Sputtering targets for heat-assisted magnetic recording media
By using specific melting point oxides as grain boundary materials in FePt magnetic particles, the problems of thermal fluctuations and insufficient signal-to-noise ratio in magnetic recording media are solved, a magnetic recording medium with high recording density and thermal stability is achieved, and magnetic recording is improved. Media performance.
Patent Information
- Application Number
- CN202080074953.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing magnetic recording media have problems with thermal fluctuations and insufficient signal-to-noise ratio during the process of high recording density. In particular, it is difficult to improve the thermal stability and signal-to-noise ratio of FePt magnetic particles.
An oxide with a specific melting point range is used as the grain boundary material of FePt magnetic particles. Through the design of the sputtering target, a heat-assisted magnetic recording medium with high saturation magnetization and magnetocrystalline anisotropy constant is formed. Specifically, the temperature is above 800°C and Oxides below 1100°C, such as SnO, PbO, and Bi2O3, are used as non-magnetic materials to optimize the magnetic film structure of FePt alloys.
It achieves the improvement of uniaxial magnetic anisotropy, thermal stability and signal-to-noise ratio, forms a high recording density magnetic recording medium, reduces noise and thermal fluctuations, and improves the performance of magnetic recording media.
Smart Images

Figure CN114600190B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a sputtering target for a thermally assisted magnetic recording medium, and in particular to a sputtering target for a thermally assisted magnetic recording medium containing a Fe-Pt alloy and a non-magnetic material as main components. Background Art
[0002] In the disk of a hard disk drive, information signals are recorded in tiny bits of the magnetic recording medium. In order to further increase the recording density of the magnetic recording medium, it is necessary to reduce the size of the bit holding a recorded information and increase the signal-to-noise ratio, which is an indicator of information quality. In order to increase the signal-to-noise ratio, it is essential to increase the signal or reduce the noise.
[0003] Currently, magnetic thin films having a granular structure of CoPt alloy-oxide are used as magnetic recording media for recording information signals (see, for example, Non-Patent Document 1). The granular structure is composed of columnar CoPt alloy grains and grain boundaries of oxide surrounding the grains.
[0004] When increasing the recording density of such a magnetic recording medium, it is necessary to smooth the transition region between recording bits to reduce noise. In order to smooth the transition region between recording bits, it is necessary to refine the CoPt alloy grains contained in the magnetic thin film.
[0005] On the other hand, when the magnetic crystal grains are miniaturized, the intensity of the recorded signal that can be retained by one magnetic crystal grain decreases. In order to achieve both miniaturization of the magnetic crystal grains and the intensity of the recorded signal, the distance between the centers of the crystal grains needs to be reduced.
[0006] On the other hand, as the CoPt alloy grains in the magnetic recording medium are refined, the so-called thermal fluctuation phenomenon may occur, in which the thermal stability of the recorded signal is impaired due to the superparamagnetic phenomenon, causing the recorded signal to disappear. This thermal fluctuation phenomenon is a major obstacle to achieving higher recording density in magnetic disks.
[0007] In order to solve this obstacle, it is necessary to increase the magnetic energy of each CoPt alloy grain so that the magnetic energy overcomes the thermal energy. The magnetic energy of each CoPt alloy grain is determined by the product v×Ku of the volume v of the CoPt alloy grain and the magnetocrystalline anisotropy constant Ku. Therefore, in order to increase the magnetic energy of the CoPt alloy grain, it is essential to increase the magnetocrystalline anisotropy constant Ku of the CoPt alloy grain (for example, refer to non-patent document 2).
[0008] In addition, in order to make CoPt alloy grains with large Ku grow in a columnar shape, it is necessary to achieve phase separation between CoPt alloy grains and grain boundary materials. If the phase separation between CoPt alloy grains and grain boundary materials is insufficient and the inter-grain interaction between CoPt alloy grains increases, the coercive force Hc of the magnetic film containing the granular structure of CoPt alloy-oxide decreases, the thermal stability is impaired, and it becomes easy to cause thermal fluctuations. Therefore, it is also important to reduce the inter-grain interaction between CoPt alloy grains.
[0009] The refinement of magnetic crystal grains and the reduction of the center-to-center distance of magnetic crystal grains may be achieved by refining the crystal grains of the Ru underlayer (underlayer provided for the purpose of controlling the orientation of the magnetic recording medium).
[0010] However, it is difficult to refine the grains of the Ru underlayer while maintaining the crystal orientation (for example, see Non-Patent Document 3). Therefore, the grain size of the Ru underlayer of the existing magnetic recording medium is about 7nm to 8nm, which is almost unchanged from the size when the in-plane magnetic recording medium is converted into a perpendicular magnetic recording medium.
