Method for producing n-type single crystal silicon, n-type single crystal silicon ingot, silicon wafer and epitaxial silicon wafer

By using high-concentration red phosphorus or arsenic dopants under the control of the inner diameter of the quartz crucible and the magnetic field, the problem of dopant evaporation and dislocation during the pulling process of single crystal silicon was solved, and a diameter of more than 200 mm was achieved. Low resistivity silicon wafer production improves yield and quality.

CN114606567BActive Publication Date: 2024-10-01SUMCO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210251415.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-04-25
Filing Date
2018-03-20
Publication Date
2024-10-01
Estimated Expiration
2038-03-20

AI Technical Summary

Technical Problem

In the existing technology, n-type single crystal silicon with low resistivity is easily reduced in yield due to the evaporation of volatile dopants during the pulling process, and is accompanied by dislocations, and it is difficult to achieve low resistivity with a diameter of more than 200 mm using the existing technology. Resistivity silicon wafer.

Method used

By setting the inner diameter of the quartz crucible to not less than 1.7 times and not more than 2.3 times the diameter of single crystal silicon, and using high-concentration red phosphorus or arsenic as a dopant, the furnace pressure and magnetic field strength of the silicon melt are controlled to suppress the evaporation of the dopant. and segregation to achieve low resistivity single crystal silicon growth.

Benefits of technology

It effectively suppresses the decrease in yield and dislocation of single crystal silicon, enables the production of low-resistivity silicon wafers and epitaxial silicon wafers with a diameter of more than 200mm, and improves the quality and yield of single crystal silicon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114606567B_ABST
    Figure CN114606567B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing n-type single crystal silicon, an ingot of n-type single crystal silicon, a silicon wafer and an epitaxial silicon wafer. The present invention provides a method for manufacturing n-type single crystal silicon, wherein single crystal silicon (10) is pulled and grown from a silicon melt (9) containing red phosphorus as a main dopant by a pulling method, wherein a quartz crucible (3A) having an inner diameter of 1.7 times or more and 2.3 times or less of a straight body diameter of the single crystal silicon (10) is used to pull single crystal silicon (10) having a resistivity of 0.5 mΩcm or more and 1.0 mΩcm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of March 20, 2018, an application number of "201880027573.X", and an invention name of "Method for manufacturing n-type single crystal silicon, n-type single crystal silicon ingot, silicon wafer and epitaxial silicon wafer". Technical Field

[0002] The present invention relates to a method for manufacturing n-type single crystal silicon, an n-type single crystal silicon ingot, a silicon wafer and an epitaxial silicon wafer. Background Art

[0003] In recent years, mobile devices such as mobile phones have become widely used. There is a strong demand for such mobile devices to be able to be carried and used for a long time, and research has been conducted to increase the capacity of batteries built into the mobile devices or to reduce the power consumption of the mobile devices themselves.

[0004] In order to reduce the power consumption of the mobile device itself, it is necessary to reduce the power consumption of the semiconductor device mounted inside the mobile device.

[0005] For example, a low-voltage power MOSFET (Metal Oxide Semi-Conductor Field Effect Transistor) used as a power device for mobile devices has a certain constant resistance inside when it is energized, and therefore consumes power according to the current flowing through the low-voltage power MOSFET.

[0006] Therefore, if the internal resistance of the low-voltage power MOSFET can be reduced when it is in the on state, the power consumption of the mobile device can be reduced. Based on this background, in order to reduce the resistance of the low-voltage power MOSFET when it is in the on state, low-resistivity n-type single crystal silicon is strongly required.

[0007] However, in the past, in the method of manufacturing single crystal silicon by the pulling method, the following technology is disclosed in Patent Document 1: the inner diameter of the quartz crucible is preferably set to be more than 3 times the diameter (straight body diameter) of the single crystal silicon, thereby enabling stable pulling of single crystal silicon even when pulling large-diameter single crystal silicon.

[0008] Furthermore, examples of dopants capable of reducing the resistivity of a silicon wafer include red phosphorus and arsenic. Patent Document 2 proposes a technique for reducing the resistivity by using red phosphorus as a dopant.

[0009] Furthermore, Patent Document 3 proposes a technique for lowering the resistivity by using arsenic as a dopant.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2009-292684

[0013] Patent Document 2: Japanese Patent No. 5890587

[0014] Patent Document 3: Japanese Patent Application Publication No. 2011-44505 Summary of the invention

[0015] Technical problem to be solved by the invention

[0016] However, if the technology described in Patent Document 1 is to be used for pulling low-resistivity n-type single crystal silicon, the following technical problems exist: n-type dopants such as red phosphorus and arsenic, which are volatile dopants, may evaporate during pulling, thereby reducing the yield of single crystal silicon in the desired low resistivity range, or dislocation of the single crystal silicon may occur as the amount of n-type dopant added increases.

[0017] Furthermore, in the technology described in Patent Document 2, red phosphorus can be used as a dopant to produce a silicon wafer with a low resistivity, but the diameter of the silicon wafer disclosed in the examples is only 200 mm.

[0018] Furthermore, in the technology described in Patent Document 3, arsenic can be used as a dopant to produce a silicon wafer with a low resistivity, but the diameter of the silicon wafer disclosed in the examples is only 150 mm.

