A method for isothermal normalizing preparatory heat treatment of 20CrMnMo forgings

By adopting the isothermal normalizing preparatory heat treatment method of multiple air cooling and heat preservation in the heat treatment of 20CrMnMo forgings, the conventional trolley furnace is used to achieve efficient heat treatment of the forgings, which solves the problems of high cost and difficult parameter control of the isothermal normalizing production line and meets the requirements of the forgings. The microstructure and hardness requirements reduce production costs and floor space.

CN114606369BActive Publication Date: 2024-10-29CHONGQING CHANGZHENG HEAVY IND
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210239156.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-11
Publication Date
2024-10-29
Estimated Expiration
2042-03-11

AI Technical Summary

Technical Problem

The existing medium-temperature normalizing production line for heat treatment of 20CrMnMo forgings is expensive and covers a large area. The process parameters are difficult to control, resulting in poor preparatory heat treatment effects and failure to meet the technical requirements of metallographic structure and hardness.

Method used

An isothermal normalizing preparatory heat treatment method is adopted, which includes parts entering the furnace for heating, insulation, multiple air cooling, and re-entering the furnace for insulation. By adjusting the heating speed, holding time and cooling temperature, a conventional trolley furnace is used for heat treatment to avoid isothermal normalizing. Use of production lines.

Benefits of technology

It achieves heat treatment in which the microstructure and hardness of 20CrMnMo forgings meet the requirements, saving production costs, reducing floor space, and simplifying the control of process parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114606369B_ABST
    Figure CN114606369B_ABST
Patent Text Reader

Abstract

The invention discloses a 20CrMnMo forging isothermal normalizing preparatory heat treatment method, comprising the following steps: S1: putting a part into a furnace, heating it first and then keeping it warm, and closing the heating system in the furnace after the keeping warm is finished; S2: removing the part from the furnace and air-cooling it to #imgabs0#, and then returning the part to the furnace to be placed for a period of time; S3: repeating the operation of S2, so that the total number of operations of S2 is not less than 2 times; S4: removing the part from the furnace and air-cooling it to #imgabs1#, and then putting the part into the furnace and cooling it to #imgabs2# with the furnace; S5: heating the furnace to a first set temperature, and then keeping it warm in the furnace; S6: closing the heating system in the furnace, and after the workpiece is furnace-cooled to a second set temperature, removing the part from the furnace and air-cooling it. By adopting the present invention, the 20CrMnMo forgings are subjected to S1-S6 heat treatment in sequence, so that the 20CrMnMo forgings after the heat treatment meet the required microstructure and hardness requirements. No isothermal normalizing production line is needed, and the heat treatment operation can be performed using a conventional trolley furnace, which saves production costs and facilitates the control of process parameters during the heat treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging heat treatment method, in particular to an isothermal normalizing preparatory heat treatment method for 20CrMnMo forgings. Background Art

[0002] 20CrMnMo forgings are widely used in gear shafts, gears, pins and other parts. They are required to have good comprehensive mechanical properties and organizational stability, so the requirements for their preliminary heat treatment are particularly high. Generally, the actual grain size after preliminary heat treatment is required to be ≥5 (GB / T6394); the metallographic structure level meets 1~2 levels (GB / T13320); the banded structure is ≤2 levels (GB / T13299); the hardness value is 140~200HB (GB / T231.1).

[0003] Existing 20CrMnMo forgings are generally prepared for heat treatment by normalizing + tempering. The obtained structure is generally granular bainite (B) or ferrite (F) + pearlite (P) + granular bainite (B), and the hardness is generally 250-320HB. The structure may even have defects such as mixed crystals and banded structures, resulting in its metallographic structure and hardness not meeting the technical requirements, which seriously affects the subsequent mechanical processing and heat treatment mechanical properties.

