Adhesive sheet and polishing pad with adhesive sheet
By using monovinyl in the adhesive layer to replace block copolymers of aromatic compounds with conjugated diene compounds and specific hydroxyl values, the adhesive layer is solved under high temperature and strong acidic or strong alkaline environments. The deviation and peeling problems achieve improved shear strength and slurry resistance at high temperatures and repellent without residual glue.
Patent Information
- Application Number
- CN202180006275.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-21
- Filing Date
- 2021-02-16
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-02-16
AI Technical Summary
The existing double-sided adhesive sheet for fixing abrasive cloth is prone to offset or peeling of the adhesive layer under high temperature and strong acidity or strong alkaline environments, and it is difficult to peel off without residual glue.
The adhesive layer with a monovinyl substituted aromatic compound and a conjugated diene compound block copolymer is used to combine a low hydroxyl value tackifying resin (T1) and a high hydroxyl value tackifying resin (T2) to improve the viscosity. The shear strength and slurry resistance of the mixture layer are achieved, and releasability without residue glue.
The shear strength and slurry resistance of the adhesive layer are significantly improved at high temperatures, ensuring stability in a strong acidic or strong alkaline environment, and achieving a residual glue-free re-peeling effect.
Smart Images

Figure CN114641548B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a pressure-sensitive adhesive sheet and also to a pressure-sensitive adhesive sheet-attached polishing pad having the pressure-sensitive adhesive sheet. Background Art
[0002] In the process of grinding semiconductor wafers, glass substrates for liquid crystals, etc. to a predetermined thickness (e.g., the chemical mechanical polishing (CMP) process), grinding is performed using a grinding cloth fixed to the platform of the grinding machine. In order to fix the grinding cloth to the platform of the grinding machine, a double-sided adhesive sheet is generally used. The double-sided adhesive sheet for fixing the grinding cloth is required to have sufficient adhesive strength to prevent the grinding cloth from peeling off during grinding, and to be able to be peeled off from the platform without residual adhesive when replacing the used grinding cloth.
[0003] As a double-sided adhesive sheet for fixing polishing cloth, for example, Patent Documents 1 and 2 describe a double-sided tape for fixing polishing material, which has a specific heat-activated adhesive on one side of a plastic film support and a removable adhesive layer on the other side of the plastic film support, and the heat-activated adhesive layer serves as a bonding surface with the polishing material.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 6-145611
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 6-172721 Summary of the invention
[0008] Problems to be solved by the invention
[0009] The performance required of double-sided adhesive sheets for fixing polishing cloths is increasing year by year. For example, during polishing, the temperature rises due to frictional heat or strong shearing force is applied, which easily causes the adhesive layer to shift or peel off. In recent years, especially, since strongly acidic or alkaline slurry liquid is used in polishing, the adhesive layer is easily degraded by the influence of acid or alkali, and the adhesive layer is easily shifted or peeled off.
[0010] However, when a high adhesive force is imparted to the adhesive layer by adding a tackifier resin, for example, to prevent displacement or peeling, the adhesive layer tends to adhere more easily, making it difficult to peel off the surface of the plate without leaving any adhesive residue.
[0011] Therefore, there is a need for a double-sided PSA sheet for fixing a polishing cloth that has a higher level of resistance to displacement or peeling when exposed to strong shear force, a strongly acidic or alkaline slurry liquid, etc. at high temperature, and removability that allows the sheet to be re-peeled from a flat plate without leaving any adhesive residue.
[0012] The present invention aims to provide an adhesive sheet having excellent shear strength and slurry resistance at high temperatures and excellent removability that allows the sheet to be re-peeled without residual adhesive. In addition, the present invention aims to provide a polishing pad with an adhesive sheet having the adhesive sheet.
[0013] Means for solving problems
[0014] The present invention is an adhesive sheet having at least one adhesive layer, wherein the adhesive layer contains a base polymer, a tackifier resin (T1) having a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin (T2) having a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less, wherein the base polymer is a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound, and wherein the content of the tackifier resin (T1) in the adhesive layer is 10 parts by weight or more and 60 parts by weight or less based on 100 parts by weight of the base polymer, and the content of the tackifier resin (T2) is 1 part by weight or more and 40 parts by weight or less based on 100 parts by weight of the base polymer.
[0015] Hereinafter, the present invention will be described in detail.
