsiloxane, C1-C 18 Alkyl, C2-C4 alkenyl, C2-C4 alkynyl, C6-C 10 Aryl, methacryl, methacryl (C1-C 10 Alkyl) or methacryloyloxy (C1-C 10 alkyl), epoxyalkyl or epoxyalkyloxyalkyl, wherein the alkyl is a linear, branched or cyclic C1-C 10 Alkyl, and alkoxy is C1-C 10 Alkoxy, C2-C 10 Halogenated alkyl, C2-C 10 Perhaloalkyl, C2-C 10 Mercaptoalkyl, C2-C 10 Aminoalkyl (C2-C 10 aminoalkyl)amino(C2-C 10 Alkyl), di(C2-C 10 Alkylene)triamino(C2-C 10 alkyl), imidazolyl-(C2-C 10 Alkyl) and C2-C 10 Iminoalkyl,
[0112] In particular, as defined above
[0113] The organoalkoxysilane may advantageously be premixed with acidified water while stirring for the time required to hydrolyze and condense the organic-inorganic hybrid network.
[0114] 3- and optionally in the presence of oxide or metal particles, in particular as defined above,
[0115] 4- by mixing the composition to condense the organic-inorganic hybrid network, the method being advantageously as described above;
[0116] As a primer coating for a composite substrate, in particular an organic matrix composite material, to protect the substrate and / or improve adhesion on the substrate during deposition of a subsequent coating, in particular by spraying, more in particular by thermal spraying. In particular, the sol-gel composition, the composite substrate and / or the subsequent coating are as described above.
[0117] Thus, its use may be to improve the adhesion of a subsequent coating on the substrate during deposition and / or the adhesion between the substrate and the subsequent coating during use.
[0118] The invention will be better understood on reading the following figures and the description of the examples given by way of non-limiting indication. BRIEF DESCRIPTION OF THE DRAWINGS
[0119] Figure 1 is a representative view of a vertical cross section of a composite substrate (1) coated with a sol-gel primer layer (2) and a subsequent coating layer (3) obtained by the method of the present invention.
[0120] Figure 2 is a representative view of a vertical cross section of a composite substrate (1) coated with a sol-gel basecoat having a controlled gel state, comprising a particle gradient (4), and with a subsequent coating (3) obtained by a variant of the process according to the invention.
[0121] Example 1: Si-Zr sol-gel primer and ZrO2 particles before thermal spray deposition
[0122] The following compounds were added to the beaker in sequence under magnetic stirring: 70% by mass zirconium (IV) propoxide solution and glacial acetic acid to make the Zr / H + = 2. After homogenization, add distilled water while stirring to make Zr / H2O = 15.
[0123] The solution was kept stirring for about 1 hour until a homogeneous clear solution was obtained.
[0124] To this solution, (3-glycidoxypropyl)trimethoxysilane was added under stirring so that Si / Zr = 0.3. The stirring was maintained for about 1 hour until a homogeneous transparent solution was obtained.
[0125] 5% by mass of ZrO2 particles (average diameter 50 nm) are added to the mixture under stirring and / or ultrasound.
[0126] Then, an organic matrix composite (OMC) substrate is prepared, wherein the OMC is made of a carbon fiber reinforced epoxy-based composite material, according to methods known to those skilled in the art, such as sanding or sandblasting, and then sequentially cleaned to remove dust on the surface.
[0127] The formulation of the primer layer is then deposited on the OMC substrate by spraying or dipping to completely cover the surface, and the substrate so coated is then placed in an oven at 110° for a period ranging from a few minutes to an hour.
[0128] The resulting substrate is then coated with a metallic aluminum layer obtained by low-pressure cold spraying.
[0129] Example 2: Si-Ti sol-gel undercoat and TiO2 particles before thermal spray deposition
[0130] The following compounds were added to the beaker in sequence under magnetic stirring: titanium (IV) butoxide and glacial acetic acid to make Ti / H + =2, and then distilled water was added under stirring to make Ti / H2O=8.
[0131] The solution was stirred for about 30 minutes, and then 3-(trimethoxysilyl)propyl methacrylate (γ-MPS) and aminopropyltriethoxysilane (APTES) were added under stirring to make Si / Ti = 0.2, γ-MPS / APTES = 3. Stirring was continued for about 1 hour.
