Cleaning method for reducing particles on semiconductor substrate wafer surface
Through multi-stage ultrasonic and chemical reagent cleaning methods, the problem of difficulty in removing the surface particles of semiconductor substrate wafers in the prior art is solved, efficient particle removal is achieved, and the surface quality of the wafer is significantly improved.
Patent Information
- Application Number
- CN202210224877.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-03-09
AI Technical Summary
The existing chemical reagent cleaning methods are difficult to fully remove particles on the surface of semiconductor substrate wafers, resulting in low surface quality and affecting device performance.
Multi-stage cleaning methods are adopted, including ultrasonic dewax cleaning, ultrasonic deionized water cleaning, chemical reagent cleaning and megasonic cleaning. Through the combination of ultrasonic and chemical reagents at different frequencies, particles of different particle sizes are gradually removed.
It effectively reduces the residual particle defects on the surface of gallium arsenide and indium phosphide wafers, with a particle size of less than 100 pieces per piece, significantly improving the surface quality of the wafer and product yield.
Smart Images

Figure CN114613697B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor wafer processing, and in particular relates to a cleaning method for reducing particles on the surface of a semiconductor substrate wafer. Background Art
[0002] Group III-V compound semiconductor materials such as gallium arsenide (GaAs) and indium phosphide (InP) have high saturated electron drift velocity and strong radiation resistance. As substrate materials, they have important applications in key electronic components such as optoelectronic devices and microelectronic devices.
[0003] Surface particle size is an important performance indicator to characterize the surface quality of semiconductor wafers. Gallium arsenide, indium phosphide and other semiconductor wafers are used as substrate materials for the preparation of epitaxial structural materials for optoelectronic and microelectronic devices. The particles on the wafer surface have an important impact on the performance of epitaxial materials. Particles on the wafer surface will act as surface defects or extend into the epitaxial structural materials, reducing the quality of epitaxial materials and thus affecting the improvement of device performance. Therefore, the particles on the wafer surface must be fully reduced to improve the wafer surface quality.
[0004] At present, the existing method of reducing the particles on the surface of the chip is to clean it with chemical reagents, but this method results in the inability to fully remove the surface particles. This is because there are many particles on the surface of the chip, up to 500 per chip; therefore, in order to further reduce the particles on the surface of the chip and improve the quality of the material, it is necessary to study a cleaning method for reducing the particles on the surface of the semiconductor substrate chip that can effectively remove the particles on the surface of the chip, improve the surface quality of the chip and the yield. Summary of the invention
[0005] The present invention provides an intelligent control switch tool for stratified injection and production, which can control multiple rounds of stratified carbon dioxide injection, stratified well shut-in, stratified blow-out and stratified oil production in a variety of ways without moving the injection and production pipe string, so as to achieve the purposes of balanced carbon dioxide injection displacement, differential effective well shut-in, reduction of interlayer interference, and improvement of oil layer utilization, thereby improving carbon dioxide utilization rate and throughput production efficiency, reducing well repair operation volume and well occupation time, avoiding oil layer pollution, and reducing operation costs.
[0006] The present invention solves the technical problem by adopting the following technical solutions:
[0007] A cleaning method for reducing particles on the surface of a semiconductor substrate wafer comprises the following steps:
[0008] The semiconductor substrate wafer is ultrasonically cleaned, wherein the ultrasonic cleaning includes ultrasonic dewaxing cleaning and ultrasonic deionized water cleaning in sequence; the ultrasonic frequency of the ultrasonic dewaxing cleaning is 25KHz; the ultrasonic deionized water cleaning is sequentially cleaned with frequencies of 40KHz, 80KHz, and 120KHz;
[0009] Cleaning the semiconductor substrate wafer after ultrasonic cleaning with chemical reagents, wherein the chemical reagent is sulfuric acid;
[0010] The semiconductor substrate wafer after chemical cleaning is cleaned by megasonic wave, and the frequency of megasonic wave cleaning is 0.9MHz~1.2MHz.
[0011] Further, the chemical reagent cleaning comprises the following steps:
[0012] The semiconductor substrate wafer is placed in sulfuric acid at a temperature of 50°C-80°C for 30s-60s to remove organic impurities and metal impurities on the surface of the wafer;
[0013] The semiconductor substrate wafer is placed in sulfuric acid at a temperature of 20°C-30°C for etching for 60s-120s to further remove metal impurities on the surface of the wafer.
[0014] Furthermore, the megasonic cleaning comprises the following steps:
[0015] The semiconductor substrate wafer is cleaned by deionized water megasonic wave for 2-5 minutes, the megasonic wave frequency is 0.9MHz-1.2MHz, and particles with a particle size less than 0.5μm on the wafer surface are removed;
[0016] The semiconductor substrate wafer is spin-dried or blow-dried.
[0017] Furthermore, the ultrasonic dewaxing cleaning comprises the following steps:
[0018] The polished semiconductor substrate wafer is placed in a dewaxing agent at a temperature of 60°C to 80°C and ultrasonically cleaned for 5-10 minutes at an ultrasonic frequency of 25KHz;
[0019] Then, the semiconductor substrate wafer after ultrasonic cleaning is placed in anhydrous ethanol at 20°C to 30°C and ultrasonically cleaned for 3-5 minutes at an ultrasonic frequency of 25KHz.
[0020] Furthermore, the ultrasonic deionized water cleaning comprises the following steps:
[0021] The semiconductor substrate wafer after ultrasonic dewaxing cleaning is placed in deionized water for ultrasonic cleaning for 3-5 minutes, the ultrasonic frequency is 40KHz, the deionized water temperature is 20℃-30℃, and particles with a particle size of 2-50μm on the surface of the wafer are removed;
[0022] The semiconductor substrate after ultrasonic deionized water cleaning is cleaned again with deionized water, with an ultrasonic frequency of 80KHz, to remove particles with a particle size of 1 to 5μm on the surface of the wafer;
[0023] The semiconductor substrate cleaned by ultrasonic deionized water is cleaned again by deionized water, with an ultrasonic frequency of 120 KHz, to remove particles with a particle size of 0.5 to 3 μm on the surface of the wafer.
[0024] Furthermore, the dewaxing agent is a neutral organic dewaxing agent with a pH value of 7.0-8.0.
[0025] Furthermore, the megasonic cleaning is single-wafer cleaning, the deionized water temperature is 20° C. to 30° C., and the water flow rate is 0.9-1.5 L / min.
[0026] Furthermore, the semiconductor substrate wafer is a gallium arsenide semiconductor substrate wafer or an indium phosphide semiconductor substrate wafer.
[0027] The advantages and positive effects of the present invention are:
[0028] The method of the invention can effectively reduce residual particle defects on the surface of gallium arsenide and indium phosphide wafers, with a particle size of less than 100 per wafer, thereby improving the surface quality of the wafer and the product yield; the method has low cost and strong practicability, and is suitable for mass production of semiconductor wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.
[0030] Figure 1 This is a particle size detection diagram of the GaAs wafer surface before cleaning in Example 2;
[0031] Figure 2 This is a graph showing the particle size detection of the GaAs wafer surface after cleaning by the method of the present invention in Example 2;
[0032] Figure 3 This is a particle detection diagram of the GaAs wafer surface after cleaning by Scheme 1 in Example 3;
[0033] Figure 4 This is a particle detection diagram of the GaAs wafer surface after cleaning by Scheme 2 in Example 3;
[0034] Figure 5 This is a particle detection diagram of the GaAs wafer surface after cleaning by Scheme 3 in Example 3;
[0035] Figure 6 This is a particle detection diagram of the GaAs wafer surface after cleaning by Scheme 4 in Example 4;
[0036] Figure 7 This is a particle detection diagram of the GaAs wafer surface after cleaning by Scheme 5 in Example 4. DETAILED DESCRIPTION
[0037] First of all, it should be noted that the specific structure, features and advantages of the present invention will be specifically described below by way of example, but all descriptions are only for illustration and should not be understood as limiting the present invention in any way. In addition, any single technical feature described or implied in the embodiments mentioned herein, or any single technical feature displayed or implied in the drawings, can still be combined or deleted between these technical features (or their equivalents) to obtain more other embodiments of the present invention that may not be directly mentioned in this document. In addition, in order to simplify the drawings, the same or similar technical features may be marked only in one place in the same drawing.
[0038] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, or are the directions or positional relationships in which the inventive product is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0039] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.
[0040] Example 1
[0041] The cleaning method for reducing particles on the surface of a semiconductor substrate wafer provided in this embodiment comprises the following steps:
[0042] The semiconductor substrate wafer is ultrasonically cleaned, wherein the ultrasonic cleaning includes ultrasonic dewaxing cleaning and ultrasonic deionized water cleaning in sequence; the ultrasonic frequency of the ultrasonic dewaxing cleaning is 25KHz; the ultrasonic deionized water cleaning is sequentially cleaned with frequencies of 40KHz, 80KHz, and 120KHz;
[0043] Cleaning the semiconductor substrate wafer after ultrasonic cleaning with chemical reagents, wherein the chemical reagent is sulfuric acid;
[0044] The semiconductor substrate wafer after chemical cleaning is cleaned by megasonic wave, and the frequency of megasonic wave cleaning is 0.9MHz~1.2MHz.
[0045] Specifically, the ultrasonic dewaxing cleaning comprises the following steps:
[0046] The polished semiconductor substrate wafer is placed in a wax remover at a temperature of 60°C to 80°C, and ultrasonically cleaned for 5-10 minutes at an ultrasonic frequency of 25KHz, wherein the wax remover is a neutral organic wax remover with a pH value of 7.0-8.0;
[0047] Then, the semiconductor substrate wafer after ultrasonic cleaning is placed in anhydrous ethanol at 20°C to 30°C and ultrasonically cleaned for 3-5 minutes at an ultrasonic frequency of 25KHz.
[0048] The ultrasonic deionized water cleaning comprises the following steps:
[0049] The semiconductor substrate wafer after ultrasonic dewaxing cleaning is placed in deionized water for ultrasonic cleaning for 3-5 minutes, the ultrasonic frequency is 40KHz, the deionized water temperature is 20℃-30℃, and particles with a particle size of 2-50μm on the surface of the wafer are removed;
[0050] The semiconductor substrate after ultrasonic deionized water cleaning is cleaned again with deionized water, the ultrasonic cleaning is 3-5 minutes, the deionized water temperature is 20℃-30℃, the ultrasonic frequency is 80KHz, and the particles with a particle size of 1-5μm on the surface of the wafer are removed;
[0051] The semiconductor substrate after ultrasonic deionized water cleaning is cleaned again with deionized water for 3-5 minutes, the deionized water temperature is 20℃-30℃, the ultrasonic frequency is 120KHz, and particles with a particle size of 0.5-3μm on the surface of the chip are removed.
[0052] Specifically, the chemical reagent cleaning includes the following steps:
[0053] The semiconductor substrate wafer is placed in concentrated sulfuric acid (concentration>95%) at a temperature of 50°C-80°C for 30s-60s to remove organic impurities and metal impurities on the surface of the wafer;
[0054] The semiconductor substrate wafer is placed in concentrated sulfuric acid (concentration>95%) at a temperature of 20° C.-30° C. for etching for 60s-120s to further remove metal impurities on the surface of the wafer, wherein the sulfuric acid specification is MOS grade or UP grade.
[0055] Specifically, the megasonic cleaning comprises the following steps:
[0056] The semiconductor substrate wafer is cleaned by deionized water megasonic wave for 2-5 minutes, the megasonic wave frequency is 0.9MHz-1.2MHz, and particles with a particle size less than 0.5μm on the wafer surface are removed; it should be noted that the megasonic wave cleaning is a single-wafer cleaning, the deionized water temperature is 20℃~30℃, and the water flow rate is 0.9-1.5L / min;
[0057] Spin dry or blow dry the semiconductor substrate wafer with nitrogen.
[0058] Example 2
[0059] The method in Example 1 was used to clean the semiconductor substrate wafer gallium arsenide (GaAs). Before cleaning, the particle size of the surface of the gallium arsenide wafer was 5390 (eg Figure 1 ), after cleaning, 20 (such as Figure 2 ), the reduction rate is (5390-20) / 5390=99.6%, which shows that the method in Example 1 can effectively remove the residual particles on the surface of the gallium arsenide wafer.
[0060] Example 3
[0061] In this embodiment, the GaAs wafer is subjected to ultrasonic cleaning, chemical reagent cleaning, and megasonic cleaning respectively. The specific implementation process is shown in Table 1.
[0062] Table 1
[0063]
[0064] The GaAs wafer was only subjected to ultrasonic cleaning, the implementation scheme is shown in Table 1, sample 1#, and the particle size of the wafer surface after ultrasonic cleaning was 671 (such as Figure 3 As shown), the reduction rate is (5390-671) / 5390=87.5%; the reason why ultrasonic cleaning can reduce particles on the chip surface is that ultrasonic waves can generate high-energy sound waves to drive the solution to accelerate, and the solution continuously impacts the chip surface in the form of accelerated fluid, so that particles and other pollutants on the chip surface leave the chip surface and enter the solution; ultrasonic waves of different frequencies can have a cleaning effect on particles of different particle sizes; in this embodiment, the dewaxing agent can remove organic wax on the chip surface, and then ultrasonic cleaning of different frequencies can achieve a good effect of reducing particle size.
[0065] The GaAs wafer was only cleaned with chemical reagents, and the implementation scheme is shown in Sample 2# in Table 1. The particle size of the wafer surface after chemical cleaning was 1560 (such as Figure 4 As shown in the figure, the reduction rate is 71.1%. In this process, the GaAs wafer has not been dewaxed and cleaned with ultrasonic waves of different frequencies, and the organic wax on the surface of the wafer has a strong adsorption effect on the particles. Concentrated sulfuric acid has a certain cleaning effect on organic particles and metal impurities, but overall the effect on reducing particles is general.
[0066] The GaAs wafer was only cleaned by megasonic wave, and the implementation scheme is shown in Table 1, Sample 3#. The particle size of the wafer surface after megasonic wave cleaning was 1913 (such as Figure 5The reduction rate is 64.5%. The higher the ultrasonic frequency, the better the removal effect on particles with smaller particle sizes. Megasonic waves of 0.9MHz-1.2MHz have a better removal effect on particles below 0.5μm. In this process, the wafer is only cleaned by megasonic waves. The organic wax contamination on the wafer surface and the large particles are difficult to be effectively removed, resulting in a general reduction effect on the overall particle size.
[0067] Example 4
[0068] In this embodiment, the experimental effects of different cleaning sequences of ultrasonic cleaning, chemical reagent cleaning, and megasonic cleaning of GaAs are analyzed, and the specific implementation scheme is shown in Table 2:
[0069] Table 2
[0070]
[0071]
[0072] In scheme 4, the GaAs wafer is firstly cleaned by ultrasonic wave, then by megasonic wave, and finally by chemical reagent cleaning. The scheme is shown in sample 4# in Table 2. After cleaning, there are 198 particles on the surface of the wafer (such as Figure 6 As shown in Table 2, the removal rate is 96.3%. In Scheme 5, the GaAs wafer is first dewaxed and cleaned by megasonic wave, then cleaned by chemical reagents, and finally ultrasonically cleaned. The implementation scheme is shown in Table 2 #5. After cleaning, there are 279 particles on the wafer surface (as shown in Table 2). Figure 7 As shown in the figure, the removal rate is 94.8%. Although the removal rates of Schemes 4 and 5 are very high, some particles still exist on the surface of the chip. This is mainly because the chemical cleaning and ultrasonic cleaning of the final cleaning are generally ineffective in removing tiny particles on the surface. Moreover, after the final chemical cleaning and ultrasonic cleaning, relatively large particles may be decomposed into tiny particles and remain on the surface of the chip.
[0073] Comparative Example 2, Example 3 and Example 4: In Example 2, the GaAs wafer is first subjected to ultrasonic cleaning to effectively remove organic wax residues on the wafer surface, and ultrasonic cleaning at 25KHz, 40KHz, 80KHz and 120KHz can effectively reduce particles larger than 0.5 microns on the wafer surface, and then chemical reagent cleaning can remove organic residual particles and metal impurities on the wafer surface, and finally megasonic cleaning can further reduce particles smaller than 0.5μm on the wafer surface; the method of the present invention can achieve a reduction rate of particles on the wafer surface of more than 99%, which has a better cleaning effect than the methods in Examples 3 and 4.
[0074] The above embodiments describe the present invention in detail, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.
Claims
1. A cleaning method for reducing particles on the surface of a semiconductor substrate wafer, characterized in that: The steps include: Ultrasonic dewaxing cleaning and ultrasonic deionized water cleaning; the ultrasonic frequency of the ultrasonic dewaxing cleaning is 25KHz; the ultrasonic deionized water cleaning is carried out in the order of 40KHz, 80KHz and 120KHz; Cleaning the semiconductor substrate wafer after ultrasonic cleaning with chemical reagents, wherein the chemical reagent is sulfuric acid; The semiconductor substrate wafer after chemical cleaning is cleaned by megasonic wave, and the frequency of megasonic wave cleaning is 0.9MHz~1.2MHz; The chemical reagent cleaning comprises the following steps: The semiconductor substrate wafer is placed in sulfuric acid at a temperature of 50°C-80°C for 30s-60s to remove organic impurities and metal impurities on the surface of the wafer; The semiconductor substrate wafer is placed in sulfuric acid at a temperature of 20°C-30°C for 60s-120s to further remove metal impurities on the wafer surface; The megasonic cleaning comprises the following steps: The semiconductor substrate wafer is cleaned by deionized water megasonic wave for 2-5 minutes, the megasonic wave frequency is 0.9MHz-1.2MHz, and particles with a particle size less than 0.5μm on the wafer surface are removed; Spin or blow dry the semiconductor substrate wafer; The ultrasonic dewaxing cleaning comprises the following steps: The polished semiconductor substrate wafer is placed in a dewaxing agent at a temperature of 60°C to 80°C and ultrasonically cleaned for 5-10 minutes at an ultrasonic frequency of 25KHz; Then, the semiconductor substrate wafer after ultrasonic cleaning is placed in anhydrous ethanol at 20°C to 30°C and ultrasonically cleaned for 3-5 minutes at an ultrasonic frequency of 25KHz; The ultrasonic deionized water cleaning comprises the following steps: The semiconductor substrate wafer after ultrasonic dewaxing cleaning is placed in deionized water for ultrasonic cleaning for 3-5 minutes, the ultrasonic frequency is 40KHz, the deionized water temperature is 20℃-30℃, and particles with a particle size of 2-50μm on the surface of the wafer are removed; The semiconductor substrate after ultrasonic deionized water cleaning is cleaned again with deionized water, with an ultrasonic frequency of 80KHz, to remove particles with a particle size of 1 to 5μm on the surface of the wafer; The semiconductor substrate cleaned by ultrasonic deionized water is cleaned again by deionized water, with an ultrasonic frequency of 120 KHz, to remove particles with a particle size of 0.5 to 3 μm on the surface of the wafer.
2. The cleaning method for reducing particles on the surface of a semiconductor substrate wafer according to claim 1, characterized in that: The dewaxing agent is a neutral organic dewaxing agent with a pH value of 7.0-8.
0.
3. The cleaning method for reducing particles on the surface of a semiconductor substrate wafer according to claim 1, characterized in that: The megasonic cleaning is single-wafer cleaning, the deionized water temperature is 20° C. to 30° C., and the water flow rate is 0.9-1.5 L / min.
4. The cleaning method for reducing particles on the surface of a semiconductor substrate wafer according to claim 1, characterized in that: The semiconductor substrate wafer is a gallium arsenide semiconductor substrate wafer or an indium phosphide semiconductor substrate wafer.
Citation Information
Patent Citations
Method for cleaning polished gallium arsenide chip and laundry drier
CN101661869A