Diamond coated tool and method for manufacturing the same

By evenly aligning the diamond layer on the edge of the diamond-covered tool and controlling the temperature distribution using the hot wire CVD method, the problem of deviation in the thickness and crystallinity of the diamond layer is solved, extending the tool life and improving wear resistance.

CN114599478BActive Publication Date: 2024-12-06SUMITOMO ELECTRIC HARDMETAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080074405.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-08
Filing Date
2020-10-09
Publication Date
2024-12-06
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

In diamond-covering tools, there are deviations in the thickness and crystallinity of the diamond layer on the substrate, resulting in uneven wear and peeling, shortening the tool life.

Method used

By uniformly aligning 11 places along the extension direction of the diamond coating tool, the thickness of the diamond layer is determined to ensure that the minimum to maximum value ratio of the thickness is above 0.7 and less than 1, the base material cutting edge is controlled by the hot wire CVD method. The temperature of the portion is distributed within 5%, forming a uniform diamond layer.

Benefits of technology

The uniform thickness and crystallinity of the diamond layer are achieved, which extends the tool life and improves the wear and peel resistance of the diamond-covered tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114599478B_ABST
    Figure CN114599478B_ABST
Patent Text Reader

Abstract

A diamond coated tool, comprising a blade consisting of a substrate and a diamond layer disposed on the substrate, wherein the length of the blade along the extension direction thereof is L, and in the blade, at 11 locations in total arranged at a distance of L / 10 from one end along the direction along the extension direction, when the thickness of the diamond layer is measured, the thickness at all locations is the same, or the minimum value d of the thickness is less than 1 / 10. min With the maximum value of the thickness d max The ratio of d min / d max It is greater than or equal to 0.7 and less than 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a diamond coated tool and a method for manufacturing a diamond coated tool. This application claims priority based on Japanese patent application No. 2019-203330 filed on November 8, 2019. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art

[0002] Diamond has a very high hardness and its smooth surface has an extremely low friction coefficient. Therefore, natural single crystal diamond and artificial diamond powder have been used for tool applications in the past. Furthermore, after the formation technology of diamond thin film based on chemical vapor deposition (CVD) method was established in the 1980s, cutting tools and wear-resistant tools with diamond film formed on three-dimensional substrates were developed.

[0003] Japanese Patent Application Laid-Open No. 11-347805 (Patent Document 1) discloses a diamond-coated tool member in which a surface of a cemented carbide substrate is coated with a diamond hard film.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 11-347805 Summary of the invention

[0007] The diamond coated tool disclosed herein is a diamond coated tool having a blade portion composed of a substrate and a diamond layer provided on the substrate, wherein:

[0008] The length of the blade along its extension direction is L,

[0009] In the blade, at 11 points in total arranged at a distance of L / 10 from one end along the direction along the extension direction, when the thickness of the diamond layer is measured, the thickness at all the points is the same, or the minimum value d of the thickness is min With the maximum value of the thickness d max The ratio of d min / d max It is greater than or equal to 0.7 and less than 1.

[0010] The manufacturing method of the diamond coated tool disclosed in the present invention is the manufacturing method of the diamond coated tool mentioned above, and the manufacturing method comprises:

[0011] The process of preparing the substrate; and

[0012] A step of forming a diamond layer on the substrate by hot wire CVD to obtain a diamond coated tool,

[0013] The hot-filament CVD method is performed by controlling the temperature distribution in the edge portion of the substrate where the cutting edge exists to be within 5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a diagram for explaining a configuration example of a diamond coated tool according to Embodiment 1-1.

[0015] Figure 2 yes Figure 1 , Figure 3 and Figure 4 Cross-sectional view of a diamond coated tool on line XX.

[0016] Figure 3 This is a diagram for explaining a configuration example of a diamond coated tool (tapered cutter) according to Embodiment 1-2.

[0017] Figure 4 This is a diagram for explaining a configuration example of a diamond coated tool (drill bit) according to Embodiment 1-3.

[0018] Figure 5 yes Figure 4 An enlarged view of the first blade portion 35A.

[0019] Figure 6 yes Figure 4 An enlarged view of the second blade portion 35B.

[0020] Figure 7 This is a diagram showing an example of the Raman spectrum at the first point.

[0021] Figure 8 This is a diagram showing an example of the Raman spectrum at the second point.

[0022] Fig. 9 This is a diagram showing an example of the C1s spectrum at the first point.

[0023] Fig.10 This is a diagram showing an example of the C1s spectrum at the second point.

[0024] Fig.11 This is a front view showing an example of a conventional hot-filament CVD apparatus.

[0025] Fig.12 yes Fig.11 Top view of the hot wire CVD device.

[0026] Fig.13 This is a diagram showing the surface temperature distribution of a substrate when a film is formed by a conventional hot-filament CVD method.

[0027] Fig.14This is a diagram showing an example of a hot filament CVD apparatus used in the second embodiment.

[0028] Fig.15 This is a diagram showing the surface temperature distribution of a substrate when a film is formed by the hot-filament CVD method according to the second embodiment. DETAILED DESCRIPTION

[0029] [Problems to be solved by this disclosure]

[0030] In diamond coated tools, if the thickness and crystallinity of the diamond layer on the substrate vary, the occurrence of wear and peeling of the diamond layer in the same tool will also vary, which tends to shorten the tool life. Therefore, a diamond coated tool with uniform thickness and crystallinity of the diamond layer and a long tool life is required.

[0031] An object of the present disclosure is to provide a diamond coated tool having a longer tool life.

