Vinyl polymer / modified polyhydroxy polymer composites and their applications
Through the blending technology of vinyl polymer and modified polyhydroxy polymer composite, the problem of insufficient robustness of polyhydroxy polymer materials in ion exchange membranes is solved, and good mechanical properties under high temperature and high humidity conditions are achieved. and gas barrier properties, extending service life and being suitable for a variety of material applications.
Patent Information
- Application Number
- CN202210199459.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-02
AI Technical Summary
Existing polyhydroxy polymer materials in the field of ion exchange membranes have unsatisfactory robustness due to strong hydrophilicity and water solubility limitations, especially insufficient mechanical properties under high temperature and high humidity conditions, and difficulty in maintaining long-term service life.
A composite of vinyl polymer and modified polyhydroxy polymer is used to obtain a non-covalent cross-linked structure composite through a blending method, forming a hydrogen bond network to improve ion conductivity and barrier properties, and through "sacrificial bonds" ” mechanism extends service life.
It achieves good mechanical properties and gas barrier properties under high temperature and high humidity conditions, extends the service life of the ion exchange membrane, and has appropriate water absorption and antibacterial properties. It is suitable for fuel cells, biomedical materials and packaging materials.
Smart Images

Figure CN114634665B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a vinyl polymer / modified polyhydroxy polymer composite and application thereof. Background Art
[0002] Ethylene-vinyl alcohol copolymer (EVOH) is one of the three major barrier materials, and has excellent barrier properties against hydrogen, oxygen and hydrocarbons. In industry, ethylene-vinyl acetate copolymer is prepared by copolymerization of ethylene and vinyl acetate, and ethylene-vinyl alcohol copolymer is obtained by alcoholysis or saponification. Compared with polyvinyl alcohol (PVA), the introduction of ethylene structural units into EVOH suppresses the hydrophilicity of the polymer, and has better barrier properties in both dry and humid environments; improves the processing performance of the polymer; high saponification EVOH with a vinyl alcohol molar content of less than 25% has a water absorption rate of less than 25% at room temperature and is insoluble in water at any temperature.
[0003] Polyvinyl alcohol is obtained by alcoholysis or saponification of polyvinyl acetate. It has extremely high bulk density and crystallinity and has extremely strong barrier properties in a dry environment. Although the chemical composition of linear polyhydroxy polymers such as chitosan, cellulose, lignin, and polyethylene glycol is different from that of PVA, their similar topological structures and functional groups make them have similar applications in the fields of ion exchange membranes, biomedical materials, and packaging materials. Taking the application of PVA in ion exchange membranes as an example, its mechanism of action is mainly divided into two categories: the first category is to use the hydroxyl reaction activity in PVA for grafting functionalization modification to enable it to have the function of transporting ions; in the second category of research, PVA itself does not have the function of ion transport, and PVA is compounded with other polymers to prepare a composite ion exchange membrane. The role of PVA is mainly to improve the barrier properties, mechanical properties, and film-forming properties of the composite membrane. At the same time, the hydrogen bonding between the hydroxyl groups of PVA and other cationic functional groups can effectively improve the ion transport capacity of the composite membrane.
[0004] However, the biggest limitation of polyhydroxy polymer materials such as PVA, chitosan, cellulose, lignin, and polyethylene glycol in the application of ion exchange membranes and other membrane materials is their strong hydrophilicity and water solubility, while grafted functionalized polyhydroxy polymers will further enhance the hydrophilicity and water solubility of the materials. Although the hydrophilicity and water solubility of the materials can be suppressed by covalent cross-linking, due to the instability of the cross-linking structure, when applied to ion exchange membranes, especially ion exchange membranes used in the electrochemical field, such as fuel cell ion exchange membranes, electrodialysis membranes, alkaline primary or secondary battery separators, and water electrolysis membranes, the robustness is not ideal. Summary of the invention
[0005] In view of this, one object of the present invention is to propose a vinyl polymer / modified polyhydroxy polymer composite, which has a non-covalent cross-linked structure, is water-insoluble, has controllable water absorption, has good water vapor permeability, excellent gas barrier properties, and can maintain good mechanical properties under high temperature and high humidity conditions. It is suitable as an ion exchange membrane, a gas humidification membrane for a fuel cell humidification device, and a biomedical material and packaging material.
[0006] Another object of the present invention is to provide the application of the vinyl polymer / modified polyhydroxy polymer composite.
[0007] Another object of the present invention is to provide a composite membrane.
[0008] Another object of the present invention is to provide a method for preparing a composite membrane.
[0009] To achieve the above objectives, the first embodiment of the present invention provides a vinyl polymer / modified polyhydroxy polymer composite, which comprises 1 to 70% of a modified polyhydroxy polymer and 30 to 99% of a vinyl polymer, by mass, and is prepared by a blending method.