[0132] 5% by mass of TiO2 particles (average diameter 20 nm) are added to the mixture under stirring and / or ultrasound.
[0133] Then, an organic matrix composite (OMC) substrate is prepared, wherein the OMC is made of a carbon fiber reinforced epoxy-based composite material, according to methods known to those skilled in the art, such as sanding or sandblasting, and then sequentially cleaned to remove dust on the surface.
[0134] The formulation of the primer layer is then deposited on the OMC substrate by spraying or dipping to completely cover the surface, and the substrate so coated is then placed in an oven at 110° for a period ranging from a few minutes to an hour.
[0135] The resulting substrate is then coated with a metallic titanium layer obtained by low-pressure cold spraying.
[0136] Example 3: Si-Al Primer Before Aluminum Spraying
[0137] The aluminum (III) isopropoxide precursor was mixed with distilled water (so that the H2O / Al molar ratio = 10). The mixture was stirred at 80°C for 1 hour.
[0138] The pH value was adjusted to 3 by adding concentrated nitric acid (68%) to form an oxide network. After vigorous stirring at 80°C for 1 hour, a clear, blue and stable sol was obtained. The solution was returned to ambient temperature and (3-glycidoxypropyl)trimethoxysilane was added thereto so that Si / Al=0.3. The solution was kept stirring for 2 hours.
[0139] Then, an organic matrix composite (OMC) substrate is prepared, wherein the OMC is made of a carbon fiber reinforced epoxy-based composite material, according to methods known to those skilled in the art, such as sanding or sandblasting, and then sequentially cleaned to remove dust on the surface.
[0140] The formulation of the primer layer is then deposited on the OMC substrate by spraying or dipping to completely cover the surface, and the substrate so coated is then placed in an oven at 110° for a period ranging from a few minutes to an hour.
[0141] The resulting substrate is then coated with a metallic aluminum layer obtained by low-pressure cold spraying.
[0142] Example 4: Si-Ti sol-gel primer and fusible polystyrene particles before thermal spray deposition
[0143] The following compounds were added to the beaker in sequence under magnetic stirring: titanium (IV) butoxide and glacial acetic acid to make Ti / H + =2, and then distilled water was added under stirring to make Ti / H2O=8.
[0144] The solution was stirred for about 30 minutes, and then (3-glycidoxypropyl)trimethoxysilane (GPTMS) and aminopropyltriethoxysilane (APTES) were added under stirring to make Si / Ti = 0.2, GPTMS / APTES = 5. Stirring was continued for about 2 hours.
[0145] 5% by mass of polystyrene particles (average diameter 5 nm) were added to the mixture under stirring and / or ultrasound.
[0146] Then, an organic matrix composite (OMC) substrate is prepared, wherein the OMC is made of a carbon fiber reinforced epoxy-based composite material, according to methods known to those skilled in the art, such as sanding or sandblasting, and then sequentially cleaned to remove dust on the surface.
[0147] The formulation of the primer layer is then deposited on the OMC substrate by spraying or dipping to completely cover the surface, and then within a few minutes to an hour, the substrate so coated is placed in an oven at 110°C for 1 hour and then at 170°C for 30 minutes to remove the pores of the polystyrene particles on the surface.
[0148] The resulting substrate is then coated with a metallic titanium layer obtained by low-pressure cold spraying.
[0149] Example 5: Dual Si-Ti sol-gel undercoat and TiO2 particles followed by Si-Al undercoat prior to aluminum layer deposition by thermal spraying
[0150] First base coat:
[0151] The following compounds were added to the beaker in sequence under magnetic stirring: titanium (IV) butoxide and glacial acetic acid to make Ti / H + =2, and then distilled water was added under stirring to make Ti / H2O=8.
[0152] The solution was stirred for about 30 minutes, and then 3-(trimethoxysilyl)propyl methacrylate (γ-MPS) and aminopropyltriethoxysilane (APTES) were added under stirring to make Si / Ti = 0.2, γ-MPS / APTES = 3. Stirring was continued for about 1 hour.
[0153] 5% by mass of TiO2 particles (average diameter 20 nm) are added to the mixture under stirring and / or ultrasound.
[0154] Then, an organic matrix composite (OMC) substrate is prepared, wherein the OMC is made of a carbon fiber reinforced epoxy-based composite material, according to methods known to those skilled in the art, such as sanding or sandblasting, and then sequentially cleaned to remove dust on the surface.