[0032] [Effects of the present disclosure]

[0033] According to the present disclosure, diamond coated tools can have longer tool life.

[0034] [Description of Embodiments of the Present Disclosure]

[0035] First, embodiments of the present disclosure will be described by way of examples.

[0036] (1) The diamond coated tool disclosed in the present invention is a diamond coated tool having a blade portion composed of a substrate and a diamond layer provided on the substrate.

[0037] The length of the blade along its extension direction is L,

[0038] In the blade, at 11 points in total arranged at a distance of L / 10 from one end along the direction along the extension direction, when the thickness of the diamond layer is measured, the thickness at all the points is the same, or the minimum value d of the thickness is min With the maximum value of the thickness d max The ratio of d min / d max It is greater than or equal to 0.7 and less than 1.

[0039] According to the present disclosure, diamond coated tools can have longer tool life.

[0040] (2) Preferably, the d min / d max It is 0.85 or more and less than 1. Thus, the tool life of the diamond coated tool is further improved.

[0041] (3) Preferably, when the thickness is the minimum value d min The first location and the thickness is the maximum value d max At the second location, the Raman shift of the diamond layer was measured from 900 cm -1 Up to 2000cm -1 In the case of Raman spectroscopy,

[0042] I min with I max Ratio I min / I max is greater than or equal to 0.7 and less than or equal to 1, the I min is the peak area intensity Id of diamond at the first location min The area intensity Is of the entire spectrum min Ratio Id min / Is min , the I max is the peak area intensity Id of diamond at the second location max The area intensity Is of the entire spectrum max Ratio Id max / Is max .

[0043] As a result, the tool life of the diamond coated tool is further improved.

[0044] (4) Preferably, when the thickness is the minimum value d min The first location and the thickness is the maximum value d max At the second location, when the C1s spectrum of the diamond layer is measured by X-ray photoelectron spectroscopy,

[0045] Ix min With Ix max Ratio Ix min / Ix max is greater than or equal to 0.7 and less than or equal to 1, the Ix min is the peak area intensity I3 of the sp3 carbon at the first location min The peak area intensity I2 of sp2 carbon min Ratio I3 min / I2 min , the 1x max is the peak area intensity I3 of the sp3 carbon at the second location max The peak area intensity I2 of sp2 carbon max Ratio I3 max / I2 max .

[0046] As a result, the tool life of the diamond coated tool is further improved.

[0047] (5) Preferably, when the thickness is the minimum value d min The first location and the thickness is the maximum value d max At the second location, when the average grain size of the diamond layer is measured by electron backscatter diffraction,

[0048] The average particle size D at the first location min The average particle size D at the second location max The ratio is D min / D max It is greater than or equal to 0.7 and less than or equal to 1.

[0049] As a result, the tool life of the diamond coated tool is further improved.

[0050] (6) Preferably, when the thickness is the minimum value d min The first location and the thickness is the maximum value d max At the second location, when the surface roughness Ra of the diamond layer is measured using a laser microscope,

[0051] The surface roughness R at the first location min The surface roughness R at the second location max R min / R max It is 0.7 or more and 1 or less.

[0052] As a result, the tool life of the diamond coated tool is further improved.

[0053] (7) The method for manufacturing a diamond coated tool disclosed in the present invention is the method for manufacturing a diamond coated tool described above, the method comprising:

[0054] The process of preparing the substrate; and

[0055] A step of forming a diamond layer on the substrate by hot wire CVD to obtain a diamond coated tool,

[0056] The hot-filament CVD method is performed by controlling the temperature distribution in the edge portion of the substrate where the cutting edge exists to be within 5%.

[0057] According to the present disclosure, a diamond coated tool having a uniform thickness of the diamond layer and a long tool life can be obtained.

[0058] [Details of the embodiments of the present disclosure]

[0059] Hereinafter, a specific example of the diamond coated cutting tool disclosed in the present invention will be described with reference to the accompanying drawings. In the accompanying drawings disclosed in the present invention, the same reference numerals represent the same parts or equivalent parts. In addition, in order to make the accompanying drawings clear and simple, the dimensional relationship such as length, width, thickness, depth, etc. can be appropriately changed and does not necessarily represent the actual dimensional relationship.

[0060] In this specification, the expression of the form "A to B" refers to the upper and lower limits of the range (i.e., greater than A and less than B). When there is no unit recorded in A and only a unit is recorded in B, the unit of A is the same as that of B.

[0061] [Implementation 1: Diamond coated tool]

[0062] Figure 1 This is a diagram showing a configuration example in which the diamond coated tool is an end mill. Figure 2 yes Figure 1 Cross-sectional view of a diamond coated tool on line XX.

[0063] like Figure 1 and Figure 2 As shown, the diamond coated tool 10 is a diamond coated tool having a blade 5 composed of a substrate 1 and a diamond layer 2 provided on the substrate 1, the length of the blade 5 along the extension direction thereof is L, and in the blade 5, at 11 points in total arranged at a distance of L / 10 from one end along the direction along the extension direction, when the thickness of the diamond layer is measured, the thickness at all the points is the same, or the minimum value d of the thickness is min The maximum value of thickness d max The ratio of d min / d max It is greater than or equal to 0.7 and less than 1.

[0064] Since the diamond coated tool disclosed in the present invention has a uniform thickness of the diamond layer, there will be no deviation in the occurrence of wear and peeling of the diamond layer, and the tool can have a longer life.