[0011] On the other hand, from the perspective of improving the magnetic recording layer instead of the Ru base layer, research has also been conducted to promote the miniaturization of magnetic grains. Specifically, the following method has been studied: increasing the amount of oxide added to the CoPt alloy-oxide magnetic film and reducing the volume ratio of the magnetic grains to miniaturize the magnetic grains (for example, refer to non-patent document 4). And the miniaturization of magnetic grains was achieved by this method. However, in this method, the width of the grain boundary is increased by increasing the amount of oxide added, so the center-to-center distance of the magnetic grains cannot be reduced.
[0012] In addition, the following method has been studied: in addition to the single oxide used in the conventional CoPt alloy-oxide magnetic film, a second oxide is added (for example, refer to non-patent document 5). However, when adding multiple oxide materials, the material selection policy is not clear, and even now, the oxide used as the grain boundary material for CoPt alloy grains is still under study. The inventors have found that in order to achieve the refinement of magnetic grains in the magnetic film and the reduction of the center-to-center distance of the magnetic grains, a low-melting-point oxide and a high-melting-point oxide (specifically, B containing a melting point as low as 450°C) are preferably used. 2 O 3 and high melting point oxides having a melting point higher than that of CoPt alloy (about 1450°C) are effective, and a B 2 O 3 A sputtering target for magnetic recording containing a CoPt alloy and an oxide having a high melting point (Patent Document 1).
[0013] On the other hand, with L1 0 FePt alloys with a structure other than CoPt alloys have attracted attention as materials for ultra-high density recording media, and a granular structure magnetic film in which FePt magnetic particles are isolated by C (carbon) has been proposed as a magnetic recording medium for the next generation hard disk using a heat-assisted magnetic recording method (Patent Document 2). However, C (carbon) is a difficult-to-sinter material, so it is extremely difficult to obtain a dense sintered body, and there is a problem of a large number of particles being generated during sputtering. In addition, as described later, the inventors' experiments have shown that when C (carbon) is used as the grain boundary material for FePt magnetic particles, the saturation magnetization intensity (M s grain ) is reduced. A reduction in saturation magnetization leads to a reduction in thermal stability, which is not preferred.
[0014] Prior art literature
[0015] Patent Literature
[0016] Patent Document 1: WO2018 / 083951
[0017] Patent Document 2: Japanese Patent No. 5946922
[0018] Non-patent literature
[0019] Non-patent document 1: T. Oikawa et al., IEEE TRANSACTIONS ON MAGNETICS, September 2002, VOL.38, NO.5, p.1976-1978
[0020] Non-patent document 2: SNPiramanayagam, JOURNAL OF APPLIED PHYSICS, 2007, 102, 011301
[0021] Non-patent document 3: SNPiramanayagam et al., APPLIED PHYSICS LETTERS, 2006, 89, 162504
[0022] Non-patent document 4: Y. Inaba et al., IEEE TRANSACTIONS ON MAGNETICS, July 2004, VOL.40, NO.4, p.2486-2488
[0023] Non-patent document 5: I. Tamai et al., IEEE TRANSACTIONS ON MAGNETICS, November 2008, VOL.44, NO.11, p.3492-3495 Summary of the invention
[0024] Problems to be solved by the invention
[0025] The present invention aims to provide a sputtering target for forming a granular magnetic thin film in which FePt magnetic grains are isolated by oxides, constituting a heat-assisted magnetic recording medium having improved uniaxial magnetic anisotropy, thermal stability and SNR (signal-to-noise ratio), in order to further increase capacity.
[0026] Methods used to solve problems
[0027] The present inventors used various oxides as grain boundary materials to isolate FePt magnetic particles and studied the saturation magnetization (M s grain ) and the magnetocrystalline anisotropy constant (Ku) which is an indicator of thermal stability grain (Ku of FePt magnetic particles other than oxides)), it was found that by using oxides with a melting point in a specific range as grain boundary materials, a saturation magnetization (M s grain ) and the magnetocrystalline anisotropy constant (Ku grain ) are high, and the use of a sputtering target containing an oxide having a melting point in a specific range as a non-magnetic material is effective for forming the thermally assisted magnetic recording medium, thereby completing the present invention.
[0028] According to the present invention, a sputtering target for a thermally assisted magnetic recording medium (hereinafter sometimes referred to as "sputtering target" or "target") is provided, which is a sputtering target for a thermally assisted magnetic recording medium comprising a FePt alloy, a non-magnetic material and inevitable impurities, characterized in that the non-magnetic material is an oxide having a melting point of above 800°C and below 1100°C.