[0004] In order to meet the technical requirements, 20CrMnMo forgings generally use isothermal normalizing process for preliminary heat treatment in isothermal normalizing line (equipment), but the isothermal normalizing production line is expensive, occupies a large area, and the process setting parameters are difficult to control. Generally, factories are not equipped with this production line, which brings great difficulties to the preliminary heat treatment of 20CrMnMo forgings. Summary of the invention

[0005] The purpose of the present invention is to provide a 20CrMnMo forging isothermal normalizing preparatory heat treatment method without using an isothermal normalizing production line in view of the high cost of the isothermal normalizing production line during the heat treatment of 20CrMnMo forgings in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A 20CrMnMo forging isothermal normalizing preparatory heat treatment method comprises the following steps:

[0008] S1: The parts are put into the furnace, heated up first and then kept warm. After the warming is over, the heating system in the furnace is turned off.

[0009] S2: Remove the parts from the furnace and air cool them to Finally, return the parts to the furnace and place them for a period of time;

[0010] S3: Repeat the operation of S2 so that the total number of operations of S2 is not less than 2 times;

[0011] S4: Remove the parts from the furnace and air cool them to Then put the parts into the furnace and cool them down.

[0012] S5: The temperature in the furnace is raised to a first set temperature, and then the temperature is kept in the furnace;

[0013] S6: Turn off the heating system in the furnace. After the workpiece is cooled to the second set temperature, remove the part from the furnace and air cool it.

[0014] The present invention adopts the above technical solution, by sequentially performing S1-S6 heat treatment on the 20CrMnMo forgings, so that the 20CrMnMo forgings after heat treatment meet the required microstructure and hardness requirements. There is no need to use an isothermal normalizing production line here, and a conventional trolley furnace can be used for heat treatment operations, which effectively saves production costs, reduces floor space, and facilitates control of process parameters during the heat treatment process.

[0015] Furthermore, in S1, the part is heated to a temperature of ≤200°C / h. Reasonably control the heating rate and select the temperature to which it is heated; 20CrMnMo is carburizing steel, and the general processing flow is: forging → normalizing → machining → carburizing → high temperature tempering → heat treatment → finishing. The carburizing temperature is generally 930°C. In order to completely eliminate material defects before carburizing, the normalizing temperature is generally not lower than the carburizing temperature. However, the higher the temperature, the greater the temperature difference during cooling, and the faster the cooling speed of the parts, which is not good for the material structure. Therefore, the normalizing temperature is selected as 930°C.

[0016] Furthermore, the heating rate of the parts is (150-200)°C / h. Too slow a heating rate will reduce the heat treatment efficiency, while too fast a heating rate will make the workpiece easily deformed.

[0017] Furthermore, the holding time is related to the thickness of the part. The thickness of the part is Amm.

[0018] In S1, the holding time is: ((0~10)+(1.5~2)A)min;

[0019] In S5, the holding time is: ((20~60)+2A)min. Two holding time selection formulas are obtained through experiments. Sufficient holding time makes the internal structure of the part more uniform, which is conducive to obtaining the set internal structure of the part.

[0020] Furthermore, in S2, the placement time of the parts back in the furnace is: (6-8) min. When the parts are back in the furnace, since the parts are in the closed space in the furnace, the core temperature of the parts is higher than the surface temperature, so the surface temperature of the parts will gradually increase, and the temperature difference between the core and the surface of the parts will decrease.

[0021] Further, in S3, the total number of operations of S2 is 2. The total number of operations of S2 can be adjusted accordingly according to the specific conditions of the parts.

[0022] Further, in S5, the first set temperature is The heating rate of the parts is ≤200℃ / h. The tempering temperature will affect the hardness of the material, and the hardness directly affects the cutting performance of the parts. For materials such as 20CrMnMo, tempering at 600-650℃ can obtain better cutting hardness; at the same time, keeping this temperature for a period of time can make the austenite structure evenly transformed into ferrite and pearlite structure, so as to obtain good cutting performance and mechanical properties.

[0023] Further, in S6, the second set temperature is ≤500° C. Influenced by the alloy elements of the 20CrMnMo material, the furnace is cooled to 500° C. to avoid the formation of bainite.

[0024] Furthermore, the parts are placed in the trolley furnace through shims, the height of the shims is not less than 100mm, and the distance between the parts is not less than 30mm. Placing the parts in the trolley furnace through shims can prevent the parts from directly contacting the trolley furnace and local overheating of the parts; maintaining an appropriate distance between the parts facilitates uniform heating of the parts.

[0025] Furthermore, the parts are loaded in the trolley furnace, and the furnace fan is turned on when the furnace is heated. The fan makes the temperature in the furnace uniform and reduces the temperature unevenness.

[0026] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0027] By sequentially performing S1-S6 heat treatment on the 20CrMnMo forgings, the 20CrMnMo forgings after heat treatment meet the required microstructure and hardness requirements. No isothermal normalizing production line is required here, and a conventional trolley furnace can be used for heat treatment operations, which effectively saves production costs, reduces floor space, and facilitates control of process parameters during the heat treatment process. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings in the specification, which constitute a part of this application, are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0029] In the attached picture:

[0030] Figure 1 A schematic diagram showing an embodiment of the isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings of the present invention. DETAILED DESCRIPTION

[0031] It should be noted that, unless otherwise specified, all technical and scientific terms used in this application have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs.

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] A 20CrMnMo forging isothermal normalizing preparatory heat treatment method comprises the following steps:

[0034] S1: The parts are put into the furnace, heated up first and then kept warm. After the warming is finished, the heating system in the furnace is turned off.

[0035] S2: Remove the parts from the furnace and air cool them to Finally, return the parts to the furnace and place them for a period of time;

[0036] S3: Repeat the operation of S2 so that the total number of operations of S2 is not less than 2 times;

[0037] S4: Remove the parts from the furnace and air cool them to Then put the parts into the furnace and cool them down.

[0038] S5: The temperature in the furnace is raised to a first set temperature, and then the temperature is kept in the furnace;

[0039] S6: Turn off the heating system in the furnace. After the workpiece is cooled to the second set temperature, remove the part from the furnace and air cool it.

[0040] The present invention adopts the above technical solution, by sequentially performing S1-S6 heat treatment on the 20CrMnMo forgings, so that the 20CrMnMo forgings after heat treatment meet the required microstructure and hardness requirements. There is no need to use an isothermal normalizing production line here, and a conventional trolley furnace can be used for heat treatment operations, which effectively saves production costs, reduces floor space, and facilitates control of process parameters during the heat treatment process.

[0041] Preferably, in S1, the part is heated to a temperature of ≤200°C / h. Reasonably control the heating rate and select the temperature to which it is heated; 20CrMnMo is carburizing steel, and the general processing flow is: forging → normalizing → machining → carburizing → high temperature tempering → heat treatment → finishing. The carburizing temperature is generally 930°C. In order to completely eliminate material defects before carburizing, the normalizing temperature is generally not lower than the carburizing temperature. However, the higher the temperature, the greater the temperature difference during cooling, and the faster the cooling speed of the parts, which is not good for the material structure. Therefore, the normalizing temperature is selected as 930°C.

[0042] Preferably, the heating rate of the part is (150-200)°C / h. A heating rate that is too slow will reduce the heat treatment efficiency, while a heating rate that is too fast will make the workpiece easily deformed.

[0043] Preferably, the holding time is related to the thickness of the part, and the thickness of the part is Amm.

[0044] In S1, the holding time is: ((0~10)+(1.5~2)A)min;

[0045] In S5, the holding time is: ((20~60)+2A)min. Two holding time selection formulas are obtained through experiments. Sufficient holding time makes the internal structure of the part more uniform, which is conducive to obtaining the set internal structure of the part.

[0046] Preferably, in S2, the placement time of the parts in the furnace is (6-8) min. When the parts are in the closed space in the furnace, the core temperature of the parts is higher than the surface temperature, so the surface temperature of the parts will gradually increase, and the temperature difference between the core and the surface of the parts will decrease.

[0047] Preferably, in S3, the total number of operations of S2 is 2. The total number of operations of S2 can be adjusted accordingly according to the specific conditions of the parts.

[0048] Preferably, in S5, the first set temperature is The heating rate of the parts is ≤200℃ / h. The tempering temperature will affect the hardness of the material, and the hardness directly affects the cutting performance of the parts. For materials such as 20CrMnMo, tempering at 600-650℃ can obtain better cutting hardness; at the same time, keeping this temperature for a period of time can make the austenite structure evenly transformed into ferrite and pearlite structure, so as to obtain good cutting performance and mechanical properties.

[0049] Preferably, in S6, the second set temperature is ≤500° C. Influenced by the alloy elements of the 20CrMnMo material, the furnace is cooled to 500° C. to avoid the formation of bainite.

[0050] Preferably, the parts are placed in the trolley furnace through shims, the height of the shims is not less than 100mm, and the distance between the parts is not less than 30mm. Placing the parts in the trolley furnace through shims can prevent the parts from directly contacting the trolley furnace and local overheating of the parts; maintaining an appropriate distance between the parts facilitates uniform heating of the parts.

[0051] Preferably, the parts are placed in a trolley furnace, and the furnace fan is turned on when the furnace is heated. The fan makes the temperature in the furnace uniform and reduces temperature unevenness.

[0052] In S2, the air cooling temperature out of the furnace is selected as It is formulated according to the cooling curve of 20CrMnMo material. If the cooling temperature is higher than The cooling speed in the two-phase zone is relatively slow, which is not conducive to cutting off tissue inheritance. It is easy to generate bainite structure. Cooling is to obtain better organization. After keeping warm, cool to the "S" nose temperature, which is the temperature at which austenite transforms into ferrite and pearlite, generally 500℃-650℃, and keep this temperature for a period of time to make the austenite organization evenly transform into ferrite and pearlite organization, and then cool to room temperature to obtain good cutting performance and mechanical properties.

[0053] like Figure 1 In one embodiment of the present invention, in S2-S3, the parts are first taken out of the furnace for air cooling, and then returned to the furnace for equalization of temperature. The number of times of taking out of the furnace is 3 times, and after the last time of taking out of the furnace, the parts are returned to the furnace for cooling to Then proceed with the subsequent operations.

[0054] The scope of the present invention is not limited by the above-described embodiments but by the appended claims and their equivalents.

[0055] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for isothermal normalizing preparatory heat treatment of 20CrMnMo forgings, characterized in that: The following steps are involved: S1: The parts are put into the furnace, heated up first and then kept warm. After the warming is over, the heating system in the furnace is turned off. S2: Remove the parts from the furnace and air cool them to ℃, then return the parts to the furnace and place them for 6~8min; S3: Repeat the operation of S2, so that the total number of operations of S2 is 2 times; S4: Remove the parts from the furnace and air cool them to ℃, and then put the parts into the furnace and cool them to ℃; S5: The temperature in the furnace is raised to a first set temperature, and then the temperature is kept in the furnace. The first set temperature is ℃, the heating rate of parts is ≤200℃ / h; S6: Turn off the heating system in the furnace, and after the workpiece is cooled to the second set temperature, remove the part from the furnace and air cool it; the second set temperature is ≤500℃.

2. The isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings according to claim 1, characterized in that: In S1, the parts are heated to a temperature of ≤200℃ / h. ℃.

3. The isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings according to claim 2, characterized in that: The heating rate of the parts is (150~200)℃ / h.

4. The isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings according to claim 1, characterized in that: The holding time is related to the thickness of the part. The thickness of the part is Amm. In S1, the holding time is: ((0~10)+(1.5~2)A)min; In S5, the holding time is: ((20~60)+2A)min.

5. The isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings according to claim 1, characterized in that: The parts are placed in the trolley furnace through shims. The height of the shims shall not be less than 100mm and the spacing between parts shall not be less than 30mm.

6. The isothermal normalizing preliminary heat treatment method for 20CrMnMo forgings according to claim 1, characterized in that: The parts are placed in a trolley furnace and the furnace fan is turned on when the furnace is heated.

Citation Information

Patent Citations

  • Isothermal normalizing method for alloy carburizing steel gear and forging shaft for wind power generator