[0019] An object of the present invention is to provide a method for manufacturing n-type single crystal silicon, an n-type single crystal silicon ingot, a silicon wafer having a diameter of 200 mm or more, and an epitaxial silicon wafer capable of suppressing a decrease in the yield of single crystal silicon and suppressing the occurrence of dislocation.

[0020] Solutions for solving technical problems

[0021] The method for manufacturing n-type single crystal silicon of the present invention pulls and grows single crystal silicon from a silicon melt containing red phosphorus as a main dopant by a pulling method. The method for manufacturing n-type single crystal silicon is characterized in that a quartz crucible having an inner diameter that is not less than 1.7 times and not more than 2.3 times the straight body diameter of the single crystal silicon is used to pull single crystal silicon in which the resistivity of a portion of the single crystal silicon is not less than 0.5 mΩcm and not more than 1.0 mΩcm.

[0022] Here, the straight body diameter refers to the diameter of a portion of the pulled silicon single crystal, in which the diameter is controlled to be substantially constant and from which the silicon wafer is cut.

[0023] According to the present invention, a quartz crucible having an inner diameter of not less than 1.7 times and not more than 2.3 times the straight body diameter of single crystal silicon is used. This can reduce the area of ​​the free surface of the melt in the quartz crucible, thereby suppressing the evaporation of red phosphorus as a dopant in the melt, and will not reduce the yield of the low resistivity portion of the single crystal silicon.

[0024] Furthermore, by suppressing the evaporation of red phosphorus, it is not necessary to add a large amount of red phosphorus from the beginning of pulling, so that the occurrence of dislocations in the silicon single crystal can be suppressed.

[0025] That is, according to the present invention, dislocation is prevented by the high concentration of red phosphorus at the beginning of pulling of single crystal silicon, and the evaporation of red phosphorus in the melt is suppressed. As the pulling proceeds, the concentration of red phosphorus in the melt increases, and a single crystal with low resistivity can be obtained.

[0026] In the present invention, preferably, the straight diameter of the silicon single crystal is 201 mm or more and 230 mm or less, and the inner diameter of the quartz crucible is 2.1 times or more and 2.3 times or less the straight diameter of the silicon single crystal.

[0027] When the straight body diameter of the silicon single crystal is 201 mm or more and 230 mm or less, evaporation of red phosphorus is suppressed. Therefore, if the inner diameter of the quartz crucible is within this range, the above-mentioned action and effect can be achieved.

[0028] In the present invention, it is preferred that the resistivity of the portion of the single crystal silicon is 0.5 mΩcm or more and 0.7 mΩcm or less.

[0029] Even in the case of such a resistivity range, by setting the diameter of the quartz crucible to 2.1 times or more and 2.3 times or less the straight body diameter of the silicon single crystal, the silicon single crystal can be pulled up without dislocation.

[0030] In the present invention, preferably, the straight diameter of the silicon single crystal is 301 mm or more and 330 mm or less, and the inner diameter of the quartz crucible is 1.7 times or more and 2.0 times or less the straight diameter of the silicon single crystal.

[0031] When the straight body diameter of the silicon single crystal is 301 mm or more and 330 mm or less, evaporation of red phosphorus is suppressed. Therefore, if the inner diameter of the quartz crucible is within this range, the above-mentioned action and effect can be achieved.

[0032] In the present invention, it is preferred that the resistivity of the portion of the single crystal silicon is 0.8 mΩcm or more and 1.0 mΩcm or less.

[0033] Even in the case of such a resistivity range, by setting the diameter of the quartz crucible to 1.7 times or more and 2.0 times or less the straight body diameter of the silicon single crystal, the silicon single crystal can be pulled up without dislocation.

[0034] The method for manufacturing n-type single crystal silicon of the present invention pulls and grows single crystal silicon from a silicon melt containing arsenic as a main dopant by a pulling method. The method for manufacturing n-type single crystal silicon is characterized in that a quartz crucible having an inner diameter that is not less than 1.7 times and not more than 2.0 times the straight body diameter of the single crystal silicon is used to pull single crystal silicon having a straight body diameter of not less than 301 mm and not more than 330 mm and a resistivity of a portion of the single crystal silicon of not less than 1.7 mΩcm and not more than 2.0 mΩcm.

[0035] According to the present invention, the same actions and effects as those described above can be enjoyed.

[0036] That is, according to the present invention, dislocation is prevented by high arsenic concentration at the beginning of pulling of single crystal silicon, while evaporation of arsenic in the melt is suppressed, so that the arsenic concentration in the melt increases as pulling proceeds, and a single crystal with low resistivity can be obtained.

[0037] In the present invention, it is preferred that the pressure in the furnace of the pulling device for pulling the single crystal silicon be set to 40 kPa or more and 80 kPa or less to pull the single crystal silicon.

[0038] According to the present invention, the pressure in the pulling device is set to 40 kPa or more, thereby suppressing the evaporation of red phosphorus or arsenic. On the other hand, the pressure in the furnace is set to 80 kPa or less, thereby preventing the dopant in the silicon melt from being concentrated due to segregation and causing dislocation.

[0039] In the present invention, it is preferred that a magnetic field having a magnetic field intensity of 0.2 T to 0.4 T be applied to the silicon melt in the quartz crucible to perform pulling.

[0040] According to the present invention, by applying a magnetic field having a magnetic field strength of 0.2 T to 0.4 T, in-plane fluctuation of single crystal silicon during pulling can be prevented, so that single crystal silicon can be pulled reliably without causing dislocation.

[0041] The n-type single crystal silicon ingot of the present invention is an n-type single crystal silicon ingot having a straight body diameter of greater than 301 mm and less than 330 mm, characterized in that the n-type single crystal silicon ingot contains red phosphorus as a dopant, and the resistivity of a part of the single crystal silicon is greater than 0.8 mΩcm and less than 1.0 mΩcm.

[0042] The silicon wafer of the present invention is a silicon wafer having a diameter of 300 mm, which is cut out from the above-mentioned n-type single crystal silicon ingot, and has a resistivity of 0.8 mΩcm or more and 1.0 mΩcm or less.

[0043] The epitaxial silicon wafer of the present invention is characterized in that an epitaxial film is formed on the surface of the silicon wafer.

[0044] According to these inventions, it is possible to obtain a single crystal silicon ingot, a low-resistivity silicon wafer, and a low-resistivity epitaxial silicon wafer having an unprecedented large diameter of 300 mm and low resistivity using red phosphorus as a dopant.

[0045] The n-type single crystal silicon ingot of the present invention is an n-type single crystal silicon ingot having a straight body diameter of 301 mm or more and 330 mm or less, characterized in that the n-type single crystal silicon ingot contains arsenic as a dopant, and a resistivity of a part of the single crystal silicon is 1.7 mΩcm or more and 2.0 mΩcm or less.

[0046] The silicon wafer of the present invention is a silicon wafer having a diameter of 300 mm, characterized in that the silicon wafer is cut out from the above-mentioned n-type single crystal silicon ingot and has a resistivity of 1.7 mΩcm or more and 2.0 mΩcm or less.

[0047] The epitaxial silicon wafer of the present invention is characterized in that an epitaxial growth film is formed on the surface of the silicon wafer.

[0048] According to these inventions, it is possible to obtain a single crystal silicon ingot, a low-resistivity silicon wafer, and a low-resistivity epitaxial silicon wafer having an unprecedented large diameter of 300 mm and low resistivity using arsenic as a dopant. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 It is a schematic diagram showing an example of the structure of a single crystal silicon pulling apparatus according to an embodiment of the present invention.

[0050] Figure 2 This is a graph showing the relationship between the straight body length and the resistivity of single crystal silicon (straight body diameter 201 to 230 mm) when red phosphorus is used as a dopant in Examples.

[0051] Figure 3 This is a graph showing the relationship between the straight body length and the resistivity of single crystal silicon (straight body diameter 201 to 230 mm) when red phosphorus is used as a dopant in Examples.

[0052] Figure 4 This is a graph showing the relationship between the straight body length and the resistivity of single crystal silicon (straight body diameter 301 to 330 mm) when red phosphorus is used as a dopant in Examples.

[0053] Figure 5 This is a graph showing the relationship between the straight body length and the resistivity of single crystal silicon (straight body diameter 301 to 330 mm) when arsenic is used as a dopant in Examples. DETAILED DESCRIPTION

[0054] [1] Structure of Single Crystal Silicon Pulling Apparatus 1

[0055] Figure 11 is a schematic diagram showing an example of the structure of a pulling device 1 for pulling a single crystal silicon to which the method for producing a single crystal silicon according to an embodiment of the present invention can be applied. The pulling device 1 is a device for pulling a single crystal silicon 10 by a Czochralski method, and includes a chamber 2 constituting an outer periphery and a crucible 3 arranged in the center of the chamber 2.

[0056] The crucible 3 has a double structure consisting of an inner quartz crucible 3A and an outer graphite crucible 3B, and is fixed to the upper end of a rotatable and elevatable support shaft 4 .

[0057] The inner diameter of the quartz crucible 3A inside the crucible 3 is 1.7 times or more and 2.3 times or less the straight body diameter when the silicon single crystal 10 is pulled.

[0058] Specifically, when the straight body diameter of the silicon single crystal 10 is greater than or equal to 201 mm and less than or equal to 230 mm, the inner diameter of the quartz crucible 3A is preferably greater than or equal to 2.1 times and less than or equal to 2.3 times the straight body diameter of the silicon single crystal 10. On the other hand, when the straight body diameter of the silicon single crystal 10 is greater than or equal to 301 mm and less than or equal to 330 mm, the inner diameter of the quartz crucible 3A is preferably greater than or equal to 1.7 times and less than or equal to 2.0 times the straight body diameter of the silicon single crystal 10.

[0059] If the inner diameter of the crucible 3 is larger than the above, the opening diameter of the heat shielding plate 12 or the chamber 2 becomes larger, so that dopant vapor deposits adhere to the furnace body and foreign matter adheres to the silicon single crystal 10, making it easy to cause dislocation.

[0060] By setting the inner diameter of crucible 3 within such a range, the gap between single crystal silicon 10 and quartz crucible 3A can be reduced, thereby suppressing the evaporation of dopants such as red phosphorus and arsenic, and preventing dislocations at the beginning of the body portion caused by segregation of dopants.

[0061] A resistance heating heater 5 is provided outside the crucible 3 to surround the crucible 3, and a heat insulating material 6 is provided outside the crucible 3 along the inner surface of the chamber 2. The heater 5 is not limited to a single heater, but may be divided into upper and lower parts, and each heater can independently set the temperature.

[0062] A wire pulling shaft 7 is provided above the crucible 3 and rotates coaxially with the support shaft 4 in the opposite direction or in the same direction at a predetermined speed. A seed crystal 8 is attached to the lower end of the pulling shaft 7 .

[0063] Furthermore, a cylindrical water-cooling body may be provided in the chamber 2 so as to surround the silicon single crystal 10 being grown on the silicon melt 9 .

[0064] The water cooler is made of a metal with good thermal conductivity such as copper, and is forcibly cooled by cooling water flowing inside. The water cooler promotes cooling of the growing silicon single crystal 10 and controls the temperature gradient in the pulling axis direction of the center and the periphery of the single crystal.

[0065] A cylindrical heat shielding plate 12 is disposed in the chamber 2 .

[0066] The heat shielding plate 12 has the following functions: it blocks the high-temperature radiant heat from the silicon melt 9 in the crucible 3, the heater 5, or the side wall of the crucible 3 for the single crystal silicon 10 being grown, and suppresses the heat diffusion to the outside near the solid-liquid interface which is the crystal growth interface, and controls the temperature gradient in the direction of the pulling axis at the center and the periphery of the single crystal.

[0067] A gas inlet 13 for introducing an inert gas such as Ar gas into the chamber 2 is provided at the upper portion of the chamber 2. An exhaust port 14 for sucking and exhausting the gas in the chamber 2 by driving a vacuum pump (not shown) is provided at the lower portion of the chamber 2.

[0068] The inert gas introduced into the chamber 2 from the gas inlet port 13 descends between the growing single crystal silicon 10 and the heat shielding plate 12, passes through the gap (liquid level Gap) between the lower end of the heat shielding plate 12 and the liquid level of the silicon melt 9, flows to the outside of the heat shielding plate 12, and then flows to the outside of the crucible 3, then descends outside the crucible 3 and is discharged from the exhaust port 14.

[0069] When such a growth device is used to grow a silicon single crystal 10, the solid raw material such as polycrystalline silicon filled in the crucible 3 is melted by heating by the heater 5 while the inside of the chamber 2 is maintained in an inert gas environment under reduced pressure, thereby forming a silicon melt 9. When the silicon melt 9 is formed in the crucible 3, the pulling shaft 7 is lowered to immerse the seed crystal 8 in the silicon melt 9, and the crucible 3 and the pulling shaft 7 are rotated in a predetermined direction, while the pulling shaft 7 is slowly pulled up, thereby growing a silicon single crystal 10 connected to the seed crystal 8.

[0070] [2] Method for producing single crystal silicon

[0071] When the single crystal silicon 10 as the n-type single crystal silicon of the present embodiment is manufactured by using the above-mentioned pulling apparatus 1, red phosphorus or arsenic can be added as a main dopant in the silicon melt 9 at the beginning of pulling or appropriately added during pulling. When red phosphorus or arsenic is used as the main dopant, 50% by mass or more of the n-type dopant is red phosphorus or arsenic, and other dopants may be added.

[0072] When pulling an ingot of a single crystal silicon 10 having a straight body diameter of not less than 201 mm and not more than 230 mm, when red phosphorus is used as a dopant, the resistivity is controlled to be not less than 0.8 mΩcm and not more than 1.05 mΩcm at the starting position of the straight body of the single crystal silicon 10. Thereafter, as the single crystal silicon 10 is pulled and grown, the resistivity of the single crystal silicon 10 gradually decreases, and finally a single crystal silicon 10 having a diameter of not less than 0.5 mΩcm and not more than 0.7 mΩcm is obtained.

[0073] During the pulling of an ingot of a single crystal silicon 10 having a straight body diameter of not less than 301 mm and not more than 330 mm, when red phosphorus is used as a dopant, the resistivity is controlled to be not less than 1.2 mΩcm and not more than 1.7 mΩcm at the starting position of the straight body portion of the single crystal silicon 10. Thereafter, as the single crystal silicon 10 is pulled and grown, the resistivity of the single crystal silicon 10 is gradually decreased, and finally a portion of the ingot having a single crystal silicon 10 of not less than 0.8 mΩcm and not more than 1.0 mΩcm is obtained.

[0074] When pulling an ingot of a single crystal silicon 10 having a straight body diameter of not less than 301 mm and not more than 330 mm, when arsenic is used as a dopant, the resistivity is controlled to be not less than 2.5 mΩcm and not more than 3.1 mΩcm at the starting position of the straight body portion of the single crystal silicon 10. Thereafter, as the single crystal silicon 10 is pulled and grown, the resistivity of the single crystal silicon 10 is gradually decreased, and finally a portion of the ingot having a single crystal silicon 10 of not less than 1.7 mΩcm and not more than 2.0 mΩcm is obtained.

[0075] The ingot of the silicon single crystal 10 of the present embodiment can be pulled according to the general pulling conditions. At this time, as a method for increasing the concentration of dopants such as red phosphorus or arsenic in the silicon melt 9 in the crucible 3, there are the following methods: changing the amount of dopant added during pulling, or utilizing the increase in dopant concentration caused by the segregation phenomenon accompanying pulling, or changing the amount of inert gas introduced into the chamber 2 to suppress the evaporation of the dopant and change the pressure in the chamber 2.

[0076] Specifically, in the first half of pulling the straight body of the silicon single crystal 10, if evaporation of the dopant is to be suppressed and the dopant concentration in the silicon melt 9 in the crucible 3 is to be increased, the Ar flow rate is set to 50 L / min to 150 L / min and the pressure in the furnace is set to 40 kPa to 80 kPa.

[0077] On the other hand, in the second half of pulling the straight body portion of the single crystal silicon 10, in order to promote the evaporation of the dopant and to offset the concentration of the dopant caused by the segregation accompanying the growth of the single crystal silicon 10 and maintain the dopant concentration in the silicon melt 9 in the crucible 3, the Ar flow rate is set to 50 L / min to 200 L / min and the pressure in the furnace is set to 20 kPa to 80 kPa (preferably above 30 kPa and below 40 kPa).

[0078] Furthermore, when pulling the silicon single crystal 10, it is preferred to apply a magnetic field with a magnetic field strength of not less than 0.2 T and not more than 0.4 T. By applying a magnetic field, melt convection of the silicon single crystal 10 being pulled can be suppressed, and temperature unevenness or turbulence in the melt can be reduced, so that the silicon single crystal 10 can be reliably pulled without dislocation.

[0079] When pulling silicon single crystal 10 , when heater 5 uses an upper heater and a lower heater whose temperatures can be independently set, the ratio of the heating amount by the upper heater to the heating amount by the lower heater is preferably set to 1 or more and 4 or less.

[0080] If it is less than 1, that is, the heating amount of the lower heater is less than the heating amount of the upper heater, the downward convection from the bottom of the crucible 3 to the solid-liquid interface will not become stronger, and the unstable convection from the surface of the silicon melt 9 with dopants added to the crystal liquid temperature cannot be weakened, so the occurrence of temperature instability and dislocation cannot be suppressed.

[0081] On the other hand, if the ratio of the heating amount exceeds 4, the heat load on the lower portion of the crucible increases, and there is a possibility that the crucible 3 may be deformed or quartz may peel off.

[0082] When forming the shoulder of the silicon single crystal 10, the silicon single crystal 10 is preferably pulled so as not to generate a high remelting region (for example, 200 μm or more). The remelting region is a region where the silicon single crystal 10 pulled from the silicon melt 9 and solidified melts and liquefies again during the pulling.

[0083] Specifically, when the shoulder is just beginning to be formed, the crucible 3 is pulled while being rotated at a rotation speed of not less than 16 rpm and not more than 30 rpm. Thereafter, when the diameter of the shoulder reaches more than half of the straight body diameter of the single crystal silicon 10, the rotation speed of the crucible 3 is slowly reduced to not less than 4 rpm and not more than 12 rpm.

[0084] When the shoulder portion is just formed, if the pulling is performed at a rotation speed exceeding 30 rpm, the operation of the pulling device 1 becomes unstable, and the possibility of deformation of the shoulder portion increases.

[0085] Next, when the diameter of the shoulder portion reaches or exceeds half of the straight diameter of the silicon single crystal 10, if the rotation speed of the crucible 3 is less than 4 rpm, the silicon melt 9 to which the dopant is added becomes unstable and the possibility of dislocations occurring increases.

[0086] On the other hand, when the rotation speed of crucible 3 exceeds 12 rpm, the oxygen density or resistivity within the plane of silicon single crystal 10 varies greatly, and the crystal quality becomes unstable.

[0087] When forming the straight body of the silicon single crystal 10, it is preferred to perform pulling so as not to generate a high remelting region (e.g., 200 μm or more). Specifically, when the straight body is just beginning to be formed, the crucible 3 is rotated at a rotation speed of 9 rpm or more and 30 rpm or less while performing pulling, and when the straight body of the silicon single crystal 10 of 50 mm or more and 200 mm or less is pulled out, the rotation speed of the crucible 3 is set to 0.1 rpm or more and 7 rpm or less.

[0088] When the straight body portion is just formed, if the pulling is performed at a rotation speed exceeding 30 rpm, the operation of the pulling device 1 becomes unstable and the possibility of deformation of the straight body portion increases.

[0089] Next, if the rotation speed of the crucible 3 is less than 0.1 rpm within a range of 50 mm to 200 mm from the start position of the straight body portion, the silicon melt 9 to which the dopant is added becomes unstable, which is likely to cause dislocation.

[0090] On the other hand, when the rotation speed of crucible 3 exceeds 7 rpm, the oxygen concentration or resistivity within the surface of silicon single crystal 10 increases, and the crystal quality becomes unstable.

[0091] A portion of single crystal silicon 10 having a straight body diameter of greater than 201 mm and less than 230 mm pulled by such pulling apparatus 1, with red phosphorus used as a dopant, yields an ingot of single crystal silicon 10 having a resistivity of greater than 0.5 mΩcm and less than 0.7 mΩcm at a portion near the tail of the single crystal silicon 10.

[0092] After the outer periphery of the ingot of single crystal silicon 10 is ground to a straight body diameter of 200 mm, the portion is cut into silicon wafers using a wire saw or the like, and the cut silicon wafers are subjected to grinding and polishing steps, thereby obtaining silicon wafers with a diameter of 200 mm and a resistivity of greater than 0.5 mΩcm and less than 0.7 mΩcm.

[0093] Then, after processing the silicon wafer, an epitaxial film is formed on the surface of the silicon wafer to manufacture an epitaxial silicon wafer with a diameter of 200 mm and ship it to the customer.

[0094] Furthermore, when red phosphorus is used as a dopant in a portion of an ingot of single crystal silicon 10 having a straight body diameter of 301 mm to 330 mm, a resistivity of 0.8 mΩcm to 1.0 mΩcm is obtained in a portion near the tail of the single crystal silicon.

[0095] After the outer periphery of the ingot of single crystal silicon 10 is ground to a straight body diameter of 300 mm, the portion is cut into silicon wafers using a wire saw or the like, and the cut silicon wafers are subjected to grinding and polishing steps, thereby obtaining silicon wafers with a diameter of 300 mm and a resistivity of greater than 0.8 mΩcm and less than 1.0 mΩcm.

[0096] After processing the silicon wafer, an epitaxial growth film is formed on the surface of the silicon wafer to manufacture an epitaxial silicon wafer with a diameter of 300 mm and ship it to the customer.

[0097] On the other hand, when arsenic is used as a dopant, an ingot of single crystal silicon 10 having a resistivity of 1.7 mΩcm to 2.0 mΩcm is obtained in a portion near the tail of single crystal silicon 10 having a body diameter of 301 mm to 330 mm.

[0098] After the outer periphery of the ingot of single crystal silicon 10 is ground to a straight body diameter of 300 mm, the portion is cut into silicon wafers using a wire saw or the like, and the cut silicon wafers are subjected to grinding and polishing steps to obtain silicon wafers with a diameter of 300 mm.

[0099] After processing the silicon wafer, an epitaxial film is formed on the surface of the silicon wafer to manufacture an epitaxial silicon wafer with a diameter of 300 mm and ship it to the customer.

[0100] Example

[0101] Next, embodiments of the present invention will be described. The present invention is not limited to the embodiments described below, and other configurations are permitted within the scope of achieving the object of the present invention.

[0102] [1] In the case of an ingot of single crystal silicon 10 having a straight body diameter of 201 mm or more and 230 mm or less

[0103] When pulling a single crystal silicon 10 having a crystal diameter of 201 mm or more and 230 mm or less, the resistivity at the start position of the straight body portion (end position of the shoulder portion) of the single crystal silicon 10 is controlled to be 0.8 mΩcm or more and 1.05 mΩcm or less. The ratio of the inner diameter of the crucible 3 to the crystal diameter (= inner diameter of the crucible 3 / crystal diameter) is set to 2.1 to 2.3 in the embodiment, 2.6 to 3.0 in the comparative example and the reference example, and the feed amount is set to 80 kg to 180 kg. In addition, the pulling speed is set to 0.3 mm / min to 1.0 mm / min, the crystal rotation speed is set to 9 to 17 rpm, and the rotation speed of the crucible 3 is set to 0.2 rpm to 22 rpm.

[0104] In addition, the argon flow rate is set to 50 L / min to 150 L / min and the furnace pressure is set to 40 kPa to 80 kPa in the front half of the straight body of the silicon single crystal 10. In the rear half of the straight body of the silicon single crystal 10, the argon flow rate is set to 50 L / min to 200 L / min and the furnace pressure is set to 20 kPa to 80 kPa.

[0105] [1-1] When the resistivity is 0.6 mΩcm or more and 0.7 mΩcm or less

[0106] The inner diameter of the quartz crucible 3A was changed relative to the straight body diameter of the single crystal silicon 10, and the resistivity was controlled by the addition of red phosphorus dopant, Ar flow rate, furnace pressure, liquid level of the heat shielding plate 12, pulling speed of the single crystal silicon 10 and their combination for multiple benchmarks, and the single crystal silicon 10 doped with red phosphorus was pulled. The results are shown in Table 1 and Figure 2 In the following description, the straight body length 0% position refers to the starting position of the straight body portion of the single crystal silicon 10, and the straight body length 100% position refers to the starting position of the tail portion of the single crystal silicon 10. Furthermore, the straight body qualified length refers to the value obtained by dividing the length of the straight body region with qualified resistivity (within the desired resistance range) and without dislocation by the total length of the straight body, and the dislocation-free success rate refers to the ratio of the number of pull-up tries that can be pulled without dislocations.

[0107] [Table 1]

[0108]

[0109] Comparing Comparative Examples 1 and 2 with Examples 1 to 3, it can be seen that the dislocation-free success rate of Examples 1 to 3 is significantly higher, the crystal yield is also higher, and a larger amount of the ingot of the single crystal silicon 10 can be ensured to have a resistivity of 0.6 mΩcm or more and 0.7 mΩcm or less. Therefore, it was confirmed that when red phosphorus is used as a dopant to manufacture an ingot of the single crystal silicon 10 with a resistivity of 0.6 mΩcm or more and 0.7 mΩcm or less, it is preferred that the inner diameter of the quartz crucible 3A is 2.1 times or more and 2.3 times or less relative to the straight body diameter of the single crystal silicon 10.

[0110] [1-2] When the resistivity is 0.5 mΩcm or more and 0.6 mΩcm or less

[0111] When a portion of the ingot of the silicon single crystal 10 having a straight body diameter of 201 mm to 230 mm had a resistivity of 0.5 mΩcm to 0.6 mΩcm, the influence of the inner diameter of the quartz crucible 3A was confirmed.

[0112] Specifically, regarding the resistivity control implemented by the control of Ar flow rate / furnace pressure / pulling speed, the control direction has two directions, namely, evaporation suppression and evaporation promotion. From the top side of the single crystal silicon 10 until the desired resistivity is reached or below, evaporation is suppressed. Then, when the desired resistivity range has been entered, the setting is turned to the evaporation promotion side in order to offset the effect of segregation. With respect to the target value of 0.6 mΩcm or more and 0.7 mΩcm or less, in the range of 0.5 mΩcm or more and 0.6 mΩcm or less, the evaporation suppression interval occupies a longer interval until the later half of the crystal position (≤ 0.6 mΩcm).

[0113] The results are shown in Table 2 and Figure 3 .

[0114] [Table 2]

[0115]

[0116] If the qualified length of the crystal in Reference Examples 1 and 2 is 0%, it is impossible to make a part of the ingot of the single crystal silicon 10 be the target 0.5 mΩcm or more and 0.6 mΩcm or less. In contrast, in Examples 4 to 6, it was confirmed that the qualified length of the crystal in the part within the target resistivity range can be ensured. Therefore, it was confirmed that when red phosphorus was used as a dopant to manufacture an ingot of the single crystal silicon 10 with the target resistivity of 0.5 mΩcm or more and 0.6 mΩcm or less, it was also preferable that the inner diameter of the quartz crucible 3A be 2.1 times or more and 2.3 times or less relative to the straight body diameter of the single crystal silicon 10.

[0117] In particular, Example 7 shows that the resistivity is greatly reduced as the pulling of the single crystal silicon 10 is performed. By greatly reducing the resistivity, the resistivity at the start of the body portion is set to 1.05 mΩcm, and the resistivity of the crystal portion up to 20% of the body length is relatively high to suppress dislocation. After that, the resistivity is greatly reduced, and a single crystal with a target resistivity of 0.5 mΩcm or more and 0.6 mΩcm or less or 0.7 mΩcm or less can be obtained with a good yield. In addition, if the resistivity at the start of the body portion exceeds 1.05 mΩcm, the length of the body portion with a target resistivity of 0.5 mΩcm or more and 0.6 mΩcm or less becomes shorter, and the yield becomes lower.

[0118] Furthermore, as shown in Example 8, by setting the resistivity at the start of the body portion to 0.8 mΩcm, dislocations were suppressed, and the proportion of the body portion with a target resistivity of 0.5 mΩcm or more and 0.6 mΩcm or less was 35% of the entire body portion, and the proportion of the body portion with a resistivity of 0.5 mΩcm or more and 0.7 mΩcm or less was as high as 70% of the entire body portion. In addition, when the resistivity at the start of the body portion was set to 0.75 mΩcm, which was lower than 0.8 mΩcm, dislocations frequently occurred before 20% of the body length, and single crystals could not be grown.

[0119] [2] In the case of an ingot of single crystal silicon 10 having a straight body diameter of 301 mm or more and 330 mm or less

[0120] A silicon single crystal 10 having a crystal diameter of 301 mm or more and 330 mm or less is pulled up.

[0121] In the embodiments and comparative examples, the ratio of the inner diameter of the crucible 3 and the crystal diameter (= inner diameter of the crucible 3 / crystal diameter) is set to 1.7 to 2.0 in the embodiments and to 2.5 to 2.6 in the comparative examples, the feeding amount is set to 80 kg to 250 kg, the pulling speed is set to 0.3 mm / min to 1.0 mm / min, the crystal rotation speed is set to 5 rpm to 17 rpm, and the rotation speed of the crucible 3 is set to 0.2 rpm to 22 rpm.

[0122] In addition, the argon flow rate is set to 50 L / min to 150 L / min and the furnace pressure is set to 40 kPa to 80 kPa in the front half of the straight body of the silicon single crystal 10. In the rear half of the straight body of the silicon single crystal 10, the argon flow rate is set to 50 L / min to 200 L / min and the furnace pressure is set to 20 kPa to 80 kPa.

[0123] [2-1] When red phosphorus is used as a dopant (0.8 mΩcm or more and 1.0 mΩcm or less)

[0124] When red phosphorus is used as a dopant, when pulling a single crystal silicon 10 having a crystal diameter of 301 mm to 330 mm, the resistivity at the straight body start position (shoulder end position) of the single crystal silicon 10 is controlled to be 1.2 mΩcm to 1.7 mΩcm.

[0125] For the case where the straight body diameter of the single crystal silicon 10 is 301 mm or more and 330 mm or less, the inner diameter of the quartz crucible 3A relative to the straight body diameter of the single crystal silicon 10 is changed as described above, and the resistivity is controlled by adding a red phosphorus dopant for multiple benchmarks, and the single crystal silicon 10 doped with red phosphorus is pulled. The results are shown in Tables 3 and Figure 4 .

[0126] [Table 3]

[0127]

[0128] In Comparative Examples 3 and 4, it is not possible to pull the single crystal without dislocation (in Figure 4 The dotted line in the figure shows the result of measuring the resistivity in a state with dislocations, but the resistivity cannot reach below 1.0 mΩcm).

[0129] On the other hand, according to Examples 9 to 12, a dislocation-free success rate of 20% or more can be achieved, and the crystal qualified length is also 7% to 50%, so that the resistivity of a part of the ingot of the single crystal silicon 10 can be ensured to be 0.8 mΩcm or more and 1.0 mΩcm or less. Therefore, it is confirmed that when using red phosphorus as a dopant to manufacture an ingot of the single crystal silicon 10 with a target resistivity of 0.8 mΩcm or more and 1.0 mΩcm or less, the inner diameter of the quartz crucible 3A must be at least 1.7 times and 2.0 times the straight body diameter of the single crystal silicon 10.

[0130] [2-2] When arsenic is used as a dopant (1.7 mΩcm or more and 2.0 mΩcm or less)

[0131] For the case where the straight body diameter of the single crystal silicon 10 is greater than 301 mm and less than 330 mm, the inner diameter of the quartz crucible 3A relative to the straight body diameter of the single crystal silicon 10 is changed as described above, and the resistivity is controlled by adding arsenic dopants for multiple benchmarks, and the arsenic-doped single crystal silicon 10 is pulled at the same time.

[0132] At this time, the resistivity at the start position of the straight body (end position of the shoulder) of the single crystal silicon 10 was controlled to be greater than 2.5 mΩcm and less than 3.1 mΩcm. The results are shown in Tables 4 and Figure 5 .

[0133] [Table 4]

[0134]

[0135] In Comparative Examples 5 and 6, it is not possible to pull the single crystal without dislocation ( Figure 5 The dotted line in the figure shows the result of measuring the resistivity in a state with dislocations, but the resistivity cannot reach below 2.0 mΩcm).

[0136] According to Examples 13 to 16, a dislocation-free success rate of 10% or more can be achieved, and the crystal qualified length is 13% to 61%, so that the resistivity of a part of the ingot of the single crystal silicon 10 can be ensured to be 1.7 mΩcm or more and 2.0 mΩcm or less. Therefore, it is confirmed that when using arsenic as a dopant to manufacture an ingot of the single crystal silicon 10 with a target resistivity of 1.7 mΩcm or more and 2.0 mΩcm or less, the inner diameter of the quartz crucible 3A should be at least 1.7 times and 2.0 times the straight body diameter of the single crystal silicon 10.

[0137] Description of Reference Numerals

[0138] 1-pulling device, 2-chamber, 3-crucible, 3A-quartz crucible, 3B-graphite crucible, 4-support shaft, 5-heater, 6-insulating material, 7-pulling shaft, 8-seed crystal, 9-silicon melt, 10-single crystal silicon, 12-heat shielding plate, 13-gas inlet, 14-exhaust port.

Claims

1. A method for producing n-type single crystal silicon, wherein single crystal silicon is pulled and grown from a silicon melt containing red phosphorus as a main dopant by a pulling method, wherein the method for producing n-type single crystal silicon is characterized in that: A single crystal silicon having a body diameter of 301 mm to 330 mm and a resistivity of 0.8 mΩcm to 1.0 mΩcm is pulled up using a quartz crucible having an inner diameter of 1.7 to 2.0 times the body diameter of the single crystal silicon.

2. The method for producing n-type single crystal silicon according to claim 1, It is characterized in that The portion of the single crystal silicon is a straight body portion having a length that is 7% or more of the entire length of the straight body portion.

3. The method for producing n-type single crystal silicon according to claim 1 or 2, It is characterized in that The single crystal silicon is pulled up by setting the pressure in the furnace of the pulling device of the single crystal silicon to be 40 kPa or more and 80 kPa or less.

4. The method for producing n-type single crystal silicon according to claim 1 or 2, It is characterized in that A magnetic field having a magnetic field intensity of 0.2 T to 0.4 T is applied to the silicon melt in the quartz crucible to perform pulling.

5. The method for producing n-type single crystal silicon according to claim 3, It is characterized in that A magnetic field having a magnetic field intensity of 0.2 T to 0.4 T is applied to the silicon melt in the quartz crucible to perform pulling.

6. A method for producing n-type single crystal silicon, wherein single crystal silicon is pulled and grown from a silicon melt containing arsenic as a main dopant by a pulling method, wherein the method for producing n-type single crystal silicon is characterized in that: A single crystal silicon having a straight body diameter of 301 mm to 330 mm and a resistivity of 1.7 mΩcm to 2.0 mΩcm is pulled up using a quartz crucible having an inner diameter of 1.7 to 2.0 times the straight body diameter of the single crystal silicon.

7. The method for producing n-type single crystal silicon according to claim 6, It is characterized in that The portion of the silicon single crystal is a straight body portion having a length that is 13% or more of the entire length of the straight body portion.

8. The method for producing n-type single crystal silicon according to claim 6 or 7, It is characterized in that The single crystal silicon is pulled up by setting the pressure in the furnace of the pulling device of the single crystal silicon to be 40 kPa or more and 80 kPa or less.

9. The method for producing n-type single crystal silicon according to claim 6 or 7, It is characterized in that A magnetic field having a magnetic field intensity of 0.2 T to 0.4 T is applied to the silicon melt in the quartz crucible to perform pulling.

10. The method for producing n-type single crystal silicon according to claim 8, It is characterized in that A magnetic field having a magnetic field intensity of 0.2 T to 0.4 T is applied to the silicon melt in the quartz crucible to perform pulling.