[0029] The sputtering target of the present invention contains FePt alloy as a main component. FePt alloy becomes a constituent component of magnetic crystal grains (micro magnets) in the granular structure of a magnetic thin film of a thermally assisted magnetic recording medium formed by sputtering.
[0030] Fe is a ferromagnetic metal element and plays a core role in the formation of magnetic grains (tiny magnets) of the granular structure of the magnetic film of the thermally assisted magnetic recording medium. From the viewpoint of increasing the magnetocrystalline anisotropy constant Ku of the FePt alloy grains (magnetic grains) in the magnetic film obtained by sputtering and maintaining the magnetism of the FePt alloy grains (magnetic grains) in the obtained magnetic film, the content ratio of Fe in the sputtering target of the present invention is preferably set to 40 mol% or more and 60 mol% or less relative to the total metal component, and more preferably set to 45 mol% or more and 55 mol% or less relative to the total metal component.
[0031] Pt has the function of reducing the magnetic moment of the alloy by alloying with Fe in a predetermined composition range, and has the function of adjusting the strength of the magnetism of the magnetic grains. From the viewpoint of increasing the magnetocrystalline anisotropy constant Ku of the FePt alloy grains (magnetic grains) in the magnetic film of the thermally assisted magnetic recording medium obtained by sputtering and adjusting the magnetism of the FePt alloy grains (magnetic grains) in the obtained magnetic film, the content ratio of Pt in the sputtering target of the present invention is preferably set to 40 mol% or more and 60 mol% or less relative to the total metal component, and more preferably set to 45 mol% or more and 55 mol% or less relative to the total metal component.
[0032] In addition, the sputtering target of the present invention may contain one or more additional elements selected from Ag, Au, and Cu as metal components in addition to Fe and Pt. These metal elements are used to reduce the L1 0 The amount of the additional metal element added is not particularly limited as long as it is within the range that does not damage the properties of the thermally assisted magnetic recording medium as a magnetic film. For example, the content ratio of the additional metal element in the sputtering target of the present invention is preferably 0 mol% or more and 20 mol% or less relative to the total metal component, and more preferably 0 mol% or more and 10 mol% or less relative to the total metal component.
[0033] Hereinafter, in the present specification, an alloy composed of Fe and Pt is referred to as a "FePt alloy", and an alloy containing one or more elements selected from Ag, Au, or Cu in addition to Fe and Pt is referred to as a "FePt-based alloy".
[0034] The non-magnetic material contained in the sputtering target of the present invention is an oxide having a melting point of 800°C to 1100°C. In the magnetic film formed by sputtering a target containing an oxide having a melting point of 800°C to 1100°C, the oxide can be arranged as a grain boundary material of FePt magnetic grains, and a thermally assisted magnetic recording medium having the magnetic film can achieve about 950emu / cm 3 Saturation magnetization (M s grain ) and 2.5×10 7 erg / cm 3 The magnetocrystalline anisotropy constant (Ku grain ). The details are as follows. Figure 2 and 3 As shown in FIG. 1 , it can be seen that the lower the melting point of the oxide used as the grain boundary material of the FePt magnetic grains, the higher the saturation magnetization (M s grain) is higher, but when an oxide with a melting point below 800°C is used as the grain boundary material, the magnetocrystalline anisotropy constant (Ku grain ) becomes low, and the saturation magnetization intensity (M s grain ) and the magnetocrystalline anisotropy constant (Ku grain ) are both high. Therefore, the sputtering target of the present invention contains an oxide having a melting point of 800°C or more and 1100°C or less. By using the sputtering target, the oxide can be used as a grain boundary material of a thermally assisted magnetic recording medium. As the oxide having a melting point of 800°C or more and 1100°C or less, particularly preferably, SnO (melting point 1080°C), PbO (melting point 886°C), Bi 2 O 3 (melting point 817°C) one or more oxides.
[0035] The content of the non-magnetic material in the sputtering target of the present invention is preferably 25% by volume or more and 40% by volume or less, more preferably 27% by volume or more and 36% by volume or less, and further preferably 29% by volume or more and 32% by volume or less. By making the content of the non-magnetic material within the above range, the FePt magnetic particles can be reliably separated from each other in the magnetic layer of the magnetic recording medium formed using the sputtering target of the present invention, the magnetic particles can be easily isolated, and the recording density can be improved.
[0036] The microstructure of the sputtering target of the present invention is not particularly limited, but is preferably a microstructure in which a metal phase and an oxide phase are finely dispersed with each other. By forming such a microstructure, defects such as nodules and particles are less likely to occur during sputtering.
[0037] The sputtering target of the present invention can be produced, for example, as follows.