[0065] Below, use Figure 1 to Figure 6 A specific example of the diamond coated tool disclosed in the present invention is described. It should be noted that, Figure 1 The diamond coated tool is shown as an end mill. Figure 3 The diamond coated tool is a conical cutter. Figures 4 to 6 The diamond coated tool is a drill bit, but the type of diamond coated tool is not limited thereto. Examples of the diamond coated tool disclosed herein include cutting tools such as a bite, a cutter, a drill, and an end mill; and wear-resistant tools such as a die, a bending die, a drawing die, and a joining tool.

[0066] [Implementation 1-1: End mill]

[0067] In the embodiment 1-1, the case where the diamond coated tool is an end mill is described. Figure 1 As shown, the end mill as a diamond coated tool 10 includes a main body 3 and a shank 4 connected to the main body 3. In the main body 3, a cutting edge 5 including a bottom edge 6 and a peripheral edge 7 is formed. Figure 2 As shown, a substrate 1 and a diamond layer 2 provided on the substrate 1 are provided.

[0068] exist Figure 1 In the embodiment 1-1, the blade 5 extends along the rotation axis O of the tool. Therefore, in the embodiment 1-1, the length L of the blade 5 along the extending direction thereof refers to the length of the blade 5 along the rotation axis O of the tool.

[0069] <Base material>

[0070] As the substrate, a substrate known in the past can be used without particular limitation. Examples of such substrates include superhard alloys (for example, WC-based superhard alloys, superhard alloys containing Co in addition to WC, or superhard alloys further containing carbonitrides such as Ti, Ta, and Nb), cermets (cermets containing TiC, TiN, and TiCN as main components), high-speed steel, tool steel, ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, and mixtures thereof), and cubic boron nitride sintered bodies.

[0071] Among these substrates, WC-based superhard alloys and cermets (particularly TiCN-based cermets) are particularly preferably selected because these substrates have an excellent balance between hardness and strength, especially at high temperatures, and have excellent properties as substrates for diamond-coated cutting tools.

[0072] <Diamond layer>

[0073] The diamond layer may be a diamond layer produced by a conventionally known chemical vapor deposition method (CVD), and preferably a diamond layer produced by a hot-filament CVD method.

[0074] (thickness)

[0075] In the blade 5, from one end (at Figure 1 11 points in total (in the center, the end portion on the front end T side) are arranged at a distance of L / 10 from each other along the extension direction (axis O) Figure 1In the case of measuring the thickness of the diamond layer, the thickness at all locations is the same, or the minimum value of the thickness is d min The maximum value of thickness d max The ratio of d min / d max It is 0.7 or more and less than 1. Thus, the thickness of the diamond layer of the diamond coated tool is uniform, and a long tool life can be achieved.

[0076] The above d min / d max It is preferably 0.85 or more and less than 1, and more preferably 0.95 or more and less than 1.

[0077] In this specification, the thickness of the diamond layer can be measured by the following procedures (1-1) to (1-2).

[0078] (1-1) The length L of the blade 5 along the rotation axis O is measured. Next, at one end of the blade (e.g., the front end of the tool, Figure 1 The end portion on the front end T side) and each location (a total of 11 locations including both ends, in Figure 1 The diamond coated tool is cut in a direction perpendicular to the rotation axis O using a wire electrical discharge machine to expose the cross section.

[0079] (1-2) The thickness of the diamond layer was measured by observing the cross section at each location using a SEM (scanning electron microscope, JEOL Ltd. "JEM-2100F / Cs" (trademark)). Specifically, the cross-sectional sample was observed at a magnification of 5000 times and the observation field area was 100 μm. 2 , measure the thickness of 3 positions in the observation field, and set the average value of the 3 positions as the thickness of the observation field. Measure in 5 observation fields, and set the average value of the thickness of the 5 observation fields as the thickness of the diamond layer.

[0080] The minimum value d of the thickness of the diamond layer min For example, the lower limit can be set to 3 μm, 4 μm, or 5 μm, and the upper limit can be set to 28 μm, 29 μm, or 30 μm.

[0081] The maximum value d of the thickness of the diamond layer max For example, the lower limit can be set to 3 μm, 4 μm, or 5 μm, and the upper limit can be set to 28 μm, 29 μm, or 30 μm.

[0082] (Raman spectroscopy)

[0083] When the thickness of the diamond layer is the minimum value d min The first location and the thickness of the diamond layer is the maximum value d max At the second location, the Raman shift of the diamond layer was measured from 900 cm -1 Up to 2000cm -1 In the case of Raman spectroscopy, I min with I max Ratio I min / I max Preferably, it is 0.7 or more and 1 or less, and the I min is the peak area intensity Id of diamond at the first location min The area intensity Is of the entire spectrum min Ratio Id min / Is min , the I max is the peak area intensity Id of diamond at the second location max The area intensity Is of the entire spectrum max Ratio Id max / Is max .

[0084] Thus, the tool life of the diamond coated tool is further improved. Although the reason is not clear, it can be considered that the reason is: if I min / I max When the value of is 0.7 or more, the crystallinity of diamond becomes uniform over the entire area of ​​the diamond layer, and the wear resistance and peeling resistance of the diamond layer also become uniform in the blade portion.

[0085] The above I min / I max It is more preferably 0.85 or more and 1 or less, and even more preferably 0.9 or more and 1 or less.

[0086] In this specification, the above I min / I max The calculation can be performed using the following steps (2-1) to (2-6).