[0010] The beneficial effects brought by the vinyl polymer / modified polyhydroxy polymer composite of the embodiment of the present invention are as follows: 1. The composite is a non-crosslinked structure with better thermochemical stability, and overcomes the strong hydrophilicity and water solubility of the polyhydroxy polymer, and can effectively regulate the water absorption rate of the composite membrane material; 2. When the composite is applied to the ion exchange membrane of the fuel cell, the cationic functional groups and the hydroxyl groups will form a hydrogen bond network, and the interaction of the multiple functional groups makes the composite membrane have high ion conductivity, high barrier properties, excellent physical and mechanical properties and suitable water absorption rate, and the non-covalent crosslinked structure enables the ion exchange membrane material to maintain the characteristics of recycling and reuse; 3. The hydrogen bonds formed by the composite The bond energy is lower than that of the covalent bond, and it has the ability to quickly rebuild after breaking. It plays the role of a "sacrificial bond" during use, that is, when the prepared ion exchange membrane is attacked by hydroxide during operation, it will preferentially destroy the weak interaction between the hydroxyl group and the cationic functional group, thereby protecting the covalent bond between the cationic functional group and the polymer main chain. This weak interaction can be quickly rebuilt after being destroyed, thereby macroscopically extending the service life of the ion exchange membrane; 4. The EVOH component of the composite has excellent barrier properties and semi-crystallinity, which is not only conducive to blocking gases, but also can effectively block the attack of hydroxide on polymers. , slowing down the rate at which the cationic functional groups leave the polymer membrane, thereby extending the service life of the ion exchange membrane when the composite is used for an ion exchange membrane; 5. The composite membrane material prepared using the composite has good gas barrier properties and water vapor permeability, and has good mechanical properties under high temperature and high humidity conditions, and can be used as a gas humidification membrane for a fuel cell humidification device; 6. The cationic functional groups of the modified polyhydroxy polymers in the composite are broad-spectrum antibacterial groups, which are commonly used antibacterial means for biomedical materials and packaging materials. Therefore, the vinyl polymer / modified polyhydroxy polymer in the embodiment of the present invention can be used for biomedical materials and food packaging materials; 7. The composite In addition to being used in fuel cell ion exchange membranes, the compound can also be used in the field of electrochemistry for polyelectrolyte membranes in the chlor-alkali industry, ion exchange membranes for water electrolysis to produce hydrogen, acidic primary battery membranes, secondary battery membranes such as lithium batteries, polyelectrolytes in supercapacitors, polyelectrolyte membranes for metal recovery batteries, and sensors (especially humidity sensors); 8. The cationic functional groups in the complex are positively charged hydrophilic groups and can be used as coatings, hydrogels and adhesives for porous membranes such as desalination membranes (nanofiltration membranes) and ultra / microfiltration membranes; 9. The complex has good water vapor permeability and optical properties and can be used in the preparation of protective clothing materials and breathable fabrics.The fabric material prepared by coating or directly laminating the composite of the embodiment of the present invention with a film or a dispersion has good barrier properties and good water vapor transmission performance. When worn on the human body, the wearer's sweat can be discharged in time, which improves comfort. At the same time, it can also effectively block external smoke, chemical reagents and biological reagents. Therefore, the composite of the embodiment of the present invention can also be applied to various fabrics in the biomedical field such as surgical gloves, medical protective clothing, sterile sheets, and protective equipment for biochemical battlefields such as military protective clothing.
[0011] In some embodiments of the present invention, the vinyl polymer is an ethylene-vinyl alcohol copolymer or an ethylene-vinyl alcohol-vinyl acetate terpolymer.
[0012] In some embodiments of the present invention, the melt index of the copolymer is 2.2-15.2 g / 10 min; the molar content of vinyl alcohol in the vinyl polymer is 28-94%, the molar content of ethylene is 6-72%, and the molar content of vinyl acetate is 0-6%.
[0013] In some embodiments of the present invention, the modified polyhydroxy polymer is obtained by grafting functional groups onto hydroxyl groups or amino groups in the polyhydroxy polymer; the degree of functionality of the modified polyhydroxy polymer is 0.1-20%.
[0014] In some embodiments of the present invention, the polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, lignin or polyethylene glycol; and the functionalized group is a quaternary ammonium group, an imidazole group, a piperidine group or a guanidine group.
[0015] In some embodiments of the present invention, the method for preparing the modified polyhydroxy polymer comprises the following steps:
[0016] (1) dissolving a polyhydroxy polymer in water and / or an organic solvent to prepare a polyhydroxy polymer dispersion;
[0017] (2) adding a functionalizing agent and a corresponding catalyst to the polyhydroxy polymer dispersion of step (1), and performing a functionalizing reaction at 0 to 150° C. for 1 to 12 hours;
[0018] (3) adding a low-order fatty alcohol to the solution system after the reaction in step (2) to precipitate, washing and drying to obtain a clean modified polyhydroxy polymer; or, adjusting the pH of the solution system after the reaction in step (2) to neutral, centrifuging and separating, taking the supernatant, dialyzing, and drying to obtain a clean modified polyhydroxy polymer.
[0019] In some embodiments of the present invention, in step (1), the organic solvent is selected from at least one of ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, phenol, m-phenol, toluene, o-dichlorobenzene, methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol; in step (2), the functionalizing agent is a quaternizing agent, an imidazole agent, or a piperidinyl agent.
[0020] In some embodiments of the present invention, the piperidinylating agent is selected from at least one of piperidine-1-carboxaldehyde, piperidine-4-carboxaldehyde, 1-methylpiperidine-4-carboxaldehyde, 1-isopropyl-piperidine-4-carboxaldehyde, 1-ethyl-piperidine-4-carboxaldehyde, 1-methyl-4-piperidineacetaldehyde, and 1-methyl-3-piperidineacetaldehyde.
[0021] In some embodiments of the present invention, the quaternary ammonium agent is selected from at least one of 2,3-epoxypropyltrimethylammonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, N-2,3-epoxypropyldimethyloctylammonium chloride, and N-2,3-epoxypropyldimethyldodecylammonium chloride; and the catalyst corresponding to the quaternary ammonium agent is selected from at least one of sodium potassium hydroxide, sodium hydroxide, rubidium hydroxide, sodium hydride, calcium hydride, sodium carbonate, and potassium carbonate.
[0022] In some embodiments of the present invention, the imidazolyl reagent is selected from at least one of imidazole aldehyde, imidazole-2-carboxaldehyde, 4-imidazole carboxaldehyde, 4-methylimidazole-5-carboxaldehyde, 1-methyl-2-aldehyde imidazole, 2-methylimidazole-4-carboxaldehyde, 4-bromo-1-methyl-1H-imidazole-5-carboxaldehyde, 1-methyl-4-phenyl-1H-imidazole-5-carboxaldehyde, 1-triphenylmethyl-4-imidazole carboxaldehyde, 4-(imidazole-1-yl)benzaldehyde, and (1H-imidazole-4-yl)-acetaldehyde; when the polyhydroxy polymer is one of PVA, cellulose, EVOH, lignin, and polyethylene glycol, the catalyst corresponding to the imidazolyl reagent is at least one of the inorganic acids; when the polyhydroxy polymer is chitosan, the catalyst corresponding to the imidazolyl reagent is acetic acid and / or NaBH4.