[0038] The metal components are weighed to obtain a predetermined composition to prepare a FePt alloy melt. Then, gas atomization is performed to prepare FePt alloy atomized powder. The prepared FePt alloy atomized powder is classified to reduce the particle size to a predetermined particle size or less (e.g., 106 μm or less).
[0039] Add oxide powder (SnO, PbO and / or Bi) with a melting point of 800°C or more and 1100°C or less to the prepared FePt alloy atomized powder. 2 O 3) and additional metal element powder (e.g., Ag, Au and / or Cu) as required, are mixed and dispersed in a ball mill to produce a mixed powder for pressure sintering. The FePt alloy atomized powder, the oxide powder and other metal element powders as required are mixed and dispersed in a ball mill to produce a mixed powder for pressure sintering in which the FePt alloy atomized powder, the oxide powder and other metal element powders as required are finely dispersed with each other.
[0040] Alternatively, FePt alloy atomized powder containing Fe and Pt and additional metal elements, oxide powder (SnO, PbO and / or Bi) with a melting point of 800°C to 1100°C may be added. 2 O 3 ), and mixed and dispersed in a ball mill to prepare a mixed powder for pressure sintering.
[0041] The prepared mixed powder for pressure sintering is subjected to pressure sintering, for example, by vacuum hot pressing, and is molded to produce a sputtering target. The mixed powder for pressure sintering is mixed and dispersed in a ball mill, and the FePt alloy atomized powder and the above-mentioned oxide powder and other metal element powders as required are finely dispersed with each other, or the FePt alloy atomized powder and the oxide powder are finely dispersed with each other, so when the sputtering target obtained by this manufacturing method is sputtered, it is not easy to cause defects such as nodules and the generation of particles. It should be noted that the method for pressure sintering the mixed powder for pressure sintering is not particularly limited, and can be a method other than vacuum hot pressing, for example, a HIP method can be used.
[0042] When preparing the mixed powder for pressure sintering, it is not limited to the alloy atomized powder, and powders of each metal element can also be used. In this case, Fe metal element powder, Pt metal element powder, the above oxide powder and other metal element element powders as needed can be mixed and dispersed by a ball mill to prepare the mixed powder for pressure sintering.
[0043] Effects of the Invention
[0044] The sputtering target for the heat-assisted magnetic recording medium of the present invention can form a granular magnetic thin film for a high-recording-density magnetic recording medium having improved uniaxial magnetic anisotropy, thermal stability and SNR. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 : is the magnetization curve of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film.
[0046] Figure 2The melting point and magnetocrystalline anisotropy (Ku) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film are shown in FIG. grain )’s relationship diagram.
[0047] Figure 3 The figure shows the melting point and saturation magnetization intensity (M) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film. s grain )’s relationship diagram.
[0048] Figure 4 The melting point and coercivity (H) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film are shown in FIG. c )’s relationship diagram.
[0049] Figure 5 This is an X-ray diffraction spectrum obtained by measuring the crystal orientation of the plane perpendicular component and the in-plane component of the heat-assisted FePt granular magnetic recording medium using X-ray diffraction.
[0050] Figure 6 The melting point and order degree (S) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film are shown in FIG. in )’s relationship diagram.
[0051] Figure 7 Graph showing the relationship between the melting point and the crystal grain size (GD) of the non-magnetic material of a FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film.
[0052] Figure 8 The graph shows the particle size (GD) and order (S) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film. in )’s relationship diagram.
[0053] Fig. 9 Figure 2 shows the relationship between the grain size (GD) and coercivity (H) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film. c )’s relationship diagram.
[0054] Fig.10 The order degree (S) of the non-magnetic material of the FePt granular magnetic recording medium having a FePt-30 volume % X (X is a non-magnetic material) magnetic film is shown in FIG. in ) and coercivity (H c )’s relationship diagram.
[0055] Fig.11 To show the relationship between the content of non-magnetic material and magnetocrystalline anisotropy (Ku) of FePt granular magnetic recording media having FePt-SnO magnetic films. grain )’s relationship diagram.
[0056] Fig.12 The relationship between the content of non-magnetic material and the saturation magnetization (M) of FePt granular magnetic recording media having FePt-SnO magnetic films is shown in FIG. s grain )’s relationship diagram.
[0057] Fig.13 The relationship between the content of non-magnetic material and the coercive force (H) of FePt granular magnetic recording media having FePt-SnO magnetic films is shown in FIG. c )’s relationship diagram. DETAILED DESCRIPTION
[0058] Example
[0059] The present invention will be described in detail below, but the present invention is not limited thereto.