[0016] As the adhesive layer that can be used as the laminating surface of the platform laminating with the grinder, the present inventors etc. have studied the adhesive layer of the block copolymer containing monovinyl substituted aromatic compound and conjugated diene compound as the base polymer. The present inventors etc. have then studied repeatedly for the tackifying resin added into such adhesive layer. As a result, the present inventors etc. have found that by using tackifying resin, especially using the tackifying resin (T1) of the relatively low hydroxyl value that meets a specific range and the tackifying resin (T2) of the relatively high hydroxyl value that meets a specific range respectively with specific content, it is possible to improve the shear strength at high temperature and the slurry resistance and the re-peelability that can be re-peeled without residual glue. Thus, the present invention has been completed.
[0017] The pressure-sensitive adhesive sheet of the present invention is a pressure-sensitive adhesive sheet having at least one pressure-sensitive adhesive layer.
[0018] The pressure-sensitive adhesive layer contains a base polymer. The base polymer is a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound (hereinafter, also referred to simply as a "block copolymer").
[0019] By containing the above-mentioned block copolymer by the above-mentioned adhesive layer, the shear strength of the above-mentioned adhesive layer at high temperature is fully improved. In addition, the polarity of the above-mentioned block copolymer is relatively low, therefore, by containing the above-mentioned block copolymer by the above-mentioned adhesive layer, compared with the situation such as containing acrylic acid polymer, the slurry liquid is not easy to be immersed in the inside of the above-mentioned adhesive layer, and the slurry resistance of the above-mentioned adhesive layer at high temperature is improved. In addition, by containing the above-mentioned block copolymer by the above-mentioned adhesive layer, compared with the situation such as containing natural rubber, the bonding aggravation of the above-mentioned adhesive layer is suppressed, and re-peelability is improved.
[0020] The monovinyl-substituted aromatic compound is not particularly limited, and examples thereof include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-tert-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, vinylxylene, vinylnaphthalene, vinylpyridine, diphenylethylene, and diphenylethylene containing a tertiary amino group. The diphenylethylene containing a tertiary amino group is not particularly limited, and examples thereof include 1-(4-N,N-dimethylaminophenyl)-1-phenylethylene. These monovinyl-substituted aromatic compounds may be used alone or in combination of two or more.
[0021] The above-mentioned conjugated diene compound is not particularly limited, and for example, isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 1,3-heptadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, etc. can be enumerated. These conjugated diene compounds can be used alone or in combination of two or more.
[0022] The block copolymer is not particularly limited as long as it has rubber elasticity at room temperature and has a hard segment portion formed of the monovinyl-substituted aromatic compound and a soft segment portion formed of the conjugated diene compound.
[0023] It should be noted that the block copolymer also includes a hydrogenated product of a block copolymer of the monovinyl-substituted aromatic compound and the conjugated diene compound.
[0024] As the above-mentioned block copolymer, specifically, for example, styrene-isoprene-styrene (SIS) block copolymer, styrene-butadiene-styrene (SBS) block copolymer, styrene-butadiene-butylene-styrene (SBBS) block copolymer, styrene-ethylene-butylene-styrene (SEBS) block copolymer, styrene-ethylene-propylene-styrene (SEPS) block copolymer, hydrogenated styrene-butylene rubber (HSBR), styrene-isobutylene-styrene (SIBS) block copolymer etc. can be cited. Wherein, from the aspect that the bonding aggravation of the above-mentioned adhesive layer is further suppressed, and the re-peelability is further improved, it is preferably SIS block copolymer and SEBS block copolymer, more preferably SIS block copolymer. In addition, from the aspect that the shear strength of the above-mentioned adhesive layer at high temperature is improved, the above-mentioned block copolymer is preferably a hydride. These block copolymers can be used alone, or two or more can be used in combination.
[0025] The block copolymer may contain a diblock copolymer of the hard segment portion and the soft segment portion in addition to the triblock copolymer of the hard segment portion and the soft segment portion.
[0026] The content of the above-mentioned diblock copolymer in the above-mentioned block copolymer is not particularly limited, and the preferred lower limit is 10 weight %, and the preferred upper limit is 40 weight %. If the content of the above-mentioned diblock copolymer is more than 10 weight %, the adhesion of the above-mentioned adhesive layer is further suppressed, and the re-peelability is further improved. If the content of the above-mentioned diblock copolymer is less than 40 weight %, it is possible to prevent the above-mentioned adhesive layer from becoming too hard, the adhesion of the above-mentioned adhesive layer becomes sufficient, and the shear strength and slurry resistance of the above-mentioned adhesive layer at high temperature become more fully high. The more preferred lower limit of the content of the above-mentioned diblock copolymer is 20 weight %, and the more preferred upper limit is 35 weight %.