[0087] (2-1) Based on the above measurement results of the thickness of the diamond layer, the thickness of the diamond layer is determined to be the minimum value d min The first location and the thickness of the diamond layer is the maximum value d max At the first and second locations, the diamond coated tool was cut by a wire electrical discharge machine in a direction perpendicular to the rotation axis O to expose the cross section. Each cross section was mirror polished using diamond slurry having an average particle size of 3 μm.

[0088] (2-2) In the cross section at each point, a rectangular measurement field of view of 50 μm×50 μm (hereinafter also referred to as “Raman spectroscopy measurement field of view”) was set in the diamond layer.

[0089] (2-3) For each Raman spectroscopy measurement field, the Raman shift from 900 cm to 100 cm was obtained by laser Raman measurement according to JIS-K0137 (2010). -1 Up to 2000cm -1 The Raman spectrometer used was "Ramantouch" (trademark) manufactured by Nanophoton. An example of the Raman spectra at the first location and the second location is shown in Figure 7 and Figure 8 In. Figure 7 and Figure 8 In the figure, the spectrum shown in Id is derived from diamond, and the spectrum shown in Is is derived from Figure 7 and Figure 8 The sum of all spectra shown in each case.

[0090] (2-4) The peak area intensity Id as diamond was calculated using image processing software ("Ramanimager" (trademark) manufactured by Nanophoton Corporation) for the Raman spectrum of the first point. min The area intensity Is of the entire spectrum min Ratio Id min / Is min I min The measurement at the first location is performed in the measurement field of any three locations, and the average value of the three locations is defined as the “I at the first location”. min ”.

[0091] (2-5) The peak area intensity Id as diamond was calculated using image processing software ("Ramanimager" (trademark) manufactured by Nanophoton Corporation) for the Raman spectrum at the second point. max The area intensity Is of the entire spectrum max Ratio Id max / Is max I max The measurement at the second location is performed in the measurement field of any three locations, and the average value of the three locations is defined as the “I at the second location”. max ”.

[0092] (2-6) Based on the above “I at the first location min ” and the above “I at the second location max ”, calculate I min / I max .

[0093] About I at the 1st location min For example, the lower limit can be set to 0.25, 0.35, 0.40, and the upper limit can be set to 0.70, 0.80, 0.90.

[0094] Regarding I at the 2nd location max For example, the lower limit can be set to 0.25, 0.35, 0.40, and the upper limit can be set to 0.70, 0.80, 0.90.

[0095] (C1s spectrum)

[0096] At a minimum thickness d min The first location and thickness are the maximum value d max When the C1s spectrum of the diamond layer is measured by X-ray photoelectron spectroscopy (XPS) at the second location, Ix min With Ix max Ratio Ix min / Ix max Preferably, 0.7 or more and 1 or less, the Ix min is the peak area intensity I3 of sp3 carbon at the first site min The peak area intensity I2 of sp2 carbon min Ratio I3 min / I2 min , the 1x max is the peak area intensity I3 of sp3 carbon at the second location max The peak area intensity I2 of sp2 carbon max Ratio I3 max / I2 max .

[0097] Thus, the tool life of the diamond coated tool is further improved. Although the reason is not clear, it can be considered that the reason is: if 1x min / Ix max When the value of is 0.7 or more, the crystallinity of diamond becomes uniform over the entire area of ​​the diamond layer, and the wear resistance of the diamond layer also becomes uniform in the blade portion.

[0098] The above Ix min / Ix max It is more preferably 0.7 or more and 1 or less, and even more preferably 0.85 or more and 1 or less.

[0099] In this specification, the above-mentioned 1x min / Ix max The calculation can be performed using the following steps (3-1) to (3-6).

[0100] (3-1) Based on the above measurement results of the thickness of the diamond layer, the thickness of the diamond layer is determined to be the minimum value d min The first location and the thickness of the diamond layer is the maximum value d max At the first and second locations, the diamond coated tool was cut by a wire electrical discharge machine in a direction perpendicular to the rotation axis O to expose the cross section. Each cross section was mirror polished using diamond slurry having an average particle size of 3 μm.

[0101] (3-2) In the cross section at each point, a rectangular measurement field of view of 50 μm×50 μm (hereinafter also referred to as “XPS measurement field of view”) was set in the diamond layer.

[0102] (3-3) For each XPS measurement field, a C1s spectrum was obtained by X-ray photoelectron spectroscopy. The X-ray photoelectron spectrometer used was "QuanteraSXM" (trademark) manufactured by ULVAC PHI. An example of the C1s spectrum at the first location and the second location is shown in FIG. Fig. 9 and Fig.10 middle.

[0103] (3-4) The peak area intensity I3 of the sp3 carbon was calculated using image processing software ("PHIMultiPak" (trademark) manufactured by ULVAC PHI) for the C1s spectrum of the first point. min The peak area intensity I2 of sp2 carbon min Ratio I3 min / I2 min Ix min The measurement at the first location is performed in the measurement field of any three locations, and the average value of the three locations is defined as “1x at the first location”. min ”.

[0104] (3-5) The peak area intensity I3 of the sp3 carbon was calculated using image processing software ("PHIMultiPak" (trademark) manufactured by ULVAC PHI) for the C1s spectrum of the second point. max The peak area intensity I2 of sp2 carbon max Ratio I3 max / I2 max Ix max The measurement at the second location is performed in the measurement field of any three locations, and the average value of the three locations is defined as “1x at the second location”. max ”.

[0105] (3-6) Based on the above “Ix at the first location min ” and the above “Ix at the second location max”, calculate Ix min / Ix max .