[0060] [Example 1]
[0061] A target of FePt-30 volume % X (X is a nonmagnetic material) in which 30 volume % of each nonmagnetic material shown in Table 1 was blended was prepared.
[0062] First, a 50Fe-50Pt alloy atomized powder is prepared. Specifically, each metal is weighed so as to have a composition of 50 atomic % Fe and 50 atomic % Pt, and both metals are heated to 1500° C. or higher to form an alloy melt, which is then gas atomized to produce a 50Fe-50Pt alloy atomized powder.
[0063] The prepared 50Fe-50Pt alloy atomized powder was classified with a 150-mesh sieve to obtain 50Fe-50Pt alloy atomized powders with a particle size of less than 106 μm.
[0064] To the classified 50Fe-50Pt alloy atomized powder was added powder of the non-magnetic material shown in Table 1 as X so as to have a composition of (50Fe-50Pt)-30 volume % X (X is each non-magnetic material shown in Table 1), and the mixture was mixed and dispersed using a ball mill to obtain 16 kinds of mixed powders for pressure sintering containing different non-magnetic materials.
[0065] Then, the prepared mixed powder for pressure sintering is used to obtain a sintered body by hot pressing under vacuum conditions. For example, SnO is used as the non-magnetic material X, and the sintering temperature is 960°C, the sintering pressure is 24.5 MPa, the sintering time is 60 minutes, and the atmosphere is 5×10 -2 Pa or less vacuum conditions were used to produce a step-shaped target (50Fe-50Pt)-30 volume % SnO with a diameter of 153.0×1.0mm (upper stage) and 161.0×4.0mm (lower stage). The relative density of the produced target was 96.5%. For other non-magnetic materials, sintered bodies were prepared under the conditions shown in Table 2 to produce targets.
[0066] The prepared target was used for sputtering with a DC sputtering device (manufactured by Canon Anelva Corporation) to form a magnetic thin film composed of (50Fe-50Pt)-30 vol % X on a glass substrate, thereby preparing a sample for measuring magnetic properties and a sample for structural observation. Specifically, a CoW seed layer with a thickness of 80 nm was formed on a glass plate by DC sputtering (1.5 kW, 0.6 Pa), a MgO base film with a thickness of 5 nm was formed on the CoW seed layer by RF magnetron sputtering (0.5 kW, 4.0 Pa), a FePt-30 volume %X (X is a non-magnetic material shown in Table 1) magnetic film with a thickness of 10 nm was formed on the MgO base film by DC sputtering (0.1 kW, 8.0 Pa, Ar gas), and a C surface protective layer with a thickness of 7 nm was formed on the magnetic film by DC sputtering (0.3 kW, 0.6 Pa), thereby obtaining a thermally assisted FePt granular magnetic recording medium, and the magnetic properties (magnetocrystalline anisotropy and saturation magnetization) were measured using a SQUID-VSM (Max 7 T) and a PPMS torque magnetometer (Max 9 T). The measurement results are shown in Table 1, and the magnetization curves are shown in Figure 1 In addition, the melting point of non-magnetic materials and the magnetocrystalline anisotropy (K u grain ), saturation magnetization (M s grain ), Coercivity (H c The results obtained by plotting the relationship between Figure 2 , 3 Furthermore, the results of measuring the crystal orientation of the plane perpendicular component and the in-plane component of the heat-assisted FePt granular magnetic recording medium by X-ray diffraction are shown in Figure 5 .
[0067] in addition, Figure 5The order of the thermally assisted FePt granular magnetic recording medium was determined by the integrated intensity of the FePt (110) and FePt (220) diffraction peaks using the formula (1): Degree of order (S in ), the melting point and order degree (S in ) and plot the resulting graph on Figure 6 . Order S in It indicates the degree of structure of repeated stacking of Fe and Pt atoms in the film thickness direction. When Fe and Pt atoms are completely and repeatedly stacked without defects, S in is 1.0 (theoretical value). In addition, when Fe and Pt atoms are not completely stacked repeatedly, S in is 0.
[0068]
[0069] Furthermore, using Figure 5 The FePt (200) diffraction peak of the in-plane diffraction spectrum of the heat-assisted FePt granular magnetic recording medium was evaluated by formula (2): Grain diameter (GD). The relationship between the melting point of the non-magnetic material and the crystal grain diameter (GD) was plotted and the resulting graph was displayed in Figure 7 .
[0070]
[0071] Here, λ is the wavelength of the radiation source of the X-ray diffraction device, 0.1542 nm, β is the half-maximum full width of the FePt (200) diffraction peak, and θχ is the diffraction angle of the FePt (200) diffraction peak.
[0072] Furthermore, the correlation between the order degree and the crystal particle size is shown in Figure 8 , the coercive force (H c The correlation between ) and the crystal particle size is shown in Fig. 9 , the coercive force (H c The correlation between ) and order is shown in Fig.10 .
[0073] [Table 1]
[0074] Table 1 Measurement results
[0075] Non-magnetic materials Melting point <![CDATA[M s grain ]]> <![CDATA[K u grain ]]> <![CDATA[H c (Coercivity)]]> ℃ <![CDATA[emu / cm 3 ]]> <![CDATA[erg / cm 3 ]]> k <![CDATA[B 2 THE 3 ]]> 450 1079 1.28E+07 3.50 <![CDATA[MoO 3 ]]> 795 1059 1.86E+07 0.26 SnO 1080 1014 3.04E+07 29.00 PbO 886 955 2.55E+07 24.00 <![CDATA[Bi 2 THE 3 ]]> 817 975 2.70E+07 26.00 <![CDATA[GeO 2 ]]> 1115 914 2.54E+07 19.50 <![CDATA[WO 3 ]]> 1473 944 1.26E+07 8.50 <![CDATA[Nb 2 THE 5 ]]> 1512 881 1.08E+07 15.63 <![CDATA[SiO 2 ]]> 1723 836 2.27E+07 19.00 <![CDATA[TiO 2 ]]> 1857 837 1.21E+07 9.50 MnO 1945 823 1.82E+07 26.68 <![CDATA[Y 2 THE 3 ]]> 2425 796 1.89E+07 6.50 <![CDATA[Zr 2 The]]> 2715 824 0.83E+07 6.50 MgO 2852 791 1.86E+07 26.08 BN 2973 764 2.94E+07 21.50 C 3500 710 2.23E+07 29.25
[0076] [Table 2]
[0077] Table 2 Sintering conditions and relative density of targets for various non-magnetic materials
[0078] Non-magnetic materials Sintering temperature Sintering pressure Sintering time atmosphere Relative density ℃ MPa minute Pa % <![CDATA[B 2 THE 3 ]]> 800 30.6 60 <![CDATA[5×10 -2 ]]> 102.5 <![CDATA[MoO 3 ]]> 980 24.5 60 <![CDATA[5×10 -2 ]]> 101.4 SnO 960 24.5 60 <![CDATA[5×10 -2 ]]> 96.5 PbO 960 24.5 60 <![CDATA[5×10 -2 ]]> 96.8 <![CDATA[Bi 2 THE 3 ]]> 960 24.5 60 <![CDATA[5×10 -2 ]]> 97.2 <![CDATA[GeO 2 ]]> 770 24.5 60 <![CDATA[5×10 -2 ]]> 102.0 <![CDATA[WO 3 ]]> 1040 24.5 60 <![CDATA[5×10 -2 ]]> 101.2 <![CDATA[Nb 2 THE 5 ]]> 1070 24.5 60 <![CDATA[5×10 -2 ]]> 102.4 <![CDATA[SiO 2 ]]> 990 30.6 60 <![CDATA[5×10 -2 ]]> 95.7 <![CDATA[TiO 2 ]]> 1020 24.5 60 <![CDATA[5×10 -2 ]]> 96.8 MnO 950 24.5 60 <![CDATA[5×10 -2 ]]> 98.8 <![CDATA[Y 2 THE 3 ]]> 1200 24.5 60 <![CDATA[5×10 -2 ]]> 96.5 <![CDATA[Zr 2 The]]> 1000 24.5 60 <![CDATA[5×10 -2 ]]> 97.1 MgO 940 24.5 60 <![CDATA[5×10 -2 ]]> 95.7 BN 900 65.7 60 <![CDATA[5×10 -2 ]]> 90.2 C 900 30.6 60 <![CDATA[5×10 -2 ]]> 91.2
[0079] Depend on Figure 1 It can be seen that the hysteresis of the magnetic recording medium depends on the grain boundary material (non-magnetic material of the sputtering target), and good results are obtained when SnO (melting point 1080°C), MnO (melting point 1945°C), MgO (melting point 2852°C) and C (melting point 3500°C) are used as grain boundary materials. In addition, as shown in Table 1, when SnO (melting point 1080°C), MnO (melting point 1945°C) and C (melting point 3500°C) are used, the coercive force is also high.
[0080] Depend on Figure 2 It can be seen that the magnetocrystalline anisotropy (Ku grain ) depends on the grain boundary material (non-magnetic material of the sputtering target), using SnO (melting point 1080℃), PbO (melting point 886℃), Bi 2 O 3 (melting point 817℃), GeO 2 (melting point 1115°C) and BN (melting point 2973°C) as grain boundary materials, showing a 2.5×10 7 erg / cm 3 High magnetocrystalline anisotropy above .
[0081] Depend on Figure 3 It can be seen that the saturation magnetization intensity (M s grain ) depends on the grain boundary material (non-magnetic material of the sputtering target). In particular, a high correlation is observed with respect to the melting point of the grain boundary material. The lower the melting point, the higher the saturation magnetization intensity. SnO (melting point 1080°C), PbO (melting point 886°C), Bi 2 O 3 (melting point 817°C) as a grain boundary material, showing 950emu / cm 3 The saturation magnetization intensity is 1000emu / cm, especially when SnO (melting point 1080℃) is used as the grain boundary material. 3 above the saturation magnetization.
[0082] Depend on Figure 4 It can be seen that the coercive force (H c ), no correlation was observed with the melting point of the grain boundary material (non-magnetic material of the sputtering target), but when PbO (melting point 886°C) was used as the grain boundary material, the coercivity was as high as 24 kOe, and when Bi 2 O 3 When SnO (melting point 817°C) is used as the grain boundary material, it has a coercive force as high as 26 kOe, and when SnO (melting point 1080°C) is used as the grain boundary material, it has a coercive force as high as about 30 kOe.
[0083] Depend on Figure 5 It can be seen that in the out-of-plane diffraction spectrum of the magnetic recording medium, when SnO (melting point 1080°C) is used as the grain boundary material, the FePt (001) diffraction peak is higher than that of other grain boundary materials C (melting point 3500°C), B 2 O 3 (melting point 450°C), TiO 2 In addition, it was further clarified that the overall noise in the in-plane diffraction spectrum of the magnetic recording medium was reduced, and when SnO (melting point 1080°C) was used as the grain boundary material, the FePt (110) diffraction peak was stronger than other grain boundary materials C (melting point 3500°C), B 2 O 3 (melting point 450°C), TiO 2 (melting point 1857°C). Therefore, it can be confirmed that when SnO is used, the plane perpendicular direction becomes the easy axis direction.
[0084] Depend on Figure 6 It is found that the order degree of the magnetic recording medium is weakly correlated with the melting point of the grain boundary material (non-magnetic material of the sputtering target). When SnO (melting point 1080° C.) is used as the grain boundary material, the order degree is about 1.0, indicating a high order degree.
[0085] Depend on Figure 7 It is found that the crystal grain size of the magnetic recording medium is weakly correlated with the melting point of the grain boundary material (non-magnetic material of the sputtering target), and when SnO (melting point 1080° C.) is used as the grain boundary material, a large crystal grain size of about 8 nm is exhibited.
[0086] Depend on Figure 8 It can be seen that the order degree of the magnetic recording medium shows a good correlation with the crystal grain size, and the larger the crystal grain size, the higher the order degree.
[0087] Depend on Fig. 9 It can be seen that the coercive force (H c ) shows a good correlation with the crystal grain size, and the larger the crystal grain size, the higher the coercive force.
[0088] Depend on Fig.10 It can be seen that the coercive force (H c ) shows a good correlation with the degree of order, and the higher the degree of order, the higher the coercivity.
[0089] From the above results, it can be seen that it can meet the requirements of good hysteresis, high coercivity, high magnetocrystalline anisotropy (Ku grain ), high saturation magnetization (M s grain), the easy axis direction is perpendicular to the plane, the order is high, and the grain boundary material with all the conditions of columnar growth of good grains is an oxide with a melting point of 800°C or more and 1100°C or less, represented by SnO. In this embodiment, only SnO, PbO or Bi as an oxide with a melting point of 800°C or more and 1100°C or less is shown. 2 O 3 As an example of a grain boundary material, it is considered that the same effect will be exhibited when an oxide having a melting point in the same range is used as the grain boundary material.
[0090] [Example 2]
[0091] Then, the 50Fe-50Pt alloy atomized powder was changed to the 47.5Fe-47.5Pt-5Y alloy atomized powder (Y is Au, Ag or Cu) containing 5 atomic % of Au, Ag or Cu respectively as shown in Table 3. The sintering temperature was 960°C, the sintering pressure was 24.5 MPa, the sintering time was 60 minutes, the atmosphere was 5×10 -2 The hot pressing was performed under vacuum conditions of less than 1.5 Pa to produce a FePtY-30 volume % SnO target (Y is Au, Ag or Cu) with a stepped shape of (upper section) diameter 153.0×1.0 mm + (lower section) diameter 161.0×4.0 mm and a heat-assisted FePt granular magnetic recording medium, and the magnetic properties (magnetocrystalline anisotropy and saturation magnetization) were measured. The measurement results are shown in Table 3.