[0027] The content of the hard segment part in the block copolymer (when the monovinyl-substituted aromatic compound is styrene, also referred to as "styrene content") is not particularly limited, and the preferred lower limit is 5% by weight, and the preferred upper limit is 25% by weight. If the content of the hard segment part is more than 5% by weight, the adhesion of the adhesive layer is further suppressed, and the re-peelability is further improved. If the content of the hard segment part is less than 25% by weight, it is possible to prevent the adhesive layer from becoming too hard, the adhesive force of the adhesive layer becomes sufficient, and the shear strength and slurry resistance of the adhesive layer at high temperature become more fully high. The more preferred lower limit of the content of the hard segment part is 10% by weight, and the more preferred upper limit is 20% by weight.
[0028] The weight average molecular weight of the above-mentioned block copolymer is not particularly limited, and the preferred lower limit is 50,000, and the preferred upper limit is 600,000. If the above-mentioned weight average molecular weight is more than 50,000, the heat resistance of the above-mentioned adhesive layer becomes high, and the shear strength at high temperature further improves. If the above-mentioned weight average molecular weight is less than 600,000, it is possible to prevent the compatibility of the above-mentioned block copolymer with other components from being too reduced. The more preferred lower limit of the above-mentioned weight average molecular weight is 100,000, and the more preferred upper limit is 500,000.
[0029] The weight average molecular weight of the block copolymer refers to the weight average molecular weight measured as a polystyrene conversion molecular weight by gel permeation chromatography (GPC). For the measurement of the weight average molecular weight by GPC, for example, column LF-804 (manufactured by Showa Denko K.K.) can be used as a column.
[0030] The pressure-sensitive adhesive layer contains a tackifier resin (T1) having a hydroxyl value of less than 20 mgKOH / g and a tackifier resin (T2) having a hydroxyl value of 20 mgKOH / g to 120 mgKOH / g.
[0031] The adhesive layer contains a tackifying resin, and the shear strength of the adhesive layer at high temperature is fully improved. In addition, the adhesive layer contains a tackifying resin, especially a tackifying resin (T1) with a relatively low hydroxyl value that satisfies the above range, and a tackifying resin (T2) with a relatively high hydroxyl value that satisfies the above range, so that the slurry resistance of the adhesive layer at high temperature is improved, and the adhesion aggravation is also suppressed, and the re-peelability is improved. The reasons are speculated to be as follows.
[0032] Generally, when a slurry penetrates into the adhesive layer at a high temperature (around 60°C), ionic substances contained in the slurry migrate to the interface between the adhesive layer and the adherend and adsorb to the adherend surface, causing displacement or peeling of the adhesive layer.
[0033] It is believed that in the adhesive sheet of the present invention, the adhesive layer contains the tackifier resin (T2) with a relatively high polarity, so that at high temperatures (at a temperature of about 60° C.), the tackifier resin (T2) will migrate to the interface between the adhesive layer and the adherend, forming a layer containing a large amount of tackifier resin at the interface. It is believed that this layer can prevent the ionic substances contained in the slurry from being adsorbed on the adherend surface, and the slurry resistance of the adhesive layer at high temperatures is improved.
[0034] In addition, when the tackifying resin is only the tackifying resin (T2), although the slurry resistance of the adhesive layer at high temperature is improved, since the polarity of the layer containing a large amount of the tackifying resin is too high, adhesion is easily aggravated, and re-peelability is reduced. In the adhesive sheet of the present invention, the adhesive layer contains the tackifying resin (T1) in addition to the tackifying resin (T2), so that the polarity of the layer containing a large amount of the tackifying resin can be adjusted to a moderate range, and therefore, the slurry resistance of the adhesive layer at high temperature is improved, and adhesion aggravation is also suppressed, and re-peelability is improved.
[0035] The hydroxyl value of the tackifier resin (T1) is not particularly limited as long as it is less than 20 mgKOH / g, and is preferably less than 5 mgKOH / g. The lower limit of the hydroxyl value of the tackifier resin (T1) is not particularly limited, and may be 0 mgKOH / g.
[0036] The hydroxyl value of the tackifier resin refers to the number of mg of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of the tackifier resin is acetylated, and is defined as a value measured based on the potentiometric titration method specified in JIS K0070:1992.
[0037] The softening point of the tackifier resin (T1) is not particularly limited, and the preferred lower limit is 110°C. If the softening point of the tackifier resin (T1) is above 110°C, the heat resistance of the adhesive layer becomes higher, and the shear strength at high temperature is further improved. The more preferred lower limit of the softening point of the tackifier resin (T1) is 115°C. The upper limit of the softening point of the tackifier resin (T1) is not particularly limited, and the actual upper limit is about 160°C.