[0155] The formulation of the primer layer is then deposited on the OMC substrate by spraying or dipping to completely cover the surface, and the substrate so coated is then placed in an oven at 80° for 45 minutes over a period ranging from a few minutes to an hour.
[0156] Second base coat:
[0157] Separately, an aluminum (III) isopropoxide mixture was prepared with distilled water (so that the H2O / Al molar ratio = 10). The mixture was stirred at 80°C for 1 hour.
[0158] The pH value was adjusted to 3 by adding concentrated nitric acid (68%) to form an oxide network. After vigorous stirring at 80°C for 1 hour, a clear, blue and stable sol was obtained. The solution was returned to ambient temperature and (3-glycidoxypropyl)trimethoxysilane was added thereto so that Si / Al=0.3. The solution was kept stirring for 2 hours.
[0159] The formulation of this primer layer was then deposited by spraying on the OMC substrate covered with the previous primer layer so as to completely cover the surface, and the substrate thus coated was then placed in an oven at 110°C for 1 hour.
[0160] The resulting substrate is then coated with a metallic aluminum layer obtained by low-pressure cold spraying.
Claims
1. A coating method for an organic matrix composite substrate, characterized in that it comprises the following steps: a- Preparation of sol-gel compositions by mixing in an aqueous medium: 1-at least one metal alkoxide M(OR 1 ) x ,in R 1 represents a C1-C4 alkyl group, M represents a metal selected from the group consisting of transition metals, lanthanides, phosphorus, magnesium, tin, zinc, aluminum and antimony, x is an integer representing the valence of the metal, 2- In at least one formula (II) R 3 m Si(OR 2 ) 4-m In the presence of an organoalkoxysilane, R 2 represents a C1-C4 alkyl group, m represents an integer selected between 1, 2 and 3, And each R 3 Each independently represents a non-hydrolyzable group selected from polydimethylsiloxane, C1-C 18 Alkyl, C2-C4 alkenyl, C2-C4 alkynyl, C6-C 10 Aryl, methacryl, methacryl (C1-C 10 Alkyl) or methacryloyloxy (C1-C 10 alkyl), epoxyalkyl or epoxyalkyloxyalkyl, wherein the alkyl is a linear, branched or cyclic C1-C 10 Alkyl, and alkoxy is C1-C 10 Alkoxy, C2-C 10 Halogenated alkyl, C2-C 10 Perhaloalkyl, C2-C 10 Mercaptoalkyl, C2-C 10 Aminoalkyl (C2-C 10 aminoalkyl)amino(C2-C 10 Alkyl), di(C2-C 10 Alkylene)triamino(C2-C 10 alkyl), imidazolyl-(C2-C 10 Alkyl) and C2-C 10 Iminoalkyl, 3- and optionally in the presence of oxide or metal particles, 4- by mixing the composition to condense the organic-inorganic hybrid network, b- depositing at least one primer layer on an organic matrix composite substrate from the sol-gel composition obtained in step a); c- and depositing at least one subsequent coating on the organic matrix composite substrate coated with the primer layer obtained in step b); wherein the subsequent coating of step c) is a metal layer comprising a pure metal or a metal alloy; Therein, the sol-gel composition obtained in step a) has a controlled gel state, and the particles deposited in step c) penetrate into the sol-gel base coating, thereby generating a concentration gradient of particles embedded in the base coating.
2. The method according to claim 1, characterized in that The metal M is selected from the group consisting of Cu, Mn, Sn, Fe, Mg, Zn, Al, P, Sb, Zr, Ti, Hf, Ce, Nb, V and Ta.
3. The method according to claim 2, characterized in that The metal M is selected from the group consisting of Zr, Ti and Al.
4. The method according to any one of claims 1 to 3, characterized in that: The Si / M molar ratio in the sol-gel composition obtained in step a) is between 0.1 and 0.
5.
5. The method according to claim 4, characterized in that 0.3≤Si / M≤0.
5.
6. The method according to any one of claims 1 to 3, characterized in that The content of oxide or metal particles in the sol-gel composition obtained in step a) is 0-50% by mass relative to the total mass of the composition.
7. The method according to claim 6, characterized in that The content of oxide or metal particles in the sol-gel composition obtained in step a) is 5-15% by mass relative to the total mass of the composition.
8. The method according to any one of claims 1 to 3, characterized in that The thickness of the sublayer obtained in step b) is between 5 μm and 200 μm.
9. The method according to any one of claims 1 to 3, characterized in that Step c) is a thermal spraying step.
10. The method according to claim 9, characterized in that Step c) is cold spraying.
11. The method according to any one of claims 1 to 3, characterized in that It comprises a preceding step α) of preparing the surface of the composite substrate before step b) of depositing the sol-gel primer layer.
12. The method according to any one of claims 1 to 3, characterized in that It comprises a preceding step α) of preparing the surface of the composite substrate prior to step b) of depositing the sol-gel primer layer, by degreasing and then sandblasting or sanding.
13. The method according to any one of claims 1 to 3, characterized in that It comprises an intermediate step b1) between steps b) and c), namely heat-treating the coated composite substrate obtained in step b) at a maximum temperature of 200° C., whereby step c) is performed on the substrate obtained in step b1).
14. The method according to any one of claims 1 to 3, characterized in that It comprises an intermediate step b1) between steps b) and c), namely heat treating the coated composite substrate obtained in step b) at a maximum temperature of 200° C. for 2 hours, whereby step c) is performed on the substrate obtained in step b1).
15. The method according to any one of claims 1 to 3, characterized in that It comprises an intermediate step b2) between steps b) and c) or optionally between steps b1) and c), increasing the surface roughness of the coated composite substrate obtained in step b) or step b1), and step c) is performed on the substrate obtained in step b2).
16. The method according to any one of claims 1 to 3, characterized in that Fusible particles are added to the sol-gel composition of step a), and an intermediate step b3) of heat treatment or chemical etching is included between steps b) and c) to remove the porosity of the substrate obtained in step b), step c) being carried out on the substrate obtained in step b3).
17. The method according to any one of claims 1 to 3, characterized in that It comprises an intermediate step b4) between steps b) and c) or between optional steps b1) and c), coating the composite substrate obtained in step b) or in optional step b1) with an additional primer layer of a sol-gel composition obtained by mixing in an aqueous medium: 1-at least one metal alkoxide M(OR 1 ) x , 2- At least one R of formula (II) as defined in claim 1 3 m Si(OR 2 ) 4-m In the presence of organoalkoxysilane, 3- and optionally in the presence of oxide or metal particles, 4- by mixing the composition to condense the organic-inorganic hybrid network, The sol-gel composition has a controlled gel state and is characterized in that step c) is carried out on the substrate obtained in step b4) so that the particles deposited during step c) penetrate into the additional sol-gel base layer, thereby generating a concentration gradient of particles embedded in the additional base layer.
18. The method according to any one of claims 1 to 3, characterized in that The composite substrate is an engine or cabin component.
19. The method according to claim 12, characterized in that The composite substrate is a fan blade, a fan casing or an outlet guide vane.
20. A coated organic matrix composite substrate obtained by the method according to any one of claims 1 to 19, characterized in that The thickness of the sol-gel base coating of the substrate is between 5 μm and 200 μm, and the subsequent coating of the substrate is a metal layer comprising a pure metal or a metal alloy.
21. Use of the sol-gel composition obtained by mixing in an aqueous medium: 1-at least one metal alkoxide M(OR 1 ) x , 2- At least one R of formula (II) as defined in claim 1 3 m Si(OR 2 ) 4-m In the presence of organoalkoxysilane, 3- and optionally in the presence of oxide or metal particles, 4- by mixing the composition to condense the organic-inorganic hybrid network, As a primer layer for an organic matrix composite substrate to protect the substrate and / or improve adhesion on the substrate during deposition of subsequent coatings, wherein The subsequent coating of the substrate is a metal layer comprising a pure metal or a metal alloy.
Citation Information
Patent Citations
Organic-inorganic hybrids surface adhesion promotor
CA2339053A1
Heat and rain erosion resistant coating
CN101331198A
Substrate element for coating with an easy-to-clean coating
CN104080754A
Method for the autophoretic coating of metallic substrates by post-treating the coating with an aqueous sol-gel composition
CN105579614A
Substrate comprising abrasion-resistant diffusion barrier layer system
CN1382073A