Super junction device and manufacturing method

By etching the inverted trapezoidal trench into a rectangular shape in the superjunction device, the charge gap between the P-type pillar and the N-type pillar is reduced, the problem of low withstand voltage performance is solved, and the effects of high withstand voltage and low on-resistance are achieved. It also saves process costs and improves stability.

CN114613835BActive Publication Date: 2024-10-18SHANGHAI GONGCHENG SEMICON TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202011445148.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-08
Publication Date
2024-10-18
Estimated Expiration
2040-12-08

AI Technical Summary

Technical Problem

In the prior art, the trench obtained by etching has an inverted trapezoidal structure, which results in a large charge gap between the superjunction P-type pillar and the N-type pillar, resulting in a problem of reduced device voltage resistance.

Method used

By etching the bottom of the inverted trapezoidal trench of the first substrate to make it rectangular, and forming a support layer on the substrate to avoid sidewall collapse, a rectangular trench is formed to reduce the size of P-type pillars and N-type pillars. The charge difference achieves charge balance.

Benefits of technology

The withstand voltage performance of the superjunction device is improved and the on-resistance is reduced, and the process cost is saved and the process stability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114613835B_ABST
    Figure CN114613835B_ABST
Patent Text Reader

Abstract

The present invention provides a super junction device and a manufacturing method, the method comprising: 1) providing a first substrate, the first substrate comprising a first main surface and a second main surface, etching a groove on the first main surface of the first substrate by a photolithography-etching process based on a photomask, the groove being in an inverted trapezoidal shape; 2) bonding the first substrate to the second substrate; 3) thinning the first substrate and retaining a supporting layer; 4) oxidizing the supporting layer, corroding and removing the oxide layer to reveal the groove; 5) etching the bottom of the groove based on a hard mask plate having the same pattern as the photomask to increase the bottom width of the groove so that the morphology of the groove is roughly rectangular. The present invention etches from the bottom of the groove with a smaller width to increase the size of the bottom of the groove, so that the groove is rectangular, thereby reducing the charge gap between the P-type column and the N-type column in the super junction structure, so that the super junction device reaches charge balance, thereby improving the withstand voltage performance of the super junction device and reducing the on-resistance of the super junction device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor device design and manufacturing, and in particular relates to a super junction device and a manufacturing method thereof. Background Art

[0002] In the field of power semiconductors, a vertical metal oxide semiconductor field effect transistor (MOSFET) formed by a vertical double diffusion process is called a VDMOSFET, or VDMOS for short. For traditional VDMOS, the breakdown voltage is generally increased by increasing the thickness of the epitaxial layer and reducing the doping concentration of the epitaxial layer. However, this method will significantly increase the resistance of the epitaxial layer. The super junction metal oxide semiconductor field effect transistor (SJ-MOSFET) is an improved structure of the VDMOS device. It forms a P-type column and an N-type column by adding an alternating PN structure in the epitaxial layer. When the device is in a blocking state, the longitudinal electric field in the epitaxial layer is almost constant, which greatly reduces the dependence of the device's on-resistance on the breakdown voltage, thereby reducing the device's on-state loss. Therefore, this structure is widely used in devices with high breakdown voltage. Summary of the invention

[0003] In view of the shortcomings of the prior art described above, the object of the present invention is to provide a super junction device and a manufacturing method, which is used to solve the problem in the prior art that the grooves etched are inverted trapezoidal structures, resulting in a large difference in charge between the super junction P-type columns and N-type columns, which is not conducive to charge balance and causes a decrease in the device's withstand voltage.

[0004] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for manufacturing a super junction device, the manufacturing method comprising: 1) providing a first substrate, the first substrate comprising a first main surface and a second main surface relative to each other, etching a groove on the first main surface of the first substrate by a photolithography-etching process based on a photomask, and the groove is in an inverted trapezoidal shape; 2) providing a second substrate, bonding the first main surface of the first substrate to the second substrate; 3) thinning the first substrate from the second main surface of the first substrate, so that a supporting layer is retained between the second main surface of the first substrate and the groove; 4) oxidizing the supporting layer to form an oxide layer, and removing the oxide layer by etching to expose the groove; 5) based on a hard mask plate with the same photomask pattern as that of step 1), after aligning the hard mask plate with the groove, directly etching the bottom of the groove to increase the bottom width of the groove so that the morphology of the groove is roughly rectangular.