[0038] The softening point of the tackifier resin refers to the temperature at which the solid resin softens and starts to deform, and is defined as a value measured based on the softening point test method (ring and ball method) specified in JIS K 5902 and JIS K 2207.
[0039] Specific examples of the tackifier resin (T1) include petroleum resins, terpene resins, styrene resins, and hydrogenated products thereof. These tackifier resins (T1) may be used alone or in combination of two or more. Among them, terpene resins are preferred.
[0040] As the above-mentioned petroleum resin, more specifically, for example, aliphatic (C5) petroleum resin, aromatic (C9) petroleum resin, C5 / C9 copolymer petroleum resin, alicyclic petroleum resin, etc. As the above-mentioned terpene resin, more specifically, for example, α-pinene polymer, β-pinene polymer, dipentene polymer and modified terpene resins as modified bodies of these polymers, etc. can be mentioned. As the modification in the above-mentioned modified terpene resin, for example, phenol modification, styrene modification, hydrogenation modification, hydrocarbon modification, etc. can be mentioned. As the above-mentioned modified terpene resin, more specifically, for example, styrene-modified terpene resin, hydrogenated terpene resin, etc. can be mentioned. As the above-mentioned styrene resin, more specifically, for example, styrene homopolymer, α-methylstyrene homopolymer, α-methylstyrene-styrene copolymer, styrene-aliphatic polymer, α-methylstyrene-styrene-aliphatic copolymer, phenol-modified styrene resin, etc. can be mentioned.
[0041] The tackifier resin (T1) may be two or more tackifier resins, in which case the tackifier resin (T1) preferably contains the styrene resin. When the tackifier resin (T1) contains the styrene resin, the shear strength of the adhesive layer at high temperature is further improved.
[0042] The content of the styrene resin in the adhesive layer is not particularly limited relative to 100 parts by weight of the base polymer, but the preferred lower limit is 3 parts by weight, the preferred upper limit is 40 parts by weight, the more preferred lower limit is 5 parts by weight, the more preferred upper limit is 30 parts by weight, the further preferred lower limit is 10 parts by weight, and the further preferred upper limit is 20 parts by weight.
[0043] In the above-mentioned adhesive layer, relative to 100 parts by weight of the above-mentioned base polymer, the lower limit of the content of the above-mentioned tackifying resin (T1) is 10 parts by weight, and the upper limit is 60 parts by weight. If the content of the above-mentioned tackifying resin (T1) is more than 10 parts by weight, the adhesion of the above-mentioned adhesive layer when used in combination with the above-mentioned tackifying resin (T2) is suppressed, and the re-peelability is improved, and the shear strength at high temperature is fully improved. If the content of the above-mentioned tackifying resin (T1) is less than 60 parts by weight, the adhesion of the above-mentioned adhesive layer is suppressed, and the re-peelability is improved. The preferred lower limit of the content of the above-mentioned tackifying resin (T1) is 20 parts by weight, and the preferred upper limit is 50 parts by weight, and the more preferred lower limit is 30 parts by weight, and the more preferred upper limit is 40 parts by weight.
[0044] The hydroxyl value of the tackifier resin (T2) is not particularly limited as long as it is 20 mgKOH / g or more and 120 mgKOH / g or less, and is more preferably 30 mgKOH / g or more and 80 mgKOH / g or less. It should be noted that when a tackifier resin (T3) having a hydroxyl value exceeding 120 mgKOH / g is used to replace the tackifier resin (T2), although the slurry resistance of the adhesive layer at high temperature is improved, bonding is more easily performed and re-peelability is reduced.
[0045] The softening point of the tackifier resin (T2) is not particularly limited, and the preferred lower limit is 120°C. If the softening point of the tackifier resin (T2) is above 120°C, the heat resistance of the adhesive layer becomes higher, and the shear strength at high temperature is further improved. The more preferred lower limit of the softening point of the tackifier resin (T2) is 140°C. The upper limit of the softening point of the tackifier resin (T2) is not particularly limited, and the actual upper limit is about 180°C.
[0046] Specific examples of the tackifier resin (T2) include coumarone resin, terpene phenol resin, rosin resin, rosin derivative resin, etc. These tackifier resins (T2) may be used alone or in combination of two or more.
[0047] As the coumarone resin, for example, a resin containing benzofuran and indene as monomer components constituting the skeleton (main chain) of the resin can be used. Examples of monomer components constituting the skeleton of the resin other than benzofuran and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, and the like.
[0048] The terpene-phenol resin refers to a polymer containing a terpene residue and a phenol residue. In addition, the terpene-phenol resin is a concept including a copolymer of a terpene and a phenol compound (terpene-phenol copolymer resin) and a phenol-modified terpene resin obtained by phenol-modifying a homopolymer or copolymer of terpene (terpene resin, typically an unmodified terpene resin).