[0106] About Ix at location 1 min For example, the lower limit can be set to 0.40, 0.45, 0.50, and the upper limit can be set to 0.70, 0.80, 0.90.

[0107] About Ix at the 2nd location max For example, the lower limit can be set to 0.40, 0.45, 0.50, and the upper limit can be set to 0.70, 0.80, 0.90.

[0108] (Average particle size)

[0109] At a minimum thickness d min The first location and thickness are the maximum value d max When the average particle size is measured by electron backscatter diffraction (EBSD) at the second location, the average particle size D at the first location is min The average particle size D at the second location max The ratio is D min / D max It is preferably 0.7 or more and 1 or less.

[0110] As a result, the tool life of the diamond coated tool is further improved. Although the reason is not clear, it is believed that the reason is that if D min / D max When the average particle size of diamond is equal to or greater than 0.7, the average particle size of diamond becomes uniform over the entire area of ​​the diamond layer, and the wear resistance and defect resistance of the diamond layer also become uniform in the blade portion.

[0111] The above D min / D max It is more preferably 0.7 or more and 1 or less, and even more preferably 0.85 or more and 1 or less.

[0112] In this specification, the "average particle size" refers to the median particle size (d50) in the volume-based particle size distribution (volume distribution).

[0113] Above D min / D max The calculation can be performed using the following steps (4-1) to (4-5).

[0114] (4-1) Based on the above-mentioned measurement results of the thickness of the diamond layer, determine the diamond layer with the minimum thickness d min The first location and thickness are the maximum value d maxAt the first and second locations, the diamond coated tool was cut by a wire electrical discharge machine in a direction perpendicular to the rotation axis O to expose the cross section. Each cross section was mirror polished using diamond slurry having an average particle size of 3 μm.

[0115] (4-2) In the cross section at each location, a 2 μm×2 μm rectangular measurement field (hereinafter also referred to as “EBSD measurement field”) is set in the diamond layer. The measurement field is set at a position where one side is 2 μm away from the surface of the diamond layer and the entire area is at least 2 μm away from the surface of the diamond layer.

[0116] (4-3) In the EBSD measurement field at the first location, the particle sizes of all diamonds contained in the measurement field are measured using the electron backscatter diffraction method to calculate the median particle size (d50). The electron backscatter diffraction device used is "SUPRA35VP" (trademark) manufactured by ZEISS. The measurement at the first location is performed in the measurement field of any three locations, and the average value of the three locations is set as "D50 at the first location". min ”.

[0117] (4-4) In the EBSD measurement field at the second location, the particle sizes of all diamonds contained in the measurement field are measured by electron backscatter diffraction, and the median particle size (d50) is calculated. The measurement at the second location is performed in the measurement field of any three locations, and the average value of the three locations is set as "D50 at the second location". max ”.

[0118] (4-5) Based on the above “D at the first location min ” and “D at the second location max ”, calculate D min / D max .

[0119] Regarding D at the 1st location min For example, the lower limit can be set to 50nm, 75nm, or 100nm, and the upper limit can be set to 800nm, 900nm, or 1000nm.

[0120] Regarding D at the second location max For example, the lower limit can be set to 50nm, 75nm, or 100nm, and the upper limit can be set to 800nm, 900nm, or 1000nm.

[0121] (Surface roughness Ra)

[0122] At a minimum thickness d min The first location and thickness are the maximum value d maxIn the second location, when the surface roughness Ra of the diamond layer is measured using a laser microscope, the surface roughness R at the first location is min The surface roughness R at the second location max R min / R max It is preferably 0.7 or more and 1 or less.

[0123] As a result, the tool life of the diamond coated tool is further improved. Although the reason is not clear, it is believed that the reason is that if R min / R max When the ratio is 0.7 or more, the surface roughness of the diamond becomes uniform over the entire area of ​​the diamond layer, and the wear resistance of the diamond layer also becomes uniform in the blade portion.

[0124] The above R min / R max It is more preferably 0.7 or more and 1 or less, and even more preferably 0.85 or more and 1 or less.

[0125] In this specification, "surface roughness Ra" refers to the arithmetic mean roughness Ra specified in JIS B 0601, which is defined as the following value: only a reference length is extracted from the roughness curve in the direction of its average line, and the distance from the average line of the extracted part to the measurement curve (absolute value of deviation) is summed and averaged.

[0126] The above R min / R max The calculation can be performed using the following steps (5-1) to (5-4).

[0127] (5-1) Based on the above-mentioned measurement results of the thickness of the diamond layer, determine the diamond layer with the minimum thickness d min The first location and thickness are the maximum value d max The second location.

[0128] (5-2) A 50 μm square measurement field of view is set on the surface of the diamond layer so as to include the first location. In this measurement field of view, the surface roughness is measured using a laser microscope ("OPTELICS HYBRID" (trademark) manufactured by Lasertech). This surface roughness is defined as "the surface roughness R of the first location". min ”.

[0129] (5-3) A 50 μm square measurement field of view is set on the surface of the diamond layer so as to include the second location. In this measurement field of view, a laser microscope ("OPTELICS HYBRID" (trademark) manufactured by Lasertech) is used to measure the surface roughness. This surface roughness is defined as "surface roughness R of the second location".max ”.

[0130] (5-4) Based on the above-mentioned "surface roughness R of the first location min ” and the above “surface roughness R at the second location max ”, calculate R min / R max .

[0131] Regarding the surface roughness R of the first point min For example, the lower limit can be set to 0.05, 0.06, 0.07, and the upper limit can be set to 0.21, 0.25, 0.30.