[0023] To achieve the above objectives, the second embodiment of the present invention relates to the application of the vinyl polymer / modified polyhydroxy polymer composite as described above in the fields of biomedical materials, packaging materials, electrochemistry, porous membranes, fabrics, and protective equipment.
[0024] The application of the vinyl polymer / modified polyhydroxy polymer composite in the embodiment of the present invention has substantially the same beneficial effects as those brought about by the above-mentioned vinyl polymer / modified polyhydroxy polymer composite, which will not be described in detail here.
[0025] To achieve the above object, a third aspect of the present invention provides a composite film, comprising the vinyl polymer / modified polyhydroxy polymer composite as described above.
[0026] The composite film of the embodiment of the present invention has substantially the same beneficial effects as those of the above-mentioned vinyl polymer / modified polyhydroxy polymer composite, which will not be described in detail herein.
[0027] To achieve the above object, the fourth aspect of the present invention provides a method for preparing a composite film, wherein a vinyl polymer and a modified polyhydroxy polymer are dissolved in a solvent to obtain a blended dispersion, and then the blended dispersion is volatilized at 20 to 180° C. for 1 to 200 hours to obtain the composite film material;
[0028] The solvent is at least one of water, ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, phenol, m-phenol, toluene, o-dichlorobenzene, methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.
[0029] The method for preparing the composite membrane of the embodiment of the present invention has simple process and convenient operation.
[0030] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0032] Figure 1 This is a performance test curve diagram of a composite membrane single cell numbered EQP-5 in Example 6 of the present invention (the curve with black squares in the figure is the voltage-current density curve of the EQP-5 composite membrane, and the curve with white squares is the power density-current density curve of the EQP-5 composite membrane).
[0033] Figure 2 This is a durability test diagram of the composite membrane numbered EQP-5 in Example 6 of the present invention.
[0034] Figure 3 This is the single cell performance test curve of the EVOH / MI-CS composite membrane numbered EMC-3 in Example 7 of the present invention (the curve with a black origin in the figure is the voltage-current density curve of the EVOH / MI-CS composite membrane, and the curve with a white origin is the power density-current density curve of the EVOH / MI-CS composite membrane).
[0035] Figure 4This is a performance comparison chart of a single cell of the comparative PVA / Q-PVA5 composite membrane and the composite membrane numbered EQP-5 in Example 6 (the curve with a black origin in the figure is the voltage-current density curve of the EQP-5 composite membrane, the curve with a white origin is the power density-current density curve of the EQP-5 composite membrane, the curve with black small squares is the voltage-current density curve of the PVA / Q-PVA5 composite membrane, and the curve with white small squares is the power density-current density curve of the PVA / Q-PVA5 composite membrane).
[0036] Figure 5 This is a durability comparison chart of the PVA / Q-PVA5 composite membrane of Comparative Example 4 and the composite membrane numbered EQP-5 in Example 6. DETAILED DESCRIPTION
[0037] The embodiments of the present application are described in detail below. The embodiments are exemplary and intended to be used to explain the present application, but should not be construed as limiting the present application.
[0038] The vinyl polymer / modified polyhydroxy polymer composite of the embodiment of the present invention comprises 1 to 70% of modified polyhydroxy polymer and 30 to 99% of vinyl polymer, calculated by mass, and is prepared by a blending method.
[0039] The beneficial effects brought by the vinyl polymer / modified polyhydroxy polymer composite of the embodiment of the present invention are as follows: 1. The composite is a non-crosslinked structure with better thermochemical stability, and overcomes the strong hydrophilicity and water solubility of the polyhydroxy polymer, and can effectively regulate the water absorption rate of the composite membrane material; 2. When the composite is applied to the ion exchange membrane of the fuel cell, the cationic functional groups and the hydroxyl groups will form a hydrogen bond network, and the interaction of the multiple functional groups makes the composite membrane have high ion conductivity, high barrier properties, excellent physical and mechanical properties and suitable water absorption rate, and the non-covalent crosslinked structure enables the ion exchange membrane material to maintain the characteristics of recycling and reuse; 3. The hydrogen bonds formed by the composite The bond energy is lower than that of the covalent bond, and it has the ability to quickly rebuild after breaking. It plays the role of a "sacrificial bond" during use, that is, when the prepared ion exchange membrane is attacked by hydroxide during operation, it will preferentially destroy the weak interaction between the hydroxyl group and the cationic functional group, thereby protecting the covalent bond between the cationic functional group and the polymer main chain. This weak interaction can be quickly rebuilt after being destroyed, thereby macroscopically extending the service life of the ion exchange membrane; 4. The EVOH component of the composite has excellent barrier properties and semi-crystallinity, which is not only conducive to blocking gases, but also can effectively block the attack of hydroxide on polymers. , slowing down the rate at which the cationic functional groups leave the polymer membrane, thereby extending the service life of the ion exchange membrane when the composite is used for an ion exchange membrane; 5. The composite membrane material prepared using the composite has good gas barrier properties and water vapor permeability, and has good mechanical properties under high temperature and high humidity conditions, and can be used as a gas humidification membrane for a fuel cell humidification device; 6. The cationic functional groups of the modified polyhydroxy polymers in the composite are broad-spectrum antibacterial groups, which are commonly used antibacterial means for biomedical materials and packaging materials. Therefore, the vinyl polymer / modified polyhydroxy polymer in the embodiment of the present invention can be used for biomedical materials and food packaging materials; 7. The composite In addition to being used in fuel cell ion exchange membranes, the compound can also be used in the field of electrochemistry for polyelectrolyte membranes in the chlor-alkali industry, ion exchange membranes for water electrolysis to produce hydrogen, acidic primary battery membranes, secondary battery membranes such as lithium batteries, polyelectrolytes in supercapacitors, polyelectrolyte membranes for metal recovery batteries, and sensors (especially humidity sensors); 8. The cationic functional groups in the complex are positively charged hydrophilic groups and can be used as coatings, hydrogels and adhesives for porous membranes such as desalination membranes (nanofiltration membranes) and ultra / microfiltration membranes; 9. The complex has good water vapor permeability and optical properties and can be used in the preparation of protective clothing materials and breathable fabrics.The fabric material prepared by coating or directly laminating the composite of the embodiment of the present invention with a film or a dispersion has good barrier properties and good water vapor transmission performance. When worn on the human body, the wearer's sweat can be discharged in time, which improves comfort. At the same time, it can also effectively block external smoke, chemical reagents and biological reagents. Therefore, the composite of the embodiment of the present invention can also be applied to various fabrics in the biomedical field such as surgical gloves, medical protective clothing, sterile sheets, and protective equipment for biochemical battlefields such as military protective clothing.