[0049] The terpene constituting the terpene-phenol resin is not particularly limited, but preferably is a monoterpene such as α-pinene, β-pinene, limonene, etc. It should be noted that limonene includes d-isomer, 1-isomer, and d / 1-isomer (dipentene).
[0050] More specifically, the rosin resin includes, for example, unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin, and modified rosins obtained by modifying these unmodified rosins. Examples of the modification of the modified rosin include hydrogenation, disproportionation, and polymerization. More specifically, the modified rosin includes, for example, hydrogenated rosin, disproportionated rosin, polymerized rosin, and other chemically modified rosins.
[0051] More specifically, examples of the rosin derivative resin include rosin ester resins obtained by esterifying the rosin resin with alcohols, unsaturated fatty acid-modified rosin resins obtained by modifying the rosin resin with unsaturated fatty acids, and unsaturated fatty acid-modified rosin ester resins obtained by modifying the rosin ester resin with unsaturated fatty acids.
[0052] Examples of the rosin derivative resin include abietol resins obtained by reducing carboxyl groups in the unsaturated fatty acid-modified rosin resin or unsaturated fatty acid-modified rosin ester resin.
[0053] In addition, the rosin derivative resin may include metal salts of the rosin resin or rosin derivative resin (especially rosin ester resin) or rosin phenol resin, etc. The rosin phenol resin is obtained by adding phenol to the rosin resin or rosin derivative resin under an acid catalyst and performing thermal polymerization.
[0054] The above-mentioned tackifying resin (T2) is preferably two or more tackifying resins. Among them, the above-mentioned tackifying resin (T2) is more preferably a coumarone resin. The above-mentioned coumarone resin interacts with the above-mentioned hard segment part in the above-mentioned base polymer, and can stabilize the physical crosslinking between the above-mentioned hard segment parts. Therefore, by the above-mentioned coumarone resin contained in the above-mentioned tackifying resin (T2), the heat resistance and overall (bulk) strength of the above-mentioned adhesive layer become higher, and the shear strength at high temperature is further improved.
[0055] The content of the coumarone resin in the adhesive layer is not particularly limited relative to 100 parts by weight of the base polymer, but the preferred lower limit is 5 parts by weight, the preferred upper limit is 30 parts by weight, the more preferred lower limit is 10 parts by weight, the more preferred upper limit is 20 parts by weight, the further preferred lower limit is 12.5 parts by weight, and the further preferred upper limit is 17.5 parts by weight.
[0056] The tackifier resin (T2) is more preferably at least one tackifier resin selected from terpene phenol resin, rosin resin and rosin derivative resin (hereinafter referred to as "terpene phenol resin, etc."). The tackifier resin (T2) contains the terpene phenol resin, etc., so that the slurry resistance of the adhesive layer at high temperature is further improved. From the aspect of further improving the slurry resistance of the adhesive layer at high temperature, the terpene phenol resin is more preferably the terpene phenol resin.
[0057] The content of the terpene phenol resin etc. in the adhesive layer is not particularly limited relative to 100 parts by weight of the base polymer, but is preferably 1 part by weight at the lower limit and 15 parts by weight at the upper limit, more preferably 5 parts by weight at the lower limit and 10 parts by weight at the upper limit.
[0058] In order to maintain a balance between the shear strength at high temperature and the slurry resistance at high temperature and to improve both, the tackifier resin (T2) particularly preferably contains both the coumarone resin and the terpene phenol resin.
[0059] In the above-mentioned adhesive layer, relative to 100 parts by weight of the above-mentioned base polymer, the lower limit of the content of the above-mentioned tackifying resin (T2) is 1 part by weight, and the upper limit is 40 parts by weight. If the content of the above-mentioned tackifying resin (T2) is more than 1 part by weight, the shear strength of the above-mentioned adhesive layer at high temperatures fully becomes high, and in addition, the slurry resistance at high temperatures improves. If the content of the above-mentioned tackifying resin (T2) is less than 40 parts by weight, the bonding aggravation of the above-mentioned adhesive layer is suppressed, and re-peelability improves. The preferred lower limit of the content of the above-mentioned tackifying resin (T2) is 3 parts by weight, and the preferred upper limit is 35 parts by weight, and the more preferred lower limit is 5 parts by weight, and the more preferred upper limit is 30 parts by weight.