[0132] Regarding the surface roughness R of the second point max For example, the lower limit can be set to 0.05, 0.06, 0.07, and the upper limit can be set to 0.21, 0.25, 0.30.

[0133] [Implementation 1-2: Conical cutter]

[0134] In the embodiment 1-2, the case where the diamond coated tool is a tapered cutter is described. Figure 3 As shown, the tapered cutter as a diamond coated tool 210 includes a main body 23 and a shank 24 connected to the main body 23. In the main body 23, a cutting edge 25 having a peripheral edge 27 is formed, as shown in the XX line cross section. Figure 2 As shown, a substrate 1 and a diamond layer 2 provided on the substrate 1 are provided.

[0135] exist Figure 3 In the embodiment 1-2, the blade 25 extends along the rotation axis O of the tool. Therefore, in the embodiment 1-2, the length L of the blade 25 along the extending direction thereof refers to the length of the blade 25 along the rotation axis O of the tool.

[0136] exist Figure 3 In the figure, the entire body 23 belongs to the blade 25, but a part of the body 23 may be the blade.

[0137] d in the blade min / d max ,I min / I max , Ix min / Ix max , D min / D max , R min / R max And their measurement methods can be the same as those in Implementation 1-1, so their description will not be repeated.

[0138] [Implementation 1-3: Drill bit]

[0139] In Embodiment 1-3, the case where the diamond coated tool is a drill bit is described. Figure 4 This is a diagram for explaining a configuration example of a diamond coated tool according to Embodiment 1-3. Figure 5 yes Figure 4 An enlarged view of the first blade portion 35A. Figure 6 yes Figure 4 An enlarged view of the second blade portion 35B.

[0140] like Figures 4 to 6 As shown, the drill bit as a diamond coated tool 310 includes a body 33 and a shank 34 connected to the body 33. The body 33 includes a first blade portion 35A having a cutting edge 8A formed at the front end and a second blade portion 35B having a cutting edge 8B formed on the side of the shank 34. The cutting edge 8B is used to chamfer the hole entrance when drilling a hole.

[0141] The blade 35A and the blade 35B are as follows in the XX line cross section: Figure 2 As shown, a substrate 1 and a diamond layer 2 provided on the substrate 1 are provided.

[0142] exist Figure 4 In the embodiment, the blade 35A and the blade 35B extend along the rotation axis O of the tool. Therefore, in the embodiment 1-3, the length L of the blade 35A and the blade 35B along the extending direction thereof refers to the length of the blade 35A and the blade 35B along the rotation axis O of the tool.

[0143] The d between the blade 35A and the blade 35B min / d max ,I min / I max , Ix min / Ix max , D min / D max , R min / R max And their measurement methods can be the same as those in Implementation 1-1, so their description will not be repeated.

[0144] [Implementation 2: Method for manufacturing diamond coated tool]

[0145] The manufacturing method of the diamond coated tool disclosed in the present invention is a manufacturing method of the diamond coated tool of embodiment 1, which comprises a step of preparing a substrate (hereinafter also referred to as a "substrate preparation step") and a step of forming a diamond layer on the substrate using a hot wire CVD method to obtain a diamond coated tool (hereinafter also referred to as a "hot wire CVD step"), and the hot wire CVD method is carried out by controlling the temperature distribution in the blade portion of the substrate where the cutting edge exists to be within 5%.

[0146] (Substrate preparation process)

[0147] First, a substrate is prepared. The substrate is the same as that described in Embodiment 1-1, and therefore its description will not be repeated.

[0148] (Hot Wire CVD Process)

[0149] Next, a diamond layer is formed on the substrate using a hot wire CVD method to obtain a diamond coated tool. The hot wire CVD method, for example, forms a diamond layer on the substrate by heating the substrate while supplying methane and hydrogen into a vacuum furnace. The hot wire CVD method is performed by controlling the temperature distribution in the cutting edge portion of the substrate to within 5%.

[0150] Here, the temperature distribution in the cutting edge portion where the cutting edge exists is within 5% means that when the surface temperatures at both ends of the cutting edge region are measured using a radiation thermometer, the temperature difference is within 5% of the temperature at the cutting edge tip.

[0151] In order to deepen the understanding of the hot wire CVD method used in this disclosure, use Figure 11 to Figure 13 The conventional hot-filament CVD method will be described. Fig.11 This is a front view showing an example of a conventional hot-filament CVD apparatus.

[0152] Fig.12 yes Fig.11 Top view of the hot wire CVD device. Fig.13 This is a diagram showing the surface temperature distribution of a substrate when a film is formed by a conventional hot-filament CVD method.

[0153] like Fig.11 and Fig.12 As shown in FIG. 1 , a conventional hot-filament CVD apparatus 20 includes a filament 21 and a mounting table 22 for mounting a substrate in a vacuum furnace 201. In the conventional hot-filament CVD apparatus 20, it is considered that only a portion of the substrate 1 corresponding to the cutting edge (hereinafter also referred to as "edge region") 55 is required to enter the heating range of the hot filament. Therefore, a non-film forming region 56 corresponding to the handle or the like is arranged outside the heating range of the filament.

[0154] In this case, if Fig.13 As shown, the front end of the substrate (at Fig.13 The upper end in the middle is the highest temperature because there is no heat dissipation site. On the other hand, the temperature decreases as it moves toward the unheated handle side, and heat flows from the substrate 1 to the mounting table 22 side (at Fig.11 , the arrow in the figure is downward), resulting in a temperature distribution in the blade region 55. Based on this knowledge, the present inventors have found that placing the shank outside the heating range causes a decrease in the temperature of the tool blade on the shank side, which causes the film thickness distribution.

[0155] For this reason, the inventor has carried out in-depth research and found that: Fig.14 As shown, in the hot filament CVD device 220, the entire substrate 1 is set as the heating range of the filament 21, and a heat insulating material 23 is provided between the non-film forming area 56 such as the handle and the mounting table to improve the heat insulation and suppress the heat from flowing from the substrate 1 to the mounting table 22 side (in Fig.14 The arrow in the figure is the downward direction), thereby controlling the temperature distribution in the blade area to within 5%, and making the film thickness of the diamond layer in the blade uniform.

[0156] In this case, if Fig.15 As shown, the temperature distribution at the tip end and the shank side of the substrate becomes smaller, and the film thickness becomes uniform.

[0157] The method of making the temperature distribution in the cutting edge within 5% is not limited to the above method. The number of filaments for the substrate, the distance between the filament and the substrate, the position of the substrate in the furnace, etc. can be appropriately changed based on the shape of the substrate, the type of material, etc.

[0158] Example

[0159] This embodiment will be described in more detail using examples, but this embodiment is not limited to these examples.

[0160]

Sample 1

[0161] As the base material, a super-hard alloy was prepared. Figure 1 The end mill (φ10 mm) has the shape shown. The length L of the blade of the end mill is 30 mm.

[0162] Next, diamond powder was applied to the surface of the substrate to perform a seeding treatment. The seeding treatment was performed by applying diamond powder with an average particle size of 5 μm to the surface of the substrate, washing the substrate in ethanol, and then drying it. Next, the substrate subjected to the seeding treatment was placed on Fig.14 The hot wire CVD device shown.

[0163] The diamond layer of sample 1 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 800°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 1%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 1 having a diamond layer formed on the substrate was obtained.

[0164] [Sample 2 to Sample 4]

[0165] For the substrates of Samples 2 to 4, the same substrates as those of Sample 1 were prepared and seeded by the same method as that of Sample 1. A diamond layer was formed on the substrate using the same hot filament CVD apparatus as that of Sample 1 to obtain a diamond coated tool.

[0166] The diamond layer of sample 2 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 780°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 1%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 2 having a diamond layer formed on the substrate was obtained.

[0167] The diamond layer of sample 3 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 780°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 3%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 3 having a diamond layer formed on the substrate was obtained.

[0168] The diamond layer of sample 3-1 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 760°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 3%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 3-1 having a diamond layer formed on the substrate was obtained.

[0169] The diamond layer of sample 3-2 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 800°C. Methane and hydrogen were supplied to the furnace at a controlled flow rate so that the methane concentration reached 4%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 3-1 having a diamond layer formed on the substrate was obtained.

[0170] The diamond layer of sample 4 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 800°C. Methane and hydrogen were supplied to the furnace at a controlled flow rate so that the methane concentration reached 3%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the blade portion of the substrate where the cutting edge existed was within 5%. Thus, a diamond-coated tool of sample 4 having a diamond layer formed on the substrate was obtained.

[0171] [Sample 5 to Sample 8]

[0172] For samples 5 to 8, the same substrate as sample 1 was prepared and seeded in the same manner as sample 1. A diamond layer was formed on the substrate using a hot filament CVD device by a method not considering temperature distribution control to obtain a diamond coated tool.

[0173] The diamond layer of sample 5 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 780°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 3%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the cutting edge portion of the substrate where the cutting edge existed exceeded 5%. Thus, the diamond-coated tool of sample 5 was obtained.

[0174] The diamond layer of sample 6 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 800°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 3%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the cutting edge portion of the substrate where the cutting edge existed exceeded 5%. Thus, the diamond-coated tool of sample 6 was obtained.

[0175] The diamond layer of sample 7 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 800°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 1%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the cutting edge portion of the substrate where the cutting edge existed exceeded 5%. Thus, the diamond-coated tool of sample 7 was obtained.

[0176] The diamond layer of sample 8 was formed under the following conditions. The filament current was controlled so that the tool surface temperature reached an average of 780°C. Methane and hydrogen were supplied to the furnace at a flow rate controlled so that the methane concentration reached 1%. The pressure during film formation was set to 500 mPa. During film formation, the temperature distribution in the cutting edge portion of the substrate where the cutting edge existed exceeded 5%. Thus, the diamond-coated tool of sample 8 was obtained.

[0177] <Evaluation>

[0178] (d min / d max d min / d max ,I min / I max , Ix min / Ix max , D min / D max , R min / R max )

[0179] For the diamond coated tools of samples 1 to 8, the d min / d max d min / d max ,I min / I max , Ix min / Ix max , D min / D max , R min / R max The specific measurement method is described in Embodiment 1, so the description thereof will not be repeated. The results are shown in Table 1.

[0180] (Cutting test)

[0181] Using the diamond coated tools of Samples 1 to 8, cutting tests were performed under the following conditions.

[0182] Workpiece: Carbon fiber reinforced resin

[0183] Cutting speed: 270m / min.

[0184] Speed: 8600rpm

[0185] Feed speed: 860m / min.

[0186] Cutting: 10mm

[0187] In the above-mentioned cutting test, the distance until the diamond layer peeled off (peeling distance) was measured. The peeling of the diamond layer was confirmed by observation based on an optical microscope. The longer the peeling distance, the longer the tool life. The results are shown in Table 1.

[0188]

[0189] <Investigation>

[0190] The methods for manufacturing the diamond coated tools of Samples 1 to 4 belong to the examples. The diamond coated tools of Samples 1 to 4 belong to the examples. It was confirmed that the diamond coated tools of Samples 1 to 4 had a long peeling distance and a long tool life.

[0191] The manufacturing methods of the diamond coated tools of Samples 5 to 8 are comparative examples. The diamond coated tools of Samples 5 to 8 are comparative examples. The peeling distances of the diamond coated tools of Samples 5 to 8 are shorter than those of Samples 1 to 4.

[0192] As mentioned above, although embodiment and Example of this disclosure were described, it is expected from the outset that the structure of each embodiment and Example mentioned above may be appropriately combined or variously modified.

[0193] The embodiments and examples disclosed this time should be considered as illustrative in all aspects and are not intended to limit the present invention. The scope of the present invention is not shown by the above-mentioned embodiments and examples, but by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims.

[0194] Description of Reference Numerals

[0195] 1 substrate; 2 diamond layer; 3, 23, 33 main body; 4, 24, 34 handle; 5, 25, 35A, 35B blade; 6 bottom blade; 7, 27 peripheral blade; 8, 8A, 8B cutting edge; 10, 210, 310, 410 diamond coated tool; 20, 220 hot wire CVD device; 21 filament; 55 blade area; 56 non-film forming area; 201 vacuum furnace.

Claims

1. A diamond coated tool comprising a cutting edge portion consisting of a substrate and a diamond layer provided on the substrate, wherein: The length of the blade along its extension direction is L, In the blade, at 11 points in total arranged at a distance of L / 10 from one end along the direction along the extension direction, when the thickness of the diamond layer is measured, the minimum value d of the thickness at all the points is min With the maximum value of the thickness d max The ratio of d min / d max is greater than 0.7 and less than 1, The thickness is the minimum value d min The first location and the thickness is the maximum value d max In the second location, when the average grain size of the diamond layer is measured by electron backscatter diffraction, The average particle size D at the first location min The average particle size D at the second location max The ratio is D min / D max It is greater than or equal to 0.7 and less than or equal to 1.

2. The diamond coated tool according to claim 1, wherein: The d min / d max It is greater than or equal to 0.85 and less than 1.

3. The diamond coated tool according to claim 1 or 2, wherein: The minimum thickness of the diamond layer is d min It is 3 μm or more and 30 μm or less.

4. The diamond coated tool according to claim 1 or 2, wherein: The maximum thickness d of the diamond layer max It is 3 μm or more and 30 μm or less.

5. The diamond coated tool according to claim 1 or 2, wherein: The thickness is the minimum value d min The first location and the thickness is the maximum value d max In the second location, the Raman shift of the diamond layer is measured from 900 cm -1 Up to 2000cm -1 In the case of Raman spectroscopy, I min with I max Ratio I min / I max is greater than or equal to 0.7 and less than or equal to 1, the I min is the peak area intensity Id of diamond at the first location min The area intensity Is of the entire spectrum min Ratio Id min / Is min , the I max is the peak area intensity Id of diamond at the second location max The area intensity Is of the entire spectrum max Ratio Id max / Is max .

6. The diamond coated tool according to claim 5, wherein: The first location I min is greater than 0.25 and less than 0.90, and the I at the second location max It is 0.25 or more and 0.90 or less.

7. The diamond coated tool according to claim 1 or 2, wherein: The thickness is the minimum value d min The first location and the thickness is the maximum value d max In the second location, when the C1s spectrum of the diamond layer is measured by X-ray photoelectron spectroscopy, Ix min With Ix max Ratio Ix min / Ix max is greater than or equal to 0.7 and less than or equal to 1, the Ix min is the peak area intensity I3 of the sp3 carbon at the first location min The peak area intensity I2 of sp2 carbon min Ratio I3 min / I2 min , the 1x max is the peak area intensity I3 of the sp3 carbon at the second location max The peak area intensity I2 of sp2 carbon max Ratio I3 max / I2 max .

8. The diamond coated tool according to claim 7, wherein: Ix at the first location min is greater than or equal to 0.40 and less than or equal to 0.90, and Ix at the second location max It is 0.40 or more and 0.90 or less.

9. The diamond coated tool according to claim 1, wherein: The average particle size D at the first location min is greater than or equal to 50 nm and less than or equal to 1000 nm, and the average particle size D at the second location is max It is greater than or equal to 50 nm and less than or equal to 1000 nm.

10. The diamond coated tool according to claim 1 or 2, wherein: The thickness is the minimum value d min The first location and the thickness is the maximum value d max In the second location, when the surface roughness Ra of the diamond layer is measured using a laser microscope, The surface roughness R at the first location min The surface roughness R at the second location max R min / R max It is greater than or equal to 0.7 and less than or equal to 1.

11. The diamond coated tool according to claim 10, wherein: The surface roughness R at the first location min is greater than or equal to 0.05 and less than or equal to 0.30, and the surface roughness R at the second location max It is 0.05 or more and 0.30 or less.

12. A method for manufacturing a diamond coated tool, the method for manufacturing a diamond coated tool according to any one of claims 1 to 11, wherein: The manufacturing method comprises: The process of preparing the substrate; and A step of forming a diamond layer on the substrate by hot wire CVD to obtain a diamond coated tool, The hot wire CVD method is performed by controlling the temperature distribution in the cutting edge portion of the substrate to within 5%. In the hot-filament CVD device, the entire substrate is set as the heating range of the filament, and a heat insulating material is provided between the non-film formation area and the mounting stage.