[0092] [Table 3]
[0093] Table 3 Measurement results
[0094]
[0095] By adding Au, Ag or Cu, there is a saturation magnetization (M s grain ) decreases, magnetocrystalline anisotropy (K u grain ) increases, coercivity (H c) increases, but the variation range is small, and it can be confirmed that even if a FePt alloy sputtering target containing Au, Ag or Cu is used as a thermally assisted magnetic recording medium, it also shows the same magnetic properties as when a 50Fe-50Pt alloy sputtering target is used. On the other hand, as a sputtering target, the relative density of (50Fe50Pt)-30 volume % SnO is 96.5%, the relative density of (47.5Fe47.5Pt5Au)-30 volume % SnO is 98.2%, the relative density of (47.5Fe47.5Pt5Ag)-30 volume % SnO is 97.8%, and the relative density of (47.5Fe47.5Pt5Cu)-30 volume % SnO is 97.3%. It can be confirmed that a FePt alloy sputtering target containing Au, Ag or Cu can increase the relative density.
[0096] [Example 3]
[0097] Then, the sintering temperature was 960°C, the sintering pressure was 24.5 MPa, the sintering time was 60 minutes, the atmosphere was 5×10 -2 The FePt-SnO target and the heat-assisted FePt granular magnetic recording medium with a step shape of (upper section) diameter 153.0×1.0mm + (lower section) diameter 161.0×4.0mm were produced by hot pressing under vacuum conditions below 1000 Pa, and the magnetic properties (magnetic anisotropy and saturation magnetization) of the heat-assisted FePt granular magnetic recording medium were measured. The measurement results are shown in Table 4. u grain ), saturation magnetization (M s grain ), Coercivity (H c The results obtained by plotting the relationship between Fig.11 , 12 and 13.
[0098] [Table 4]
[0099] Table 4 Measurement results
[0100]
[0101] Depend on Fig.11 and 12 It can be seen that when the content of non-magnetic material SnO is 25 volume %, the saturation magnetization (M s grain ) and magnetocrystalline anisotropy (K u grain) is the largest, and decreases with the increase of content when it is above 25 volume %, and is 950emu / cm when the content of non-magnetic material SnO is above 20 volume % and below 45 volume %. 3 Above, especially when it is 20 volume % or more and 40 volume % or less, it can show more than 980emu / cm 3 The high saturation magnetization (M s grain ), and when the content of the non-magnetic material SnO is 20 volume % or more and 45 volume % or less, 2.5×10 7 erg / cm 3 Above, especially when it is 25 volume % or more and 45 volume % or less, it can show more than 2.6×10 7 erg / cm 3 The high magnetocrystalline anisotropy (K u grain ).
[0102] Depend on Fig.13 It can be seen that the coercive force (Hc) is maximum when the content of the non-magnetic material SnO is 30 volume % and 35 volume %, and when the content of the non-magnetic material SnO is 25 volume % or more and 40 volume %, a high coercive force exceeding 25 kOe can be exhibited.
[0103] From the above, it can be confirmed that when the content of the non-magnetic material SnO is 25 volume % or more and 40 volume % or less, the saturation magnetization (M s grain ), magnetocrystalline anisotropy (K u grain ) and coercive force (Hc) are improved.
[0104] It is believed that the heat-assisted magnetic recording medium having the above magnetic characteristics and structure has a high saturation magnetization (M s grain ) and thus improve the signal of the heat-assisted magnetic recording medium and the SNR (signal-to-noise ratio). In addition, it is believed that the high uniaxial magnetic anisotropy increases the magnetic energy of the heat-assisted magnetic recording medium and improves the thermal stability.
Claims
1. A sputtering target for a thermally assisted magnetic recording medium, comprising a FePt alloy, a non-magnetic material and inevitable impurities, characterized in that: The non-magnetic material is contained in an amount of 25% by volume or more and 40% by volume or less relative to the sputtering target for the thermally assisted magnetic recording medium, The non-magnetic material is an oxide having a melting point of 800° C. or higher and 1100° C. or lower, and the non-magnetic material is one or more oxides selected from SnO and Bi 2 O 3 .
2. The sputtering target for a thermally assisted magnetic recording medium according to claim 1, wherein: It also contains one or more elements selected from Ag, Au, and Cu.
Citation Information
Patent Citations
Herbicidal composition and manufacturing method thereof
JP1984046922B2
Sputtering target for magnetic recording media
WO2018083951A1
Magnetic recording media and sputter targets with compositions of high anisotropy alloys and oxide compounds
CN101136213A
NON-MAGNETIC MATERIAL-DISPERSED Fe-Pt SPUTTERING TARGET
CN108138313A