[0060] In the above-mentioned adhesive layer, relative to 100 parts by weight of the above-mentioned base polymer, the total content of the above-mentioned tackifying resin (T1) and the above-mentioned tackifying resin (T2) is not particularly limited, preferably with a lower limit of 20 parts by weight, and a preferred upper limit of 80 parts by weight. If the total content of the above-mentioned tackifying resin (T1) and the above-mentioned tackifying resin (T2) is less than 80 parts by weight, the adhesion of the above-mentioned adhesive layer is suppressed, and the re-peelability is further improved. The more preferred lower limit of the total content of the above-mentioned tackifying resin (T1) and the above-mentioned tackifying resin (T2) is 40 parts by weight, and the more preferred upper limit is 60 parts by weight.
[0061] The adhesive layer may contain a tackifier resin (T3) having a hydroxyl value exceeding 120 mgKOH / g.
[0062] The content of the tackifying resin (T3) is not particularly limited relative to 100 parts by weight of the base polymer, and the preferred upper limit is 5 parts by weight. If the content of the tackifying resin (T3) is less than 5 parts by weight, the adhesion of the adhesive layer is suppressed and the re-peelability is improved. The more preferred upper limit of the content of the tackifying resin (T3) is 2.5 parts by weight, and the further preferred upper limit is 0.1 parts by weight.
[0063] Among them, it is particularly preferred that the pressure-sensitive adhesive layer does not contain the tackifier resin (T3), that is, the content of the tackifier resin (T3) is 0 parts by weight.
[0064] The adhesive layer may further contain additives such as a filler, an anti-aging agent, an antioxidant, and a colorant.
[0065] The thickness of the adhesive layer is not particularly limited, but the preferred lower limit is 20 μm, and the preferred upper limit is 100 μm. If the thickness of the adhesive layer is within the above range, the adhesive force of the adhesive layer becomes sufficient, and the shear strength and slurry resistance of the adhesive layer at high temperature become more sufficiently high. The more preferred lower limit of the thickness of the adhesive layer is 40 μm, and the more preferred upper limit is 85 μm.
[0066] The adhesive sheet of the present invention preferably further comprises a substrate, and has an adhesive layer as described above on one side of the substrate, and more preferably has another adhesive layer on the other side of the substrate. It should be noted that, in such a case, it is preferred that the adhesive layer as described above becomes the bonding surface with the grinding machine platform, and the other adhesive layer becomes the bonding surface with the grinding cloth, grinding material, grinding pad, etc.
[0067] The substrate is not particularly limited, and is preferably a resin film. The resin film is not particularly limited, and examples thereof include polyester resin films, polypropylene resin films, etc. Among them, polyester resin films are preferred from the perspectives of flatness, small thickness deviation, and high strength, and among polyester resin films, polyethylene terephthalate films are more preferred.
[0068] The above-mentioned base material may contain additives such as a filler, an ultraviolet absorber, a light stabilizer, and an antistatic agent within a range that does not impair its physical properties.
[0069] The thickness of the substrate is not particularly limited, and the preferred lower limit is 12 μm, and the preferred upper limit is 300 μm. If the thickness of the substrate is 12 μm or more, it is possible to prevent the substrate from breaking when the adhesive sheet is peeled off again, so the re-peelability of the adhesive sheet is further improved. If the thickness of the substrate is 300 μm or less, it is easy to adjust the pressure when the adhesive sheet is pressed against the adherend, and sufficient bonding strength can be obtained. The more preferred lower limit of the thickness of the substrate is 20 μm, and the more preferred upper limit is 250 μm.
[0070] The above-mentioned additional adhesive layer may have the same composition, thickness, etc. as the above-mentioned adhesive layer, ie, the adhesive layer to be bonded to the polishing machine platen, or may have a different composition, thickness, etc.
[0071] When having a composition different from that of the above-mentioned pressure-sensitive adhesive layer, the other pressure-sensitive adhesive layer preferably contains a pressure-sensitive adhesive commonly used in pressure-sensitive adhesive sheets, such as an acrylic resin pressure-sensitive adhesive, a rubber pressure-sensitive adhesive, a silicone pressure-sensitive adhesive, or a polyurethane pressure-sensitive adhesive.
[0072] The method for producing the pressure-sensitive adhesive sheet of the present invention is not particularly limited. For example, when the pressure-sensitive adhesive sheet has the above-mentioned substrate and pressure-sensitive adhesive layers having the same composition and thickness are provided on both surfaces of the substrate, the following method can be mentioned.