[0005] Optionally, the bottom width of the groove in step 1) is between one quarter and three quarters of the top width.

[0006] Optionally, the depth of the groove is between 1 and 50 microns.

[0007] Optionally, the depth of the groove is between 30 and 45 microns.

[0008] Optionally, the etching method of step 1) and step 5 includes one of reactive ion etching (RIE) and deep silicon etching (ICP).

[0009] Optionally, in step 3), the first substrate is thinned by a chemical mechanical polishing process, and the thickness of the support layer after thinning is between 0.5 microns and 2 microns.

[0010] Optionally, the manufacturing method further includes the step: 6) the first substrate is doped with a first conductivity type, and a semiconductor material layer doped with a second conductivity type is filled in the groove to form a super junction structure together with the first substrate.

[0011] Optionally, the manufacturing method also includes the steps of: 7) forming a second conductive type body region on the super junction structure; 8) forming a first conductive type source region in the second conductive type body region; 9) manufacturing a gate structure on the first conductive type source region and the second conductive type body region; 10) forming an insulating layer and an electrode lead-out structure; wherein the second substrate includes a first conductive type drain region.

[0012] Optionally, step 8) further includes the step of forming a second conductivity type contact region in the first conductivity type source region.

[0013] Optionally, the first conductivity type is N-type, and the second conductivity type is P-type, or the first conductivity type is P-type, and the second conductivity type is N-type.

[0014] The present invention also provides a super junction device, which includes: a first conductive type drain region; a super junction structure located on the first conductive type drain region, including a first conductive type column and a second conductive type column arranged in sequence, and the first conductive type column and the second conductive type column are both roughly rectangular in shape; a second conductive type body region formed on the super junction structure; a first conductive type source region formed in the second conductive type body region; a gate structure formed on the first conductive type source region and the second conductive type body region; an insulating layer and an electrode lead-out structure located on the first conductive type source region and the gate structure.

[0015] Optionally, it also includes a second conductivity type contact region formed in the first conductivity type source region.

[0016] Optionally, the depth of the super junction structure is between 30 and 45 microns.

[0017] Optionally, the first conductivity type is N-type, and the second conductivity type is P-type, or the first conductivity type is P-type, and the second conductivity type is N-type.

[0018] As described above, the super junction device and the manufacturing method of the present invention have the following beneficial effects:

[0019] The present invention bonds a first substrate with an inverted trapezoidal groove formed by etching to a second substrate, thins the back side to expose the bottom of the inverted trapezoidal groove, and then etches from the bottom of the groove with a smaller width to increase the size of the bottom of the groove, so that the groove is rectangular, thereby reducing the charge difference between the P-type column and the N-type column in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.

[0020] The present invention adopts a hard mask having the same pattern as that of etching the inverted trapezoidal groove, directly etches the bottom of the inverted trapezoidal groove to make the groove rectangular, does not need to perform photolithography, and can greatly save process costs.

[0021] The present invention thins the substrate by chemical mechanical grinding, oxidation, and removal of the oxide layer. Compared with direct grinding to reveal the groove, the retained support layer can provide support for the groove and its sidewalls during grinding, which can effectively avoid the risk of groove sidewall collapse that is easily caused by direct grinding to reveal the groove, thereby improving process stability.

[0022] The super junction device manufactured by the present invention has the advantages of high process stability, strong voltage resistance and low on-resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figures 1 to 10 Shown is a schematic structural diagram of each step of a method for manufacturing a super junction device according to an embodiment of the present invention.

[0024] Component number description

[0025] 101 First Substrate

[0026] 102 Groove

[0027] 103 Second substrate

[0028] 104 Support layer

[0029] 105 Oxide layer

[0030] 106 Hard Mask

[0031] 201 Leakage Area

[0032] 202 Drain electrode

[0033] 203 N-type column

[0034] 204 P-type column

[0035] 205 Body Area

[0036] 206 Source Area

[0037] 207 Contact Zone

[0038] 208 Gate structure

[0039] 209 Insulation layer

[0040] 210 Electrode lead structure DETAILED DESCRIPTION

[0041] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0042] For example, when describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional view showing the device structure will not be partially enlarged according to the general scale, and the schematic view is only an example, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional space dimensions of length, width and depth should be included.

[0043] For ease of description, spatially relative terms such as "under", "below", "below", "below", "above", "on", etc. may be used herein to describe the relationship of one element or feature shown in the drawings to other elements or features. It will be understood that these spatially relative terms are intended to encompass other orientations of the device in use or operation in addition to the orientation depicted in the drawings. In addition, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present.

[0044] In the context of the present application, a structure in which a first feature is described as being "above" a second feature may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0045] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and therefore the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0046] The key to superjunction devices achieving high withstand voltage and low on-resistance is to achieve PN charge balance by forming N-type and P-type conductive areas in the substrate. Therefore, the ideal P-type conductive area is a rectangle, but due to the limitation of the etching process, the etched groove can only be an inverted trapezoidal structure, which results in a large difference in charge between the P-type column and the N-type column at different depths, which is not conducive to charge balance and has a certain impact on the withstand voltage of the device.

[0047] In order to solve the problem that there is a large difference in charge between the P-type column 204 and the N-type column 203, which is not conducive to charge balance, this embodiment provides a method for manufacturing a super junction device, and the manufacturing method includes the following steps:

[0048] like Figure 1-2 As shown, firstly, step 1) is performed to provide a first substrate 101, wherein the first substrate 101 includes a first main surface and a second main surface relative to each other, and based on a photomask, a groove 102 is etched on the first main surface of the first substrate 101 by a photolithography-etching process, wherein the groove 102 is in an inverted trapezoidal shape.

[0049] The first substrate 101 may be a semiconductor substrate such as a silicon substrate, a silicon-germanium substrate, or a germanium substrate. In the present embodiment, the first substrate 101 is an N-type lightly doped silicon substrate.

[0050] Based on a photomask, a groove 102 is etched on the first main surface of the first substrate 101 by a photolithography-etching process. The etching method may be, for example, one of ordinary plasma etching, reactive ion etching RIE and deep silicon etching ICP. Since the groove 102 has a high aspect ratio, such as more than 10:1, and due to the limitation of the etching process, the sidewall of the etched groove 102 is inclined inward from the top of the groove 102 to the bottom of the groove 102, so that the groove 102 is in an inverted trapezoidal shape. For example, the bottom width of the inverted trapezoidal groove 102 is between one quarter and three quarters of the top width. In a specific implementation process, the bottom width of the inverted trapezoidal groove 102 is one quarter of the top width.

[0051] According to the size requirements of the device, the depth of the groove 102 may be between 1 and 50 microns. Preferably, the depth of the groove 102 is between 30 and 45 microns.

[0052] like Figure 3 and Figure 4 As shown, step 2) is then performed to provide a second substrate 103 and bond the first main surface of the first substrate 101 to the second substrate 103 .

[0053] In this embodiment, the second substrate 103 is made of the same material as the first substrate 101, and the second substrate 103 is an N-type lightly doped silicon substrate. The bonding method of the first substrate 101 and the second substrate 103 can be a silicon-silicon direct bonding process.

[0054] like Figure 5 As shown, step 3) is then performed to thin the first substrate 101 from the second main surface of the first substrate 101 so that a supporting layer 104 is retained between the second main surface of the first substrate 101 and the groove 102 .

[0055] For example, a chemical mechanical polishing process can be used to thin the first substrate 101 from the second main surface of the first substrate 101, so that a support layer 104 is retained between the second main surface of the first substrate 101 and the groove 102. The thickness of the thinned support layer 104 is between 0.5 microns and 2 microns. In a specific embodiment, the thickness of the thinned support layer 104 is 1 micron.

[0056] like Figure 6-7 As shown, step 4 is then performed to oxidize the support layer 104 to form an oxide layer 105 , and then remove the oxide layer 105 by etching to expose the trench 102 .

[0057] In this embodiment, the support layer 104 is oxidized by a thermal oxidation process so that the support layer 104 is completely oxidized to form an oxide layer 105. Then, the oxide layer 105 is removed by a wet etching process to expose the groove 102. The etching solution used in the wet etching has a high selectivity to silicon dioxide and silicon. For example, the etching solution can be hydrofluoric acid (HF).

[0058] The present invention thins the substrate by chemical mechanical grinding, oxidation, and removal of the oxide layer 105. Compared with direct grinding to reveal the groove 102, the retained support layer 104 can provide support for the groove 102 and its sidewalls during grinding, which can effectively avoid the risk of collapse of the sidewalls of the groove 102 that is easily caused by direct grinding to reveal the groove 102, thereby improving process stability.

[0059] like Figure 8-Figure 9As shown, step 5) is then performed. Based on the hard mask plate 106 having the same photomask pattern as that of step 1), after the hard mask plate 106 is aligned with the groove 102, the bottom of the groove 102 is directly etched to increase the bottom width of the groove 102 so that the shape of the groove 102 is roughly rectangular.

[0060] The etching method shown can be one of ordinary plasma etching, reactive ion etching RIE and deep silicon etching ICP. The etching depth can be set to be the same as the depth of the groove 102 to ensure that the morphology of the groove 102 is roughly rectangular, and the roughly rectangular means that the groove 102 is roughly rectangular, which may include a certain degree of morphological change caused by errors caused by technical or process limitations, and such morphological changes should not be excluded from the scope of the claims of this application.

[0061] The present invention uses a hard mask 106 having the same pattern as that of the inverted trapezoidal groove 102 to directly etch the bottom of the inverted trapezoidal groove 102 to make the groove 102 rectangular, without the need for photolithography, which can greatly save process costs.

[0062] like Fig.10 As shown, step 6 is then performed: the first substrate 101 is doped with the first conductivity type, and a semiconductor material layer doped with the second conductivity type is filled in the trench 102 to form a super junction structure together with the first substrate 101.

[0063] For example, the second conductive type doped semiconductor material layer may be a P-type silicon layer, and the P-type silicon layer and the N-type doped first substrate 101 are arranged together to form a super junction structure in which the P-type columns 204 and the N-type columns 203 are alternately arranged.

[0064] The present invention bonds a first substrate 101 having an inverted trapezoidal groove 102 formed by etching to a second substrate 103, thins the back side to expose the bottom of the inverted trapezoidal groove 102, and then etches from the bottom of the groove 102 with a smaller width to increase the size of the bottom of the groove 102, thereby making the groove 102 rectangular, thereby reducing the charge difference between the P-type column 204 and the N-type column 203 in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.

[0065] like Fig.10 As shown, step 7) is then performed to form a second conductivity type body region 205 on the super junction structure.

[0066] For example, the P-type body region 205 may be formed on the super junction structure by an ion implantation process.

[0067] like Fig.10As shown, step 8) is then performed to form a first conductivity type source region 206 in the second conductivity type body region 205 .

[0068] For example, an N-type source region 206 may be formed in the P-type body region 205 by photolithography and ion implantation. In this step, a P-type contact region 207 may be formed in the N-type source region 206 by ion implantation to facilitate subsequent electrical extraction of the N-type source region 206.

[0069] like Fig.10 As shown, step 9 is then performed to form a gate structure 208 on the first conductivity type source region 206 and the second conductivity type body region 205 .

[0070] like Fig.10 As shown, step 10) is finally performed to form an insulating layer 209 and an electrode lead structure 210.

[0071] It should be noted that, in the present embodiment, a first conductive type drain region 201 is formed in the second substrate 103, and a first conductive type drift region may also be formed on the first conductive type drain region 201. After the first conductive type drift is bonded to the first substrate 101, they jointly form the drift region of the super junction device, and a drain electrode 202 is also formed on the first conductive type drain region 201.

[0072] In this embodiment, the first conductivity type is N type, and the second conductivity type is P type. Of course, in other embodiments, the first conductivity type may also be P type, and the second conductivity type may also be N type.

[0073] like Fig.10 As shown, this embodiment also provides a super junction device, which includes: a first conductive type drain region 201; a super junction structure, located on the first conductive type drain region, including an N-type column 203 and a P-type column 204 arranged in sequence, and the morphology of the N-type column 203 and the P-type column 204 are both roughly rectangular; a second conductive type body region 205, formed on the super junction structure; a first conductive type source region 206, formed in the second conductive type body region 205; a gate structure 208, formed on the first conductive type source region 206 and the second conductive type body region 205; an insulating layer 209 and an electrode lead-out structure 210, located on the first conductive type source region 206 and the gate structure 208.

[0074] In this embodiment, the super junction device further includes a second conductivity type contact region 207 formed in the first conductivity type source region 206 .

[0075] In this embodiment, the depth of the super junction structure is between 30 and 45 microns.

[0076] In this embodiment, the first conductivity type is N type, and the second conductivity type is P type. Of course, in other embodiments, the first conductivity type may also be P type, and the second conductivity type may also be N type.

[0077] As described above, the super junction device and the manufacturing method of the present invention have the following beneficial effects:

[0078] The present invention bonds a first substrate 101 having an inverted trapezoidal groove 102 formed by etching to a second substrate 103, thins the back side to expose the bottom of the inverted trapezoidal groove 102, and then etches from the bottom of the groove 102 with a smaller width to increase the size of the bottom of the groove 102, thereby making the groove 102 rectangular, thereby reducing the charge difference between the P-type column 204 and the N-type column 203 in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.

[0079] The present invention uses a hard mask 106 having the same pattern as that of the inverted trapezoidal groove 102 to directly etch the bottom of the inverted trapezoidal groove 102 to make the groove 102 rectangular, without the need for photolithography, which can greatly save process costs.

[0080] The present invention thins the substrate by chemical mechanical grinding, oxidation, and removal of the oxide layer. Compared with direct grinding to reveal the groove 102, the retained support layer 104 can provide support for the groove 102 and its sidewalls during grinding, which can effectively avoid the risk of collapse of the sidewalls of the groove 102 that is easily caused by direct grinding to reveal the groove 102, thereby improving process stability.

[0081] The super junction device manufactured by the present invention has the advantages of high process stability and strong voltage resistance.

[0082] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.

[0083] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for manufacturing a super junction device, It is characterized in that The production method comprises: 1) providing a first substrate, wherein the first substrate comprises a first main surface and a second main surface opposite to each other, and etching a groove on the first main surface of the first substrate by a photolithography-etching process based on a photomask, wherein the groove is in an inverted trapezoidal shape; 2) providing a second substrate, and bonding the first main surface of the first substrate to the second substrate; 3) thinning the first substrate from the second main surface of the first substrate so that a supporting layer is retained between the second main surface of the first substrate and the groove; 4) oxidizing the support layer to form an oxide layer, and removing the oxide layer by etching to expose the groove; 5) Based on a hard mask plate having the same photomask pattern as that of step 1), after aligning the hard mask plate with the trench, directly etching the bottom of the trench to increase the bottom width of the trench so that the morphology of the trench is roughly rectangular; 6) The first substrate is doped with a first conductivity type, and a semiconductor material layer doped with a second conductivity type is filled in the trench to form a super junction structure together with the first substrate.

2. The method for manufacturing a super junction device according to claim 1, Features: The bottom width of the groove in step 1) is between one quarter and three quarters of the top width.

3. The method for manufacturing a super junction device according to claim 1, Features: The depth of the groove is between 1 and 50 micrometers.

4. The method for manufacturing a super junction device according to claim 3, Features: The depth of the groove is between 30 and 45 microns.

5. The method for manufacturing a super junction device according to claim 1, Features: The etching method of step 1) and step 5) includes one of reactive ion etching (RIE) and deep silicon etching (ICP).

6. The method for manufacturing a super junction device according to claim 1, Features: In step 3), the first substrate is thinned by a chemical mechanical polishing process, and the thickness of the support layer after thinning is between 0.5 microns and 2 microns.

7. The method for manufacturing a super junction device according to claim 1, Features: Also includes the steps: 7) forming a second conductivity type body region on the super junction structure; 8) forming a first conductivity type source region in the second conductivity type body region; 9) Fabricating a gate structure on the first conductive type source region and the second conductive type body region; 10) forming an insulating layer and an electrode lead structure; Wherein, the second substrate includes a first conductivity type drain region.

8. The method for manufacturing a super junction device according to claim 7, Features: Step 8) also includes the step of forming a second conductivity type contact region in the first conductivity type source region.

9. The method for manufacturing a super junction device according to any one of claims 1, 7 to 8, Features: The first conductivity type is N type and the second conductivity type is P type, or the first conductivity type is P type and the second conductivity type is N type.