[0040] Among them, the content of the modified polyhydroxy polymer is preferably 1 to 50%, more preferably 1 to 40%, by mass.
[0041] Among them, the content of the vinyl polymer (EVOH) is preferably 50 to 99%, more preferably 60 to 99%, by mass.
[0042] Wherein, the vinyl polymer is an ethylene-vinyl alcohol copolymer or an ethylene-vinyl alcohol-vinyl acetate terpolymer. The melt index of the copolymer is 2.2 to 15.2 g / 10 min, preferably 2.7 to 14.7 g / 10 min, and more preferably 2.9 to 13.9 g / 10 min. In the vinyl polymer: the molar content of vinyl alcohol is 28 to 94%, preferably 36 to 92%, and more preferably 42 to 84%; the molar content of ethylene is 6 to 72%, preferably 8 to 64%, and more preferably 16 to 58%; the molar content of vinyl acetate is 0 to 6%, preferably 0.01 to 6%, and more preferably 0.01% to 5.5%.
[0043] Wherein, the modified polyhydroxy polymer is obtained by grafting the hydroxyl or amino group in the polyhydroxy polymer with the functional group containing propylene oxide through epoxy ring-opening reaction, or by grafting the hydroxyl or amino group in the polyhydroxy polymer with the aldehyde group of the functional group containing aldehyde group through aldol condensation or aldehyde amine condensation reaction. Wherein, the polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, lignin or polyethylene glycol. Preferably, when the vinyl polymer / modified polyhydroxy polymer composite is applied to ion exchange membrane and / or gas humidification membrane, the polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, lignin; preferably, when the vinyl polymer / modified polyhydroxy polymer composite is applied to biomedical materials, the polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, polyethylene glycol; preferably, when the vinyl polymer / modified polyhydroxy polymer composite is applied to packaging materials, the polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, lignin, polyethylene glycol.
[0044] Wherein, the functionalized group is a quaternary ammonium group, an imidazole group, a piperidine group or a guanidine group.
[0045] The molar percentage of the functionalized groups to all structural units is the functionalization degree. The functionalization degree of the modified polyhydroxy polymer is 0.1 to 20%, preferably 0.1 to 15%, and more preferably 0.1 to 10%.
[0046] The preparation method of the modified polyhydroxy polymer comprises the following steps:
[0047] (1) dissolving a polyhydroxy polymer in water and / or an organic solvent to prepare a polyhydroxy polymer dispersion;
[0048] (2) adding a functionalizing agent and a corresponding catalyst to the polyhydroxy polymer dispersion of step (1), and performing a functionalizing reaction at 0 to 150° C. for 1 to 12 hours;
[0049] (3) adding a low-order fatty alcohol to the solution system after the reaction in step (2) to precipitate, washing and drying to obtain a clean modified polyhydroxy polymer; or, adjusting the pH of the solution system after the reaction in step (2) to neutral, centrifuging and separating, taking the supernatant, dialyzing, and drying to obtain a clean modified polyhydroxy polymer.
[0050] Wherein, in step (1), the organic solvent is selected from at least one of ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, phenol, m-phenol, toluene, o-dichlorobenzene, methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.
[0051] Wherein, in step (2), the functionalizing agent includes a quaternary ammonium agent, an imidazole agent, and a piperidinium agent. Considering the performance and cost, the quaternary ammonium agent and the imidazole agent are preferred.
[0052] Optionally, the piperidinylating agent is selected from at least one of piperidine-1-carboxaldehyde, piperidine-4-carboxaldehyde, 1-methylpiperidine-4-carboxaldehyde, 1-isopropyl-piperidine-4-carboxaldehyde, 1-ethyl-piperidine-4-carboxaldehyde, 1-methyl-4-piperidineacetaldehyde, and 1-methyl-3-piperidineacetaldehyde.
[0053] Optionally, the quaternary ammonium agent is selected from at least one of 2,3-epoxypropyltrimethylammonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, N-2,3-epoxypropyldimethyloctylammonium chloride, and N-2,3-epoxypropyldimethyldodecylammonium chloride; and the catalyst corresponding to the quaternary ammonium agent is selected from at least one of sodium potassium hydroxide, sodium hydroxide, rubidium hydroxide, sodium hydride, calcium hydride, sodium carbonate, and potassium carbonate. The general structural formula of the obtained quaternary ammonium modified polyhydroxy polymer is:
[0054]
[0055] Wherein n represents the molar percentage content in the quaternized modified polyhydroxy polymer, which is 1-20%; R is any one of methyl, n-octyl and dodecyl; A is at least one of PVA, cellulose, lignin, EVOH and polyethylene glycol that do not contain amino groups (-NH2); and B is chitosan containing amino groups.
[0056] Optionally, the imidazole reagent is a small molecule compound of the imidazole type containing an aldehyde group, preferably at least one selected from imidazole aldehyde, imidazole-2-carboxaldehyde, 4-imidazole carboxaldehyde, 4-methylimidazole-5-carboxaldehyde, 1-methyl-2-aldehyde imidazole, 2-methylimidazole-4-carboxaldehyde, 4-bromo-1-methyl-1H-imidazole-5-carboxaldehyde, 1-methyl-4-phenyl-1H-imidazole-5-carboxaldehyde, 1-triphenylmethyl-4-imidazole carboxaldehyde, 4-(imidazole-1-yl)benzaldehyde, and (1H-imidazole-4-yl)-acetaldehyde. When the polyhydroxy polymer is one of PVA, cellulose, EVOH, lignin, and polyethylene glycol that does not contain an amino group (-NH2), the small molecule imidazole compound containing an aldehyde group will react and graft with the hydroxyl group, and the catalyst corresponding to the imidazole reagent is at least one of inorganic acids such as hydrochloric acid, nitric acid, phosphoric acid or sulfuric acid. The general structural formula of the obtained imidazole-modified polyhydroxy polymer is formula (a) and formula (b):
[0057]
[0058] Wherein n represents the molar percentage content in the imidazole modified polyhydroxy polymer, which is 1-20%; R1 is any one of H and methyl; R2 is any one of H and methyl; R3 is any one of H and methyl; R4 is any one of H, methyl, Br, and phenyl; formula (a) is the general structure of grafted imidazole-2-carboxaldehyde and 1-methyl-2-formylimidazole; formula (b) is the general structure of grafted 4-imidazolecarboxaldehyde, 4-methylimidazole-5-carboxaldehyde, 2-methylimidazole-4-carboxaldehyde, 4-bromo-1-methyl-1H-imidazole-5-carboxaldehyde, and 1-methyl-4-phenyl-1H-imidazole-5-carboxaldehyde.
[0059] When the polyhydroxy polymer is chitosan containing amino groups, the small molecule imidazole compounds containing aldehyde groups will react and graft with the amino groups with stronger reaction activity. The catalyst corresponding to the imidazole reagent is acetic acid and / or NaBH4. The general structural formula of the obtained imidazole-modified polyhydroxy polymer is formula (c) and formula (d):
[0060]
[0061] Wherein n represents the molar percentage content in the imidazole modified polyhydroxy polymer, which is 1-20%; R1 is any one of H and methyl; R2 is any one of H and methyl; R3 is any one of H and methyl; R4 is any one of H, methyl, Br, and phenyl; formula (c) is the general structure of grafted imidazole-2-carboxaldehyde and 1-methyl-2-formylimidazole; formula (d) is the general structure of grafted 4-imidazolecarboxaldehyde, 4-methylimidazole-5-carboxaldehyde, 2-methylimidazole-4-carboxaldehyde, 4-bromo-1-methyl-1H-imidazole-5-carboxaldehyde, and 1-methyl-4-phenyl-1H-imidazole-5-carboxaldehyde.
[0062] Wherein, in step (3), the lower aliphatic alcohol is at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol or isobutanol.
[0063] The composite film of the embodiment of the present invention comprises the above-mentioned vinyl polymer / modified polyhydroxy polymer composite. The preparation method of the composite film comprises: dissolving the vinyl polymer and the modified polyhydroxy polymer in a solvent to obtain a blended dispersion, and then volatilizing the blended dispersion at 20 to 180°C for 1 to 200 hours to obtain the composite film material; wherein the solvent is at least one of water, ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, phenol, metaphenol, toluene, o-dichlorobenzene, methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol.
[0064] The following is a description of the vinyl polymer / modified polyhydroxy polymer composite and the ion exchange membrane containing the vinyl polymer / modified polyhydroxy polymer composite according to the embodiments of the present invention in conjunction with specific embodiments. Unless otherwise specified, the raw materials involved in the embodiments of the present invention are all commercially available products, and the experimental methods involved are all conventional methods.
[0065] 1. Performance testing method
[0066] The tensile test method under the conditions of 80°C and 95% relative humidity refers to the standard test method given in the tensile performance test section of GB / T 20042.3-2009 "Proton exchange membrane fuel cell part 3: proton exchange membrane test method".
[0067] The tensile properties of dry films were tested according to GB / T 1040-2006.
[0068] The water vapor transmission rate is tested according to GB1037-1988 "Test method for water vapor permeability of plastic film and sheet - Cup method".
[0069] The conductivity test uses a Swiss Metrohm AC workstation and an AC impedance four-electrode method to test the membrane internal resistance. The AC frequency range is 100 Hz-1 MHz, the perturbation voltage is 10 mV, the membrane is cut into samples of 4*3 cm size and mounted in a four-electrode fixture, the fixture is immersed in ultrapure water at 80°C, and the conductivity of the sample is tested at 80°C-100% RH.
[0070] Durability The stability of the composite of the present invention in alkaline solution was investigated by immersing it in 1M KOH solution at 80° C. for 720 h, taking it out at regular intervals and washing it with ultrapure water until it was neutral, and then testing the change in conductivity at 80° C.
[0071] The specific method of single cell performance test is as follows: the membrane is cut into 2.5*2.5cm size, and Pt / C catalyst is evenly sprayed on both sides of the membrane using an electrostatic sprayer to prepare CCM (fuel cell chip). The loading of the cathode and anode is 0.5mg / cm 2 Carbon paper and gaskets were pressed on both sides of CCM by hot pressing to prepare MEA (membrane electrode). Single cell test system was used for online detection, with anode and cathode gas flow rate of 800 mL / min and back pressure of 0.2 MPa.
[0072] 2. Examples and Comparative Examples
[0073] Example 1: Preparation of quaternary ammonium modified PVA
[0074] Weigh a certain mass of PVA and dissolve it in 200 mass parts of water at 90°C, add a certain mass of 2,3-epoxypropyltrimethylammonium chloride, add 10 mass parts of KOH as a catalyst, and stir the reaction at 65°C for 0.5 to 6 hours under nitrogen protection. Add methanol to obtain a polymer precipitate, and dry to obtain pure quaternary ammonium modified PVA (Q-PVA). The functionalization degree of quaternary ammonium modified PVA (Q-PVA) at different ratios of PVA and 2,3-epoxypropyltrimethylammonium chloride is shown in Table 1.
[0075] Table 1 Functionalization degree of quaternary ammonium modified PVA at different ratios of PVA and 2,3-epoxypropyltrimethylammonium chloride
[0076] Product No. Q-PVA1 Q-PVA2 Q-PVA3 Q-PVA4 Q-PVA5 PVA / mass 60 30 10 7.5 5 2,3-Epoxypropyltrimethylammonium chloride / mass parts 30 30 30 30 30 Mass ratio of 2,3-epoxypropyltrimethylammonium chloride to PVA 0.5 1 3 4 6 Reaction time / h 0.5 2 4 5 6 Functionalization degree / % 0.42 1.54 2.16 3.21 4.05
[0077] Example 2: Preparation of imidazole-modified chitosan
[0078] Weigh 2 parts by mass of chitosan and disperse it in 100 parts by mass of water, stir for 12 hours, adjust the pH value of the system to 4-5 with dilute acetic acid solution, add 0.5 parts by mass of 4-imidazole-formaldehyde, and react at 80°C for 24 hours. Adjust the pH value to neutral (pH=7) with dilute NaOH solution, add 10wt% NaBH4, add 3mol / L HCl to neutral, take the supernatant after centrifugation, dialyze to remove small molecular impurities, and dry at 60°C to obtain imidazole-modified chitosan (MI-CS) with a functionalization degree of 2.35%.
[0079] Example 3: Preparation of quaternized modified hydroxyethyl cellulose
[0080] 1 part by mass of hydroxyethyl cellulose was dispersed in a mixed medium of 10 parts by mass of water and 10 parts by mass of isopropanol, and after being stirred evenly, 1.5 parts by mass of NaOH and 3 parts by mass of N-2,3-epoxypropyldimethyldodecylammonium chloride solution were added in batches, and then stirred and reacted at 65°C for 4 hours. 3 mol / L HCl was added to adjust to neutrality, washed, purified, and dried at 60°C to obtain quaternary ammonium modified hydroxyethyl cellulose (Q-HEC) with a functionalization degree of 0.34%.
[0081] Example 4: Preparation of imidazole-modified EVOH
[0082] Weigh 1 part by mass of EVOH-2 (ethylene content 27 mol%, saponification degree> 99.9%) and dissolve it in 10 parts by mass of water and 10 parts by mass of isopropanol at 80°C, add 1 part by mass of imidazole-2-carboxaldehyde, add 0.78 parts by mass of KOH as a catalyst, and stir the reaction at 80°C for 12 hours under nitrogen protection. Add methanol to obtain a polymer precipitate, and dry it to obtain pure imidazole-modified EVOH (MI-EVOH).
[0083] Example 5: EVOH / Q-PVA composite
[0084] A certain mass part of EVOH-1 (ethylene content 44 mol%, saponification degree> 99.9%) and a certain mass part of Q-PVA in Example 1 were weighed into 9 mass parts of dimethyl sulfoxide, and stirred at room temperature for 24 hours to dissolve EVOH-1 and Q-PVA in dimethyl sulfoxide to obtain EVOH / Q-PVA composite. The properties of the EVOH / Q-PVA composites obtained under different ratios are shown in Table 2.
[0085] Table 2 Viscosity of EVOH / Q-PVA composites obtained from EVOH-1 / Q-PVA at different ratios
[0086] Product No. EVOH-1 / part by mass Q-PVA / part by weight Composite viscosity / (mPa·s) EVOH / Q-PVA-1 0.5 0.5 114.2 EVOH / Q-PVA-2 0.6 0.4 107.4 EVOH / Q-PVA-3 0.7 0.3 87.6 EVOH / Q-PVA-4 0.8 0.2 65.2
[0087] The product numbered EVOH / Q-PVA-4 composite was dried at 120°C for 36 hours to obtain a dry film, and then immersed in a 2 mol / L NaOH solution at room temperature for 24 hours to obtain a composite film. The composite film had a tensile strength of 67.7 MPa, an elongation at break of 91.6%, a water absorption of 63.8% at 25°C, and an electrical conductivity of 77.3% at 80°C.
[0088] Example 6: EVOH / Q-PVA composite film
[0089] 0.7 parts by mass of EVOH-1 (ethylene content 44 mol%, saponification degree> 99.9%) and 0.3 parts by mass of Q-PVA in Example 1 were weighed and dissolved in 9 parts by mass of dimethyl sulfoxide. The dried film was dried at 120°C for 36 hours, and the EVOH / Q-PVA composite film was obtained by soaking in a 2 mol / L NaOH solution at room temperature for 24 hours. The thickness of the composite film of different components was 40 μm. The tensile properties, water absorption at 25°C and conductivity at 80°C of the dried film are shown in Table 3.
[0090] Table 3 Properties of EVOH / Q-PVA composite films
[0091]
[0092] The composite film EQP-5 prepared by EVOH-1 and Q-PVA5 has a tensile strength of 7.6MPa and an elongation at break of 201.8% at 80℃ and 95% relative humidity. The water vapor permeability of the composite film is 1826.2g / (m 2 ·24h). At 80℃, the water absorption of the film is 127.8%.
[0093] Figure 1 This is a single cell performance test curve of the composite membrane numbered EQP-5. Figure 1 It can be seen that the single cell test shows that the current density of the EQP-5 composite membrane is 1.5A / cm 2 The peak power reaches 975mW / cm 2 .
[0094] Figure 2 Durability test diagram of composite membrane numbered EQP-5. Figure 2 It can be seen that after the EQP-5 composite membrane was immersed in 80℃-1M KOH solution for 150h, the conductivity decreased by about 34%, and then until 720h, the conductivity reduction amplitude decreased and tended to be stable.
[0095] Compared with Comparative Example 1 (see below) and Comparative Example 4 (see below), the introduction of EVOH overcomes the water solubility problem of Q-PVA. Compared with Comparative Example 7 (see below), the composite membrane EQP-5 has higher conductivity and battery performance, and is more suitable as an ion exchange membrane for fuel cells; it has higher water vapor permeability at high temperatures and can be used as a gas humidification membrane; and the non-cross-linked membrane has better robustness under alkaline conditions.
[0096] Example 7: EVOH / MI-CS composite film
[0097] A certain mass of EVOH-2 (ethylene content 27 mol%, saponification degree> 99.9%) and a certain mass of MI-CS (imidazole modified chitosan) in Example 2 were weighed and dissolved in 9 parts by mass of N,N-dimethylformamide. The dried film was dried at 60°C for 24 hours, and the EVOH / MI-CS composite film was obtained by soaking in a 2 mol / L NaOH solution at room temperature for 24 hours. The thickness of the composite film of different components was 40 μm. The tensile properties, water absorption at 25°C and conductivity at 80°C of the dried film are shown in Table 4.
[0098] Table 4 Properties of EVOH / MI-CS composite films
[0099]
[0100] Composite film EMC-3, 80 ℃, 95% relative humidity conditions, the tensile strength of the composite film is 5.6MPa, the elongation at break is 102.5%; at 38 ℃-90% RH (RH is relative humidity), the water vapor permeability of the composite film is 1521.9g / (m 2 ·24h). At 80℃, the water absorption of the film is 98.8%.
[0101] Figure 3 This is the single cell performance test curve of EVOH / MI-CS composite film numbered EMC-3. Figure 3 It can be seen that the single cell test shows that the current density of the EVOH / MI-CS composite film is 1.7A / cm 2 The peak power reached 892.5mW / cm 2 .
[0102] Compared with Comparative Example 2 (see below) and Comparative Example 5 (see below), the introduction of EVOH overcomes the water solubility problem of MI-CS.
[0103] Example 8: Preparation of EVOH-2 / Q-HEC composite film
[0104] Weigh 0.75 parts by mass of EVOH-2 (ethylene content 27 mol%, saponification degree> 99.9%) and 0.25 parts by mass of Q-HEC in Example 3 and add them to 9 parts by mass of N,N-dimethylacetamide. Dry at 100°C for 18 hours to obtain a dry film, and soak it in 2 mol / L NaOH solution at room temperature for 24 hours to obtain an EVOH-2 / Q-HEC composite film. The thickness of the dried composite film is 40μm, the tensile strength of the dried composite film is 69.4MPa, and the elongation at break is 78.9%; at 80°C and 95% relative humidity, the tensile strength of the composite film is 10.3MPa, and the elongation at break is 143.6%; at 25°C, the water absorption of the film is 32.1%, and at 38°C-90%RH, the water vapor permeability of the film is 1402.2g / (m 2 ·24h). At 80°C, the water absorption of the film is 90.8%.
[0105] Compared with Comparative Examples 3 and 6, the introduction of EVOH overcomes the water solubility problem of Q-HEC.
[0106] Example 9: Preparation of EVOH / MI-EVOH composite film
[0107] Weigh 0.65 parts by mass of EVOH-2 (ethylene content 27 mol%, saponification degree> 99.9%) and 0.35 parts by mass of MI-EVOH in Example 4 and add them to 9 parts by mass of N,N-dimethylformamide. Dry at 60°C for 24 hours to obtain a dry film, and soak it in 2 mol / L NaOH solution at room temperature for 24 hours to obtain an EVOH-2 / Q-EVOH composite film. The thickness of the dried composite film is 40μm, the tensile strength of the dried composite film is 47.8MPa, and the elongation at break is 110.7%; at 80°C and 95% relative humidity, the tensile strength of the composite film is 10.8MPa, and the elongation at break is 195.3%; at 25°C, the water absorption of the film is 53.9%, and at 38°C-90%RH, the water vapor permeability of the film is 1476.9g / (m 2 ·24h). At 80℃, the water absorption of the film is 116.3%.
[0108] Comparative Example 1
[0109] The five functionalized Q-PVAs in Example 1 were placed in deionized water and stirred at room temperature. The Q-PVA swelled, broke and dispersed into gel particles. The temperature was raised to 80°C and stirred to form a transparent and uniform dispersion. This shows that even if Q-PVA is dried to form a film, it cannot be used under water conditions.
[0110] Comparative Example 2
[0111] The MI-CS in Example 2 was placed in deionized water and stirred at room temperature. The MI-CS swelled, broke and dispersed into gel particles. The temperature was raised to 80°C and stirred to form a transparent and uniform dispersion. This shows that even if MI-CS is dried to form a film, it cannot be used under water conditions.
[0112] Comparative Example 3
[0113] The Q-HEC in Example 3 was placed in deionized water and stirred at room temperature to form a transparent and uniform dispersion. This shows that even if MI-CS is dried to form a film, it cannot be used under water-containing conditions.
[0114] Comparative Example 4
[0115] 0.7 parts by mass of PVA and 0.3 parts by mass of Q-PVA5 in Example 1 were weighed and dissolved in 9 parts by mass of dimethyl sulfoxide. After drying at 120°C for 36 hours, a PVA / Q-PVA5 composite film with a thickness of 40 μm was obtained. The composite film was placed in deionized water and stirred at room temperature. The composite film swelled, broke and dispersed into gel particles. The temperature was raised to 80°C and stirred to form a transparent and uniform dispersion, which shows that the PVA / Q-PVA1 composite film cannot be used under water conditions.
[0116] The single cell performance of the PVA / Q-PVA5 composite membrane of this comparative example was compared with the composite membrane numbered EQP-5 in Example 6. The results are shown in FIG. Figure 4 .from Figure 4 It can be seen that the maximum power density of the PVA / Q-PVA5 composite film is 833mW / cm 2 , lower than that of EQP-5 composite membrane.
[0117] The PVA / Q-PVA5 composite membrane of this comparative example and the composite membrane numbered EQP-5 in Example 6 were immersed in 80°C-1M KOH solution for 800 hours, and the durability of the two was compared. The results are shown in FIG. Figure 5 .from Figure 5 It can be seen that after immersion in 80 °C-1 M KOH solution for 720 h, the conductivity decreases more than that of EQP-5, and is still on a downward trend at 720 h.
[0118] Comparative Example 5
[0119] 0.9 parts by mass of PVA and 0.1 parts by mass of MI-CS in Example 2 were weighed and dissolved in 9 parts by mass of N,N-dimethylformamide. The film was dried at 60°C for 24 hours to obtain a PVA / MI-CS composite film with a thickness of 40 μm. The composite film was placed in deionized water and stirred at room temperature. The composite film swelled, broke and dispersed into gel particles. The temperature was raised to 80°C and stirred to form a transparent and uniform dispersion. This shows that the PVA / MI-CS composite film cannot be used under water conditions.
[0120] Comparative Example 6
[0121] 0.75 parts by mass of PVA and 0.25 parts by mass of Q-HEC in Example 3 were weighed and added to 9 parts by mass of N,N-dimethylacetamide. After drying at 100°C for 18 hours, a PVA / Q-HEC composite film with a thickness of 40 μm was obtained. The composite film was placed in deionized water and stirred at room temperature. The composite film swelled, broke and dispersed into gel particles. The temperature was raised to 80°C and stirred to form a transparent and uniform dispersion, which shows that the PVA / Q-HEC composite film cannot be used under water conditions.
[0122] Comparative Example 7
[0123] The composite film PVA / Q-PVA5 in comparative example 4 was placed in a 10% glutaraldehyde solution for heat treatment and crosslinking at a temperature of 80°C for 4 hours. After the reaction, the excess crosslinking agent was removed by deionizing rinse and then placed in a 2mol / L NaOH solution and soaked at room temperature for 24 hours to obtain a crosslinked composite film CS-PVA / Q-PVA5. The tensile strength of the dry film was 78.2MPa and the elongation at break was 32.7%; at 80°C and 95% relative humidity, the tensile strength of the composite film was 15.3MPa and the elongation at break was 66.7%; at 25°C, the water absorption of the film was 43.6%; at 38°C-90%RH, the water vapor permeability of the film was 1510.4g / (m 2 ·24h). At 80°C, the water absorption of the film is 108.8%.
[0124] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0125] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A vinyl polymer / modified polyhydroxy polymer composite, characterized in that: The invention comprises 1 to 70% of a modified polyhydroxy polymer and 30 to 99% of a vinyl polymer, by mass, and is prepared by a blending method; The vinyl polymer is an ethylene-vinyl alcohol binary copolymer or an ethylene-vinyl alcohol-vinyl acetate terpolymer; The modified polyhydroxy polymer is obtained by grafting functional groups of hydroxyl or amino groups in the polyhydroxy polymer; the functionalization degree of the modified polyhydroxy polymer is 0.1 to 20%; The polyhydroxy polymer is PVA, chitosan, cellulose, EVOH, lignin or polyethylene glycol; the functionalized group is a quaternary ammonium group or an imidazole group; The vinyl polymer / modified polyhydroxy polymer complex is a non-covalently cross-linked structure.
2. The vinyl polymer / modified polyhydroxy polymer composite according to claim 1, characterized in that: The melt index of the copolymer is 2.2 to 15.2 g / 10 min. The molar content of vinyl alcohol in the vinyl polymer is 28 to 94%, the molar content of ethylene is 6 to 72%, and the molar content of vinyl acetate is 0 to 6%.
3. The vinyl polymer / modified polyhydroxy polymer composite according to claim 1, characterized in that: The preparation method of the modified polyhydroxy polymer comprises the following steps: (1) dissolving a polyhydroxy polymer in water and / or an organic solvent to prepare a polyhydroxy polymer dispersion; (2) adding a functionalizing agent and a corresponding catalyst to the polyhydroxy polymer dispersion of step (1), and performing a functionalizing reaction at 0 to 150° C. for 1 to 12 hours; (3) adding a low-order fatty alcohol to the solution system after the reaction in step (2) to obtain a precipitate, washing and drying to obtain a clean modified polyhydroxy polymer; or, adjusting the pH of the solution system after the reaction in step (2) to neutral, centrifuging and separating, taking the supernatant, dialyzing, and drying to obtain a clean modified polyhydroxy polymer.
4. The vinyl polymer / modified polyhydroxy polymer composite according to claim 3, characterized in that: In step (2), the functionalizing agent is a quaternizing agent or an imidazole agent.
5. The vinyl polymer / modified polyhydroxy polymer composite according to claim 4, characterized in that: The quaternary ammonium agent is selected from at least one of 2,3-epoxypropyltrimethylammonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, N-2,3-epoxypropyldimethyloctylammonium chloride, and N-2,3-epoxypropyldimethyldodecylammonium chloride; and the catalyst corresponding to the quaternary ammonium agent is selected from at least one of potassium hydroxide, sodium hydroxide, rubidium hydroxide, sodium hydride, calcium hydride, sodium carbonate, and potassium carbonate.
6. The vinyl polymer / modified polyhydroxy polymer composite according to claim 4, characterized in that: The imidazolyl reagent is selected from at least one of imidazole aldehyde, imidazole-2-carboxaldehyde, 4-imidazole carboxaldehyde, 4-methylimidazole-5-carboxaldehyde, 1-methyl-2-formylimidazole, 2-methylimidazole-4-carboxaldehyde, 4-bromo-1-methyl-1H-imidazole-5-carboxaldehyde, 1-methyl-4-phenyl-1H-imidazole-5-carboxaldehyde, 1-triphenylmethyl-4-imidazole carboxaldehyde, 4-(imidazole-1-yl)benzaldehyde, and (1H-imidazole-4-yl)-acetaldehyde; when the polyhydroxy polymer is one of PVA, cellulose, lignin, EVOH, and polyethylene glycol, the catalyst corresponding to the imidazolyl reagent is at least one of inorganic acids; when the polyhydroxy polymer is chitosan, the catalyst corresponding to the imidazolyl reagent is acetic acid and / or NaBH4.
7. Use of the vinyl polymer / modified polyhydroxy polymer composite according to any one of claims 1 to 6 in the fields of biomedical materials, packaging materials, electrochemistry, porous membranes, fabrics, and protective equipment.
8. A composite membrane, characterized in that The method comprises the vinyl polymer / modified polyhydroxy polymer composite according to any one of claims 1 to 6.
9. A method for preparing the composite membrane according to claim 8, characterized in that: The vinyl polymer and the modified polyhydroxy polymer are dissolved in a solvent to obtain a blended dispersion, and then the blended dispersion is volatilized at 20 to 180° C. for 1 to 200 hours to obtain the composite membrane material.
10. The method according to claim 9, characterized in that The solvent is at least one of water, ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, o-dichlorobenzene, methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.