[0073] First, prepare an adhesive solution comprising the block copolymer, the tackifying resin (T1) and the tackifying resin (T2). Next, apply the adhesive solution obtained above to the release treatment surface of the release film on one side and dry it, and make a laminated sheet with an adhesive layer on the release treatment surface of the release film. Make a total of 2 laminated sheets according to the same method. Next, transfer the adhesive layers of the 2 laminated sheets to a substrate and integrate them by lamination, and obtain an adhesive sheet with an adhesive layer on both sides of the substrate.
[0074] Figure 1 A cross-sectional view schematically showing one embodiment of the pressure-sensitive adhesive sheet of the present invention is shown. Figure 1 The adhesive sheet 1 shown has an adhesive layer 3a on one surface of a substrate 2. Figure 2 A cross-sectional view schematically showing another embodiment of the pressure-sensitive adhesive sheet of the present invention is shown. Figure 2 The adhesive sheet 1 shown has an adhesive layer 3a on one surface of a substrate 2 and another adhesive layer 3b on the other surface. The adhesive layers 3a and 3b may have the same composition, thickness, etc., or different compositions, thicknesses, etc.
[0075] It should be noted that Figure 1 and Figure 2 The pressure-sensitive adhesive sheets shown above all have a substrate, but the pressure-sensitive adhesive sheet of the present invention is not limited to such a form and may not have a substrate.
[0076] The use of the adhesive sheet of the present invention is not particularly limited, but it is preferably used to fix a polishing cloth, abrasive material, a polishing pad, etc. to a platform of a grinder in a process of grinding a semiconductor wafer, a glass substrate for liquid crystal, etc. to a predetermined thickness, from the perspective of excellent shear strength and slurry resistance at high temperatures and excellent re-peelability without residual adhesive. As such a grinding process, for example, a chemical mechanical polishing (CMP) process can be cited.
[0077] A polishing pad with a pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive sheet of the present invention and a polishing pad are laminated is also one of the present invention.
[0078] The polishing pad is not particularly limited as long as it is a polishing pad made of an absorbent material, nonwoven fabric, polyurethane, etc. fixed to a platen of a polishing machine, and also includes polishing cloth, polishing material, etc.
[0079] The pressure-sensitive adhesive sheet of the present invention may have only one layer of the polishing pad or may have a plurality of layers of the polishing pad.
[0080] The polishing pad with an adhesive sheet of the present invention is not particularly limited as long as the adhesive sheet of the present invention and the polishing pad described above are laminated, and may further include another adhesive sheet in addition to the adhesive sheet of the present invention and the polishing pad described above.
[0081] Figure 3 A cross-sectional view schematically showing a state in which one embodiment of the polishing pad with an adhesive sheet of the present invention is bonded to a platen is shown. Figure 3 The polishing pad 5 with an adhesive sheet shown is obtained by laminating an adhesive sheet 1 and a polishing pad 4, and the adhesive sheet 1 side is fixed to the platform 6 of the polishing machine. The adhesive sheet 1 has an adhesive layer 3a on one side of the substrate 2 and another adhesive layer 3b on the other side. The adhesive layers 3a and 3b may have the same composition, thickness, etc., or may have different compositions, thicknesses, etc., and at least the adhesive layer 3b as the bonding surface with the platform 6 may be the adhesive layer as described above.
[0082] Effects of the Invention
[0083] According to the present invention, a PSA sheet having excellent shear strength and slurry resistance at high temperatures and excellent removability that can be re-peeled without residual adhesive can be provided. In addition, according to the present invention, a PSA sheet-attached polishing pad having the PSA sheet can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0084] Figure 1 This is a cross-sectional view schematically showing one embodiment of the pressure-sensitive adhesive sheet of the present invention.
[0085] Figure 2 This is a cross-sectional view schematically showing another embodiment of the pressure-sensitive adhesive sheet of the present invention.
[0086] Figure 3 This is a cross-sectional view schematically showing a state in which one embodiment of the polishing pad with an adhesive sheet of the present invention is bonded to a platen. DETAILED DESCRIPTION
[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0088] As block copolymers, SIS (styrene-isoprene-styrene block copolymers) 1 to 3 manufactured by Zeon Co., Ltd., SEBS (styrene-ethylene butylene-styrene copolymer) 1 manufactured by JSR Co., Ltd., and natural rubber were used as shown in Table 1. As natural rubber, Crepe Rubber No. 1 manufactured by Toyota Tsusho Corporation was used.
[0089] [Table 1]
[0090]
[0091] As tackifying resins, tackifying resin (T1), tackifying resin (T2) and tackifying resin (T3) shown in Table 2 below were used. It should be noted that C5-based petroleum resin M-100 is manufactured by Arakawa Chemical Industries, Ltd., terpene resins PX1000 and PX1150 are manufactured by YASUHARA Chemical, and styrene resin FTR2120 is manufactured by Mitsui Chemicals, Inc. Coumarin resin V-120 is manufactured by Nippon Coating Chemical Co., Ltd., terpene phenol resins T-130, T-160, S-145 and G-150 are manufactured by YASUHARA Chemical, and rosin ester resin A-125 is manufactured by Arakawa Chemical Industries, Ltd.
[0092]
[0093] (Example 1)
[0094] As shown in Table 3 below, 10 parts by weight of a tackifying resin (T1) and 15 parts by weight of a tackifying resin (T2) were added to 100 parts by weight of a block copolymer and stirred to prepare an adhesive solution. A polyethylene terephthalate film with one side subjected to demolding treatment was prepared. The adhesive solution obtained above was applied to the demolding treatment surface of the polyethylene terephthalate film in a manner such that the thickness after drying became 50 μm, and dried at 110° C. for 5 minutes to prepare a laminate having an adhesive layer on the demolding treatment surface of the polyethylene terephthalate film. A total of 2 laminates were prepared in the same manner.
[0095] A polyethylene terephthalate film was prepared as a substrate. One laminated sheet was laminated on one side of the substrate in a manner that its adhesive layer was in a state opposite to the substrate, the adhesive layer was transferred to the substrate, and the laminated sheets were integrated, and another laminated sheet was laminated on the other side of the substrate in a manner that its adhesive layer was in a state opposite to the substrate, the adhesive layer was transferred to the substrate, and the laminated sheets were integrated to obtain a double-sided adhesive sheet having adhesive layers with a thickness of 50 μm on both sides of the substrate.
[0096] (Examples 2 to 21, Comparative Examples 1 to 5)
[0097] A double-sided PSA sheet was obtained in the same manner as in Example 1 except that the types and amounts of the block copolymer, tackifier resin (T1), tackifier resin (T2), and tackifier resin (T3) were changed as shown in Table 3 or 4.
[0098] <Evaluation>
[0099] The double-sided PSA sheets obtained in Examples and Comparative Examples were evaluated as follows.
[0100] (1) Evaluation of removability
[0101] The double-sided adhesive sheet was cut into 25mm×75mm, the release film on one side was peeled off, and it was pasted to a polyethylene terephthalate (PET) film with a thickness of 23μm as a liner to prepare a test piece. Under a 23°C environment, the release film covering the other adhesive surface of the test piece was peeled off, and the test piece was crimped to the surface of a stainless steel (SUS304) plate by moving a 2kg roller back and forth once. It was allowed to stand for 20 minutes in the same environment to obtain a test sample before heat treatment. The test sample before heat treatment was allowed to stand for 7 days in an atmosphere of 60°C to obtain a test sample after heat treatment. For the test samples obtained before and after heat treatment, the following method was used to evaluate the residual glue and determine the adhesion aggravation rate.
[0102] (Evaluation of residual adhesive)
[0103] After the double-sided adhesive sheet of the test sample after the heat treatment was peeled off, the presence or absence of adhesive residue was observed on the stainless steel plate.
[0104] (Determination of adhesion aggravation rate)
[0105] In an atmosphere of 23°C, the double-sided PSA sheet of the test sample before and after the heat treatment was peeled off in the 180° direction at a speed of 300 mm / min using a tensile tester in accordance with JIS Z 0237, and the 180° peel strength was measured. The adhesion strength of the double-sided PSA sheet was calculated from the 180° peel strength before and after the heat treatment using the following formula.
[0106] Adhesion aggravation rate (%) = {(180° peel strength after heating treatment) / (180° peel strength before heating treatment)-1}×100
[0107] It should be noted that the adhesion aggravation rate was calculated only when there was no residual adhesive in the residual adhesive evaluation.
[0108] In the residual adhesive evaluation, the case where there was no residual adhesive and the adhesion enhancement rate was less than 5% was marked as ◎, the case where there was no residual adhesive and the adhesion enhancement rate was 5% or more was marked as ○, and the case where there was residual adhesive was marked as ×.
[0109] (2) Evaluation of slurry resistance
[0110] The double-sided adhesive sheet was cut into 25 mm × 75 mm, the release film on one side was peeled off, and the test piece was pasted to a polyethylene terephthalate (PET) film with a thickness of 23 μm as a liner. Under a 23°C environment, the release film covering the other adhesive surface of the test piece was peeled off, and the test piece was pressed onto the surface of a stainless steel (SUS304) plate by rolling a 2 kg roller back and forth once to obtain a test sample before immersion in a chemical solution.
[0111] Semi-Sperse 25 (manufactured by Cabot Microelectronics) was diluted with ