Crosslinking agent, microemulsion, polymer microspheres and preparation methods and applications thereof
Polyacrylamide polymer microspheres prepared by temperature-sensitive crosslinking agent solve the problem of excessive swelling of existing polymer microspheres, realize selective swelling and sealing at the depth of the reservoir, and improve the three oil production in the oil field Adjust the anatomy and block the water effect.
Patent Information
- Application Number
- CN202210292503.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-03-23
AI Technical Summary
Existing polyacrylamide polymer microspheres swell too quickly when used as dissecting agents, making it difficult to enter deeper reservoir formations, and the crosslinking structure is too hydrophilic, resulting in poor sealing effect in medium and low formations. good.
The polyacrylamide polymer microspheres formed by cross-polymerization of acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and other monomers have the characteristics of ester bond fracture. As the formation temperature increases, the microspheres are small in medium and low formations, and enter the deep layer through the pore throat, and achieve intelligent swelling sealing in high temperature environments.
The selective swelling of polymer microspheres at the depth of the reservoir is achieved, which improves the dissection and water blocking effect in the three oil productions in the oil field, and reduces the oil displacement cost.
Smart Images

Figure CN114634426B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil reservoir exploitation, and in particular to a cross-linking agent for preparing a plugging agent in oil reservoir exploitation, polymer microspheres formed therefrom, and applications of the plugging performance thereof in formations. Background Art
[0002] With the increasing demand for crude oil due to industrialization, crude oil resources in major domestic oil fields have become increasingly scarce after primary and secondary oil recovery. The natural decline in crude oil production in my country is the primary problem faced by old oil fields. Nowadays, some large oil fields have entered the stage of tertiary oil recovery, the purpose of which is to increase the yield of remaining heavy oil and high-viscosity oil in the process of extracting remaining crude oil and reduce the cost of extracting remaining crude oil.
[0003] The problem that my country's oil fields are facing in the third recovery is that after a large amount of water flooding, some oil field strata have poor geological conditions and coexistence of high and low permeability layers, and crude oil in the low permeability layer is difficult to recover. Ineffective injection of profile control agents will damage the pore size of the oil field, reduce the crude oil yield of the oil field, and increase the cost of oil recovery. Therefore, there is a need for profile control technology that can effectively selectively plug strata with different permeabilities according to the reservoir environment.
[0004] Since the 1960s, people have begun to use bulk-expanded polyacrylamide polymer microgels as profile control agents. The plugging mechanism of this type of profile control agent is mainly physical plugging, which achieves the purpose of reducing permeability and plugging high aquifers through the adsorption and mechanical capture effect of polymer microgel balls in porous formations. Bulk-expanded polyacrylamide microspheres swell when exposed to water, which enhances their plugging ability and can swell and plug deep fractures and large pores.
[0005] At present, polymer microsphere profile control technology is an important technical research direction for increasing crude oil yield. Most of the polyacrylamide polymer microspheres currently used for profile control on the market use N,N'-methylenebisacrylamide (MBA) as a covalent cross-linking cross-linking agent. The problem is that the cross-linked structure of the polymer microspheres is too hydrophilic, and once it comes into contact with water, it will swell uncontrollably and quickly, and it is easy to break by shear. At the same time, during the swelling process, the mutual adhesion between the microspheres will cause the microspheres to agglomerate, resulting in the polymer microspheres swelling too fast in the early stage, blocking in the middle and low formations, and having difficulty entering the deeper reservoir formations.
[0006] Therefore, improving the raw materials for preparing polyacrylamide-based bulk-swelling profile control agents such as cross-linking agents to prepare polymer microspheres, especially those that can penetrate deeper formations, has important application value for improving the tertiary recovery rate of oil fields. Summary of the invention
[0007] In view of the problem that polyacrylamide polymer microspheres swell too quickly when used as profile control agents and are difficult to enter deeper oil reservoirs, the inventors have found after in-depth research that the cross-linking agent of the structure shown in the following formula I provided in the present application is a temperature-sensitive compound. The cross-linking agent is used to cross-link and polymerize monomers having an acryl group such as acrylamide, acrylic acid, and 2-acrylamide-2-methylpropane sulfonic acid to form polyacrylamide polymer microspheres. In the early stage of the microspheres in the middle and low formations, the volume is small or only slightly deformed and passes through the pore throat. Subsequently, as the formation goes deeper, the formation temperature becomes higher, and the high temperature environment causes the microspheres to absorb water with a high swelling rate, which can achieve intelligent swelling and plugging, thereby completing the present invention.
[0008] The crosslinking agent of the present invention is solid, has no irritating odor, and is easy to prepare. The crosslinking agent has the advantages of being temperature sensitive and having good water solubility. When the polyacrylamide polymer microspheres polymerized by the crosslinking agent are applied to the profile control and water plugging in the deep part of the oil reservoir in tertiary oil recovery, as the formation goes deeper, the formation temperature becomes higher, and the ester bond in the crosslinking agent shown in the following formula II is broken, the crosslinking degree of the polymer microspheres is reduced, and the water absorption and swelling ratio is higher.
[0009]
[0010] The polyacrylamide polymer microspheres prepared by using the crosslinking agent of the present invention have the advantage of increasing swelling ratio of the microspheres with increasing temperature at 25-150°C, and can realize environmental selective swelling of the polymer microspheres. They are particularly suitable for use in profile control and water plugging in deep reservoirs in tertiary oil recovery.
[0011] The present invention includes the following technical solutions.
[0012] [1] A cross-linking agent of formula I:
[0013]
[0014] In formula I, X is selected from a single bond, -O-, -COO-, -OCO-, -CO 3 -, -NHCO-, -CONH-, -NHCONH-, -(CH 2 ) m -、-O(CH 2 ) m -、-(CH 2 ) m O(CH 2 ) n -、-(CH 2 CH 2 O) m -、-(CH 2 ) m (CH 2 CH2 O) n -、-(CH 2 ) m (CH 2 CH 2 O) n O-、-(CH 2 ) m (OCH 2 CH 2 ) n O-, -COO(CH 2 ) m -、-OCO(CH 2 ) m -、-(CH 2 ) m COO(CH 2 ) n -、-(CH 2 ) m OCO(CH 2 ) n -、-CO 3 (CH 2 ) m -、-(CH 2 ) m CO 3 (CH 2 ) n -、-NHCO(CH 2 ) m -、-CONH(CH 2 ) m -、
[0015] -(CH 2 ) m NHCO(CH 2 ) n -、-(CH 2 ) m CONH(CH 2 ) n -、-NHCONH(CH 2 ) m -、
[0016] -(CH 2 ) m NHCONH(CH 2 ) n -、or、-(CH 2 ) m NHCO(CH 2 ) n O-, wherein m and n are each independently 1, 2, 3, 4, 5, 6, 7 or 8;
[0017] Y is selected from a single bond, -O-, -COO-, -OCO-, -CO 3 -, -NHCO-, -CONH-, -NHCONH-, -(CH 2 ) j -, -O(CH 2 ) j -, -(CH 2 ) j O(CH 2 ) k -, -(CH 2 CH 2 O) j -, -(CH 2 ) j (CH 2 CH 2 O) k -, -(CH 2 ) j (CH 2 CH 2 O) k O-, -(CH 2 ) j (OCH 2 CH 2 ) k O-, -COO(CH 2 ) j -, -OCO(CH 2 ) j -, -(CH 2 ) j COO(CH 2 ) k -, -(CH 2 ) j OCO(CH 2 ) k -, -CO 3 (CH 2 ) j -, -(CH 2 ) j CO 3 (CH 2 ) k -, -NHCO(CH 2 ) j -, -CONH(CH 2 ) j -, -(CH 2 ) j NHCO(CH 2 ) k -, -(CH 2 ) jCONH(CH 2 ) k -、-NHCONH(CH 2 ) j -、-(CH 2 ) j NHCONH(CH 2 ) k -、or、-(CH 2 ) j NHCO(CH 2 ) k O-, wherein j and k are each independently 1, 2, 3, 4, 5, 6, 7 or 8;
[0018] R 1 , R 2 Each independently selected from CH 2 =CHCH 2 -、CH 2 =C(CH 3 )CH 2 -、CH 3 CH=CHCH 2 -、CH 2 =CHCH(CH 3 )-、CH 2 =CHCOO-, CH 2 =C(CH 3 )COO- and CH 3 The group composed of CH=CHCOO-.
[0019] [2] The cross-linking agent according to [1], wherein the R 1 , R 2 Each independently selected from CH 2 =CHCH 2 -、CH 2 =C(CH 3 )CH 2 -、CH 2 =CHCOO- and CH 2 =C(CH 3 )COO-composed group.
[0020] [3] The cross-linking agent according to [1] or [2], wherein
[0021] The aforementioned X is selected from a single bond, -O-, -(CH 2 ) m -、-O(CH 2 ) m -、-(CH 2 ) m O(CH 2 )n - and - (CH 2 CH 2 O) m -, wherein m and n are each independently 1, 2, 3, 4, 5, 6, 7 or 8;
[0022] The aforementioned Y is selected from a single bond, -O-, -(CH 2 ) j -、-O(CH 2 ) j -、-(CH 2 ) j O(CH 2 ) k - and - (CH 2 CH 2 O) j -, wherein j and k are each independently 1, 2, 3, 4, 5, 6, 7 or 8.
[0023] [4] The cross-linking agent according to any one of [1] to [3], which is selected from the group consisting of the following structural formulas:
[0024]
[0025] [5] A microemulsion for preparing polymer microspheres, comprising an aqueous phase and an oil phase,
[0026] The aqueous phase contains the crosslinking agent described in any one of [1] to [4] and a crosslinking monomer, wherein the crosslinking monomer contains acrylamide and at least one selected from acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid.
[0027] [6] The microemulsion according to [5], wherein the mass ratio of the crosslinking agent to the crosslinking monomer is 0.1-1:0.1-40.
[0028] [7] The microemulsion according to [5] or [6], wherein the oil phase contains a continuous phase and an emulsifier, the continuous phase contains at least one of white oil, liquid paraffin, isooctane, and kerosene, and the emulsifier contains at least one of Span 80 and Tween 40.
[0029] [8] A polymer microsphere prepared using the microemulsion described in any one of [5] to [7] as a raw material.
[0030] [9] A method for preparing the polymer microspheres described in [8], comprising:
[0031] The cross-linking agent described in any one of [1] to [4] and a cross-linking monomer containing acrylamide and at least one selected from acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid are uniformly mixed in a ratio of cross-linking agent: cross-linking monomer = 0.1-1: 0.1-40 parts by weight, and the pH is adjusted to 7 with sodium hydroxide solution. After the pH is cooled to room temperature, an inert gas is introduced to prepare an aqueous precursor solution for standby use;
[0032] Adding an emulsifier to a continuous phase containing at least one of white oil, liquid paraffin, isooctane and kerosene, stirring for 10 to 30 minutes while passing an inert gas to perform pre-emulsification to obtain an oil phase precursor solution, wherein the mass ratio of the emulsifier to the continuous phase is 1:40 to 1:8;
[0033] While passing an inert gas into the aforementioned oil phase precursor solution, slowly drip the aforementioned water phase precursor solution, stir and mix evenly, heat to 40-60° C., and then slowly drip an initiator to carry out a polymerization reaction for 2-6 hours to generate the aforementioned polymer microspheres.
[0034]
[10] An application of the polymer microspheres described in [9] in profile control and water plugging in deep oil reservoirs during tertiary oil recovery. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the scanning electron microscope of the polymer microsphere 1 prepared in Example 2.
[0036] Figure 2 The diagram is a microscope observation of the swelling of polymer microspheres 1 prepared in Example 2 at different temperatures.
[0037] Figure 3 3 is a shear viscosity diagram of the polymer microspheres 2 prepared in Example 4 at different temperatures.
[0038] Figure 4 This is a diagram showing the change in blocking pressure of a solution of polymer microspheres 3 on the filter membrane.
[0039] Figure 5 It is a schematic diagram of the swelling ratio of the polymer microsphere 1 prepared in Example 2 and the polymer microsphere prepared in the comparative example at different temperatures.
[0040] Figure 6 is a schematic diagram of the device used in the plugging performance test.
[0041] 1. Beaker; 2. Beaker; 3. Valve; 4. Valve; 5. Peristaltic pump; 6. Pressure gauge; 7. Beaker; 8. Filter membrane holder. DETAILED DESCRIPTION
[0042] [Crosslinking agent]
[0043] The crosslinking agent of the present invention is shown in Formula I below.
[0044]
[0045] In formula I, X is selected from a single bond, -O-, -COO-, -OCO-, -CO 3 -, -NHCO-, -CONH-, -NHCONH-, -(CH 2 ) m -、-O(CH 2 ) m -、-(CH 2 ) m O(CH 2 ) n -、-(CH 2 CH 2 O) m -、-(CH 2 ) m (CH 2 CH 2 O) n -、-(CH 2 ) m (CH 2 CH 2 O) n O-、-(CH 2 ) m (OCH 2 CH 2 ) n O-, -COO(CH 2 ) m -、-OCO(CH 2 ) m -、-(CH 2 ) m COO(CH 2 ) n -、-(CH 2 ) m OCO(CH 2 ) n -、-CO 3 (CH 2 ) m -、-(CH 2 ) m CO 3 (CH 2 ) n -、-NHCO(CH 2 ) m -、-CONH(CH 2 ) m -、-(CH 2 ) mNHCO(CH 2 ) n -、-(CH 2 ) m CONH(CH 2 ) n -、-NHCONH(CH 2 ) m -、-(CH 2 ) m NHCONH(CH 2 ) n -、or、-(CH 2 ) m NHCO(CH 2 ) n O-, wherein m and n are each independently 1, 2, 3, 4, 5, 6, 7 or 8;
[0046] Y is selected from a single bond, -O-, -COO-, -OCO-, -CO 3 -, -NHCO-, -CONH-, -NHCONH-, -(CH 2 ) j -、-O(CH 2 ) j -、-(CH 2 ) j O(CH 2 ) k -、-(CH 2 CH 2 O) j -、-(CH 2 ) j (CH 2 CH 2 O) k -、-(CH 2 ) j (CH 2 CH 2 O) k O-、-(CH 2 ) j (OCH 2 CH 2 ) k O-, -COO(CH 2 ) j -、-OCO(CH 2 ) j -、-(CH 2 ) j COO(CH 2 ) k -、-(CH 2 ) j OCO(CH2 ) k -、-CO 3 (CH 2 ) j -、-(CH 2 ) j CO 3 (CH 2 ) k -、-NHCO(CH 2 ) j -、-CONH(CH 2 ) j -、-(CH 2 ) j NHCO(CH 2 ) k -、-(CH 2 ) j CONH(CH 2 ) k -、-NHCONH(CH 2 ) j -、-(CH 2 ) j NHCONH(CH 2 ) k -、or、-(CH 2 ) j NHCO(CH 2 ) k O-, wherein j and k are each independently 1, 2, 3, 4, 5, 6, 7 or 8;
[0047] R 1 , R 2 Each independently selected from CH 2 =CHCH 2 -、CH 2 =C(CH 3 )CH 2 -、CH 3 CH=CHCH 2 -、CH 2 =CHCH(CH 3 )-、CH 2 =CHCOO-, CH 2 =C(CH 3 )COO- and CH 3 The group composed of CH=CHCOO-.
[0048] By using the cross-linking agent described in the aforementioned formula I, the cross-linking agent can be used to cross-link and polymerize with a monomer having an acryloyl group such as acrylamide to form polyacrylamide polymer microspheres. When the polymer microspheres are used for profile control and water plugging in deep oil reservoirs in tertiary oil recovery, the polymer microspheres only undergo slight deformation in the middle and low formations with low temperatures, and have a small volume, and can pass through the pore throats of the middle and low formations. Subsequently, as the formation goes deeper, the formation temperature becomes higher, and the high temperature environment triggers the ester bond from the cross-linking agent in the microspheres to break, and the cross-linking degree of the polymer microspheres is reduced, thereby having a higher water absorption and swelling ratio, and exerting a plugging effect. Thus, the polymer microspheres prepared by using the cross-linking agent of the present invention can achieve different water absorption and swelling ratios according to changes in formation temperature, and can enter deep formations to achieve the effect of profile control and water plugging.
[0049] Among the aforementioned cross-linking agents, preferably, the aforementioned R 1 , R 2 Each independently selected from CH 2 =CHCH 2 -、CH 2 =C(CH 3 )CH 2 -、CH 2 =CHCOO- and CH 2 =C(CH 3 )COO-composed group.
[0050] Among the above cross-linking agents, from the perspective of better exerting the effect of profile control and water plugging in the polyacrylamide polymer microspheres, preferably, the above X is selected from a single bond, -O-, -(CH 2 ) m -、-O(CH 2 ) m -、-(CH 2 ) m O(CH 2 ) n - and - (CH 2 CH 2 O) m -, wherein m and n are each independently 1, 2, 3, 4, 5, 6, 7 or 8.
[0051] Among the above cross-linking agents, from the perspective of better exerting the effect of profile control and water plugging in the polyacrylamide polymer microspheres, preferably, the above Y is selected from a single bond, -O-, -(CH 2 ) j -、-O(CH 2 ) j -、-(CH 2 ) j O(CH 2 ) k - and - (CH2 CH 2 O) j -, wherein j and k are each independently 1, 2, 3, 4, 5, 6, 7 or 8.
[0052] Among the aforementioned cross-linking agents, from the perspective of better exerting the effect of profile control and water plugging in the polyacrylamide polymer microspheres, preferably, they are selected from the group consisting of the following structural formulas:
[0053]
[0054] [Microemulsion]
[0055] The microemulsion of the present invention is used for preparing polymer microspheres, and comprises an aqueous phase and an oil phase. The aqueous phase of the microemulsion contains the aforementioned crosslinking agent and crosslinking monomer. The aforementioned crosslinking monomer contains acrylamide and at least one selected from acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid.
[0056] The cross-linking monomers may contain other components in addition to acrylamide, acrylic acid, and 2-acrylamido-2-methylpropanesulfonic acid, as long as they do not hinder the formation of polyacrylamide polymers. There is no particular limitation on the proportion of each component in the cross-linking monomer, and those skilled in the art can make appropriate adjustments according to the desired properties of the polymer microspheres.
[0057] In the aqueous phase of the microemulsion, the crosslinking agent of the present invention may be used in combination with other crosslinking agents such as MBA.
[0058] In the aqueous phase of the microemulsion, the mass ratio of the crosslinking agent to the crosslinking monomer may be, for example, in the range of 0.1-1:0.1-40.
[0059] An example of the aqueous phase composition of the microemulsion includes 0.1 to 20 parts by mass of acrylamide, 0.1 to 20 parts by mass of acrylic acid, 0.1 to 2 parts of 2-acrylamido-2-methylpropanesulfonic acid, 0.1 to 1 part of the crosslinking agent, and 0.1 to 1 part of an MBA crosslinking agent.
[0060] In the aforementioned microemulsion, the aforementioned oil phase contains a continuous phase and an emulsifier. The aforementioned continuous phase can include, for example, white oil, liquid paraffin, isooctane, and kerosene. The aforementioned continuous phase can contain at least one of white oil, liquid paraffin, isooctane, and kerosene. In addition to the aforementioned white oil, liquid paraffin, isooctane, and kerosene, the aforementioned continuous phase can also contain other oil substances as a continuous phase.
[0061] The emulsifier may be, for example, Span and Tween, but is not particularly limited. Preferably, at least one of Span 80 and Tween 40 is contained.
[0062] In the aforementioned microemulsion, there is no particular limitation on the ratio of the aqueous phase to the oil phase, and those skilled in the art can appropriately set the ratio according to needs.
[0063] [Polymer microspheres]
[0064] The polymer microspheres of the present invention are prepared using the aforementioned microemulsion as raw material.
[0065] The aqueous phase of the aforementioned microemulsion contains the aforementioned cross-linking agent of the present invention, so the prepared polymer microspheres contain the ester bonds possessed by the aforementioned cross-linking agent (as shown by the dotted line in the formula II described later). When the polymer microspheres are applied to the deep profile control and water plugging of the reservoir in tertiary oil recovery, when in the middle and low formations, the formation temperature is low, the ester bonds in the cross-linking agent remain connected, the cross-linking degree of the polymer microspheres is high, and the absorption and swelling ratio is low, so that the polymer microspheres are small in volume or only slightly deformed, and can pass through the pore throats in the middle and low formations to reach deeper formations. As the formation goes deeper, the formation temperature becomes higher, so that the ester bonds in the cross-linking agent are broken, the cross-linking degree of the polymer microspheres is reduced, and they have a higher water absorption and swelling ratio, thereby achieving the effect of achieving profile control and water plugging in deeper formations.
[0066]
[0067] The polymer microspheres of the present invention have the advantage that the microsphere swelling ratio increases with temperature within the range of 25-150°C, and can achieve environmental selective swelling of the polymer microspheres. Therefore, the polymer microspheres of the present invention are particularly suitable for use in profile control and water plugging in deep reservoirs in tertiary oil recovery.
[0068] The polymer microspheres of the present invention have a water absorption rate of, for example, 5 to 20 times the mass equivalent at 25° C., and when the temperature rises to, for example, 140° C., the water absorption rate increases to, for example, 120 to 200 times the mass equivalent.
[0069] [Method for preparing polymer microspheres]
[0070] The method for preparing polymer microspheres of the present invention comprises the following steps:
[0071] The crosslinking agent of the present invention and the crosslinking monomer are mixed uniformly in a ratio of 0.1-1:0.1-40 parts by weight, and the pH is adjusted to 7 with a sodium hydroxide solution. After the solution is cooled to room temperature, an inert gas is introduced to prepare an aqueous precursor solution for standby use. The crosslinking monomer contains acrylamide and at least one selected from acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid.
[0072] Adding an emulsifier to a continuous phase containing at least one of white oil, liquid paraffin, isooctane and kerosene, stirring for 10 to 30 minutes while passing an inert gas to perform pre-emulsification to obtain an oil phase precursor solution, wherein the mass ratio of the emulsifier to the continuous phase is 1:40 to 1:8;
[0073] While passing an inert gas into the aforementioned oil phase precursor solution, slowly drip the aforementioned water phase precursor solution, stir and mix evenly, heat to 40-60° C., and then slowly drip an initiator to carry out a polymerization reaction for 2-6 hours to generate the aforementioned polymer microspheres.
[0074] In the above-mentioned method for preparing polymer microspheres, the concentration of the sodium hydroxide solution used for adjusting the pH can be, for example, 1 M, or other concentrations can be selected without particular limitation.
[0075] In the above-mentioned method for preparing polymer microspheres, the above-mentioned inert gas can be, for example, nitrogen, argon, etc., without particular limitation. The purpose of introducing the inert gas is to remove oxygen in the reaction environment.
[0076] In the aforementioned step of preparing the aqueous precursor solution, the time for passing the inert gas may be, for example, 20 minutes to 2 hours, or may be, for example, 30 minutes to 60 minutes.
[0077] In the aforementioned preparation step of the oil phase precursor, the aforementioned continuous phase may contain, in addition to white oil, liquid paraffin, isooctane, and kerosene, other oil substances that can serve as a continuous phase. The aforementioned stirring may be, for example, mechanical stirring, magnetic stirring, etc., and may be stirred at a speed of, for example, 600-1200 r / min. The aforementioned pre-emulsification time may be, for example, 10 to 60 minutes, and further, for example, 10 to 30 minutes.
[0078] There is no particular limitation on the aforementioned initiator. For example, it can be selected from at least one of the initiators listed in (1) to (2). Furthermore, a co-initiator listed in (3) to (4) can be added to accelerate the process of the initiator generating free radicals to initiate polymerization.
[0079] (1) 0.001% to 0.5% potassium persulfate, ammonium persulfate, or persulfated hydrochloric acid;
[0080] (2) 0.001% to 0.5% azobisisobutyronitrile;
[0081] (3) 0.001% to 0.5% sodium bisulfite, potassium bisulfite, sodium thiosulfate;
[0082] (4) 0.001% to 0.5% of tetramethylethylenediamine, dimethylethylenediamine or ethylenediamine.
[0083] [Application of polymer microspheres]
[0084] The polymer microspheres of the present invention can be used for profile control and water plugging in deep oil reservoirs during tertiary oil recovery. The polymer microspheres of the present invention are injected into formation oil reservoirs to achieve swelling, profile control and water plugging in the formation. In the middle and low formations, the formation temperature is low, the ester bonds from the cross-linking agent in the polymer microspheres remain connected, the polymer microspheres have a high degree of cross-linking, and the absorption swelling ratio is low, so that the polymer microspheres are small in size or only slightly deformed, and can pass through the pore throats in the middle and low formations to reach deeper formations. As the formation goes deeper, the formation temperature becomes higher, the ester bonds break, the cross-linking degree of the polymer microspheres decreases, and the moisture outside the microspheres penetrates into the inner cavity of the microspheres, achieving temperature-sensitive swelling of the microspheres, thereby achieving the effect of profile control and water plugging in deeper formations.
[0085] Example
[0086] In order to explain the present disclosure more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0087] In this manual, unless otherwise specified, percentages refer to mass percentages, temperatures are in degrees Celsius (℃), and the specific meanings of other symbols and test conditions are as follows:
[0088] Example 1: Synthesis of the cross-linking agent shown in Formula I-1
[0089]
[0090] In a 250mL single-necked flask, hydrazine hydrate (0.5g 10mmol) is dissolved in water and tetrahydrofuran mixed solvent (30mL:10mL). Allyl chloroformate (2.4g 20mmol) is dissolved in 10mL tetrahydrofuran, and allyl chloroformate solution is slowly added to the mixed solution of hydrazine hydrate using a constant pressure dropping funnel. The ice bath magnetic stirring reaction is 6 hours, and then the tetrahydrofuran in the mixed solution is removed by rotary evaporator concentration evaporation. Use DCM (50mL) to extract the remaining aqueous solution after rotary evaporation 3 times, purify and obtain the DCM layer of lower floor. The solvent in the spin-dried product is obtained to obtain cross-linking agent I-1.
[0091] NMR data of crosslinker I-1: 1 H NMR (500MHz, Chloroform-d) δ7.59 (s, 1H), 5.98–5.85 (m, 1H), 5.34–5.23 (m, 2H), 4.60 (dt, J = 5.9, 1.0Hz, 2H).
[0092] Example 2: Preparation of polymer microspheres 1
[0093] 16 g of acrylamide, 2 g of acrylic acid, 2 g of 2-acrylamido-2-methylpropanesulfonic acid, and 0.1 g of the crosslinking agent represented by formula I-1 prepared in Example 1 were dissolved in 20 mL of water. A 1 M NaOH aqueous solution was used to adjust the pH value of the solution to 7. After passing argon gas for 60 minutes, an aqueous precursor solution was obtained.
[0094] 80g of liquid paraffin was placed in a 500mL three-necked flask, and 8g of Span 80 and 4g of Tween 40 were added to the three-necked flask. Argon was continuously introduced and mechanical stirring was performed at 800r / min. After pre-emulsification for 30 minutes, an oil phase precursor solution was obtained.
[0095] The aqueous precursor solution was slowly added to the oil precursor solution using a constant pressure dropping funnel. After mixing for 30 minutes, the stirring speed was adjusted to 400 r / min, and the reaction temperature was raised to 40° C. The emulsion polymerization reaction was performed for 3 hours to obtain a polymer microsphere suspension emulsion.
[0096] The suspended emulsion was poured into 200 mL of ethanol and stirred evenly to break the emulsion. The suspension after demulsification was filtered to obtain polymer microspheres. The polymer microspheres were washed three times with 200 mL of ethanol and filtered under reduced pressure to obtain powdered polymer microspheres. The powdered polymer microspheres were placed in a 30°C constant temperature oven and dried for 48 hours to obtain dehydrated particles of polymer microspheres 1. Figure 1 Schematic diagram of the prepared polymer microsphere 1 by scanning electron microscope. Figure 2 It is a picture of the swelling of polymer microsphere 1 at different temperatures observed under a microscope.
[0097] Example 3: Synthesis of the cross-linking agent shown in Formula I-2
[0098]
[0099] 2.16 g of 2-methyl-2-propen-1-ol (30 mmol) was dissolved in 30 mL of DCM, and triphosgene (2.361 g 12 mmol) at 0° C. Pyridine (2.37 g 30 mmol) was added dropwise, and stirring was continued at room temperature for 1 hour to obtain compound 3a.
[0100] In a 250mL single-necked flask, hydrazine hydrate (0.5g 10mmol) was dissolved in a mixed solvent of water and tetrahydrofuran (the volume ratio of water to tetrahydrofuran was 30mL:10mL, respectively). Compound 3a (2.4g 20mmol) was dissolved in 10mL tetrahydrofuran, and the 3a solution was slowly added to the mixed solution of hydrazine hydrate using a constant pressure dropping funnel. The reaction was stirred with an ice bath magnet for 6 hours, and then the tetrahydrofuran in the mixed solution was concentrated and evaporated using a rotary evaporator. The aqueous solution was extracted 3 times with DCM (50mL) and purified to obtain a DCM layer in the lower layer. The solvent in the product was spin-dried to obtain a cross-linking agent shown in Formula I-2.
[0101] The NMR data of the cross-linking agent shown in formula I-2: 1 H NMR (500MHz, Chloroform-d) δ7.75(s,1H),5.08(dp,J=2.4,1.1Hz,1H),4.95(tq,J=2.0,1.1Hz,1H),4.56(t,J=1.0Hz,2H),1.78(d,J=2.5Hz,1H).
[0102] Example 4: Preparation of polymer microspheres 2:
[0103] 16 g of acrylamide, 2 g of acrylic acid, 2 g of 2-acrylamido-2-methylpropanesulfonic acid, and 0.1 g of the crosslinking agent of formula I-2 prepared in Example 3 were dissolved in 20 mL of water. A 1 M NaOH aqueous solution was used to adjust the pH value of the solution to 7. After passing argon gas for 60 minutes, an aqueous precursor solution was obtained.
[0104] 80 g of liquid paraffin was placed in a 500 mL three-necked flask, and 8 g of Span 80 and 4 g of Tween 40 were added to the three-necked flask. Argon was continuously introduced, and mechanical stirring was performed at 800 r / min for 30 minutes for pre-emulsification to obtain an oil phase precursor solution.
[0105] The aqueous precursor solution was slowly added to the oil precursor solution using a constant pressure dropping funnel. After mixing for 30 minutes, the stirring speed was adjusted to 400 r / min, and the reaction temperature was raised to 40° C. The emulsion polymerization reaction was carried out for 3 hours to obtain a polymer microsphere suspension emulsion.
[0106] The above-mentioned suspension emulsion was poured into 200 mL of ethanol and stirred evenly to break the emulsion. The suspension after demulsification was filtered to obtain polymer microspheres. It was washed with ethanol (200 mL) and filtered under reduced pressure for 3 times to obtain a powdered product of polymer microspheres. It was placed in a 30°C constant temperature oven and dried for 48 hours to obtain particles of dehydrated polymer microspheres 2. Figure 3 The shear viscosity diagram of the prepared polymer microspheres 2 at different temperatures is shown. Figure 3 It can be seen that under shear stress, the microsphere suspensions at different temperatures all show the physical property of "shear thinning", and the shear viscosity also increases with the increase of temperature. -1 At a shear rate of 1.5, the shear viscosity of the microsphere suspension at 25°C is 62.5 mPa·s, while the shear viscosity of the microsphere suspension at 140°C can reach 4.61×10 2 mPa·s, indicating that the microsphere suspension has a temperature-responsive viscosity-increasing effect.
[0107] Example 5: Synthesis of the cross-linking agent shown in Formula I-3
[0108]
[0109] 3.48 g of hydroxyethyl acrylate (30 mmol) was dissolved in 30 mL of ethyl acetate, triphosgene (2.361 g 12 mmol) at 0°C was added, and N,N-diethylaniline (4.47 g 30 mmol) was added dropwise, and stirred at room temperature for 3 hours to obtain the compound shown in Formula 5a.
[0110] In a 250mL single-mouth flask, hydrazine hydrate (0.5g 10mmol) is dissolved in a mixed solvent of water and tetrahydrofuran (the volume ratio of water to tetrahydrofuran is 30mL:10mL). The compound shown in Formula 5a (3.57g 20mmol) is dissolved in 10mL tetrahydrofuran and slowly added to the mixed solution of hydrazine hydrate using a constant pressure dropping funnel. The reaction is stirred with an ice bath magnet for 6 hours, and then the tetrahydrofuran in the mixed solution is removed by concentrated evaporation through a rotary evaporator. The aqueous solution is extracted 3 times using DCM (50mL), and the DCM layer of the lower layer is purified. The product is spin-dried for solvent to obtain the cross-linking agent shown in Formula I-3.
[0111] The NMR data of the cross-linking agent shown in formula I-3: 1 H NMR(500MHz,Chloroform-d)δ7.68(s,1H),6.13–6.01(m,2H),6.05–5.92(m,1H),4.45–4.30(m,4H).
[0112] Example 6: Preparation of polymer microspheres 3
[0113] 16 g of acrylamide, 2 g of acrylic acid, 2 g of 2-acrylamido-2-methylpropanesulfonic acid, and 0.1 g of the crosslinking agent of formula I-3 prepared in Example 5 were dissolved in 20 mL of water. A 1 M NaOH aqueous solution was used to adjust the pH value of the solution to 7. After passing argon gas for 60 minutes, an aqueous precursor solution was obtained.
[0114] 80g of liquid paraffin was placed in a 500mL three-necked flask, and 8g of Span 80 and 4g of Tween 40 were added to the three-necked flask. Argon was continuously introduced and mechanical stirring was performed at 800r / min. After pre-emulsification for 30 minutes, an oil phase precursor solution was obtained.
[0115] The aqueous precursor solution was slowly added to the oil precursor solution using a constant pressure dropping funnel. After mixing for 30 minutes, the stirring speed was adjusted to 400 r / min, and the reaction temperature was raised to 40° C. The emulsion polymerization reaction was carried out for 3 hours to obtain a polymer microsphere suspension emulsion.
[0116] The suspended emulsion was poured into 200 mL of ethanol and stirred evenly to break the emulsion. The suspension after demulsification was filtered to obtain polymer microspheres 3. The polymer microspheres 3 were washed with ethanol (200 mL) and filtered under reduced pressure for 3 times to obtain a powdered product of polymer microspheres 3. The polymer microspheres 3 were placed in a 30° C. constant temperature oven and dried for 48 hours to obtain dehydrated particles of polymer microspheres 3.
[0117] Example 7
[0118] Synthesis route of compound I-4:
[0119]
[0120] Synthesis and characterization of compound I-4:
[0121] 3.90 g of hydroxyethyl methacrylate (30 mmol) was dissolved in 30 mL of ethyl acetate, triphosgene (2.361 g 12 mmol) at 0°C was added, and NN-diethylaniline (4.47 g 30 mmol) was added dropwise, and the mixture was stirred at room temperature for 3 hours to obtain compound 7a.
[0122] In a 250mL single-mouth flask, hydrazine hydrate (0.5g 10mmol) is dissolved in water and tetrahydrofuran mixed solvent (30mL: 10mL). 7a compound (3.57g 20mmol) is dissolved in 10mL tetrahydrofuran, and 7a compound solution is slowly added to the mixed solution of hydrazine hydrate using a constant pressure dropping funnel. After 6 hours of stirring reaction with an ice bath magnet, the tetrahydrofuran in the mixed solution is concentrated and evaporated by a rotary evaporator. DCM (50mL) is used to extract and purify the aqueous solution three times to obtain the lower DCM layer. The product is spin-dried for solvent to obtain compound I-4.
[0123] NMR data of compound I-4: 1 H NMR(500MHz,Chloroform-d)δ7.68(s,2H),5.87(p,J=1.5Hz,1H),5.85(dt,J=1.7,0.9Hz,1H),5. 75(dq,J=1.9,0.9Hz,1H),5.69(dq,J=2.7,1.3Hz,1H),4.39–4.19(m,9H),1.96(d,J=2.9Hz,2H).
[0124] Example 8: Preparation of polymer microspheres 4
[0125] 16 g acrylamide, 2 g acrylic acid, 2 g 2-acrylamido-2-methylpropanesulfonic acid, and 0.1 g I-4 were dissolved in 20 mL water. 1 M NaOH aqueous solution was used to adjust the pH value of the solution to 7. After argon was introduced for 60 minutes, an aqueous precursor solution was obtained.
[0126] 80g of liquid paraffin was placed in a 500mL three-necked flask, and 8g of Span 80 and 4g of Tween 40 were added to the three-necked flask. Argon was continuously introduced and mechanical stirring was performed at 800r / min. After pre-emulsification for 30 minutes, an oil phase precursor solution was obtained.
[0127] The aqueous precursor solution was slowly added to the oil precursor solution using a constant pressure dropping funnel. After mixing for 30 minutes, the stirring speed was adjusted to 400 r / min, and the reaction temperature was raised to 40° C. The emulsion polymerization reaction was carried out for 3 hours to obtain a microsphere suspension emulsion.
[0128] The above-mentioned suspension emulsion was poured into 200 mL of ethanol and stirred evenly to break the emulsion. The suspension after demulsification was filtered to obtain polymer microspheres 4. It was washed three times with ethanol (200 mL) and filtered under reduced pressure to obtain a powdered product of polymer microspheres. The polymer microspheres were placed in a 30°C constant temperature oven and dried for 48 hours to obtain dehydrated particles of polymer microspheres 4.
[0129] Comparative Example 1
[0130] Polymer microspheres as a comparative example were prepared in the same manner as in Example 2, except that N,N′-methylenebisacrylamide (MBA) was used instead of the cross-linking agent represented by Formula I-1 used in Example 2.
[0131] For the polymer microspheres prepared in the aforementioned examples and comparative examples, the plugging performance test was performed as described below.
[0132] Plugging performance test
[0133] use Figure 6 The experimental device shown in the figure is used to test the plugging performance by high pressure difference microporous membrane filtration method. Specifically, Figure 6 In the figure, beakers 1 and 2 are connected to a filter membrane holder 8 through a conduit, a peristaltic pump 5 and a pressure gauge 6 are arranged in the middle, and valves 3 and 4 are used to control the conduction of the conduit.
[0134] The polymer microspheres prepared in the above-mentioned embodiments and comparative examples are respectively configured into a microsphere suspension with a mass concentration of 0.5% and placed in beaker 1, and deionized water is injected into beaker 2. The microporous filter membrane (not shown) set in the filter membrane holder 6 is moistened with deionized water, and then the valve of the beaker 2 filled with deionized water is opened, and the peristaltic pump is started to adjust the flow rate to 0.4mL / min. The timing starts when liquid drips out of the beaker 7 at the outlet. After 60 seconds, close valve 4, and open valve 3 of the beaker 1 on one side of the suspension of polymer microspheres for 60 seconds. Finally, close valve 3 and open valve 4 for 480 seconds. The pressure data measured by the pressure gauge 6 is recorded in real time. The pore size of the aforementioned microporous filter membrane is 10μm, and the pore size here refers to the average pore size of the membrane.
[0135] Figure 4 The figure shows the change of the plugging pressure obtained by the above plugging performance test using polymer microspheres 3. Figure 4 It can be seen that the microsphere suspension swollen at 140°C has a better plugging effect, and the plugging pressure can reach 0.1MPa, while the microsphere suspension swollen at 25°C and 100°C cannot achieve effective plugging in the experiment.
[0136] Swelling properties of polymer microspheres
[0137] For the polymer microspheres prepared in the examples and comparative examples, the swelling properties at different temperatures were tested as described below.
[0138] Weigh 200 mg of polymer microspheres 1 prepared in Example 2 and 5 portions of polymer microspheres prepared in Comparative Example 1, dissolve in 40 mL of water, and place in a 150 mL pressure bottle. Heat in an oil bath at 25°C, 130°C, 140°C, 150°C, and 160°C for 30 minutes, then place the microsphere suspension at room temperature to swell the polymer microspheres, and swell with water for 24 hours. Then filter and screen the swollen polymer microspheres using a 400-mesh sieve, and weigh the mass of the swollen microspheres m. t , calculate the swelling ratio at different temperatures according to the following swelling ratio calculation formula.
[0139] Swelling ratio = (m t -m 0 ) / m 0
[0140] Where m t is the mass of microspheres after swelling, m 0 is the initial mass of microsphere powder, fixed at 200 mg.
[0141] The calculated swelling ratios at different temperatures are shown in Figure 5 In. From Figure 5 It can be seen that the polymer microspheres of the comparative example have no temperature responsiveness, and the swelling ratios at different temperatures are between about 80 and 100 times. However, the polymer microspheres prepared in Example 2 have a small swelling ratio at relatively low temperatures (25°C, 130°C), only about 10 to 20 times, but the swelling ratio of the microspheres after high temperature treatment (140°C, 150°C, 160°C) is significantly increased, up to 180 times, showing obvious temperature-responsive swelling performance.
[0142] Obviously, the above embodiments of the present disclosure are merely examples for clearly illustrating the present disclosure, and are not limitations on the implementation methods of the present disclosure. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present disclosure are still within the protection scope of the present disclosure.
Claims
1. A microemulsion for preparing polymer microspheres, comprising an aqueous phase and an oil phase, in, The aqueous phase contains a crosslinking agent selected from the group consisting of the following structural formulas, and a crosslinking monomer, wherein the crosslinking monomer contains acrylamide and at least one selected from acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid, 2 . The microemulsion according to claim 1 , wherein the mass ratio of the crosslinking agent to the crosslinking monomer is 0.1-1:0.1-40.
3. The microemulsion according to claim 1, wherein The oil phase contains a continuous phase and an emulsifier, the continuous phase contains at least one selected from white oil, liquid paraffin, isooctane, and kerosene, and the emulsifier contains at least one selected from Span 80 and Tween 40.
4. A polymer microsphere prepared using the microemulsion according to any one of claims 1 to 3 as a raw material.
5. A method for preparing the polymer microspheres according to claim 4, comprising: A cross-linking agent selected from the group consisting of the following structural formulas and a cross-linking monomer containing acrylamide and at least one selected from acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid are uniformly mixed in a ratio of cross-linking agent: cross-linking monomer = 0.1-1: 0.1-40 parts by weight, and the pH is adjusted to 7 with a sodium hydroxide solution, and an inert gas is introduced into the solution after the pH is cooled to room temperature to be used as an aqueous precursor solution; Adding an emulsifier to a continuous phase containing at least one of white oil, liquid paraffin, isooctane and kerosene, stirring for 10 to 30 minutes while passing an inert gas to perform pre-emulsification to obtain an oil phase precursor solution, wherein the mass ratio of the emulsifier to the continuous phase is 1:40 to 1:8; While passing an inert gas into the oil phase precursor solution, slowly dripping the water phase precursor solution, stirring and mixing evenly, heating to 40-60° C., and then slowly dripping an initiator to carry out a polymerization reaction for 2-6 hours to generate the polymer microspheres; 6. Use of the polymer microspheres according to claim 4 in profile control and water plugging in deep oil reservoirs during tertiary oil recovery.
Citation Information
Patent Citations
Cross-linked polymer microsphere for oil displacement of oilfield and preparation method for cross-linked polymer microsphere
CN102603966A
Polymer microemulsion for deep profile control of oil reservoir
CN104558402A
Unsaturated diesters of hydrazodicarbonic acid and polymers thereof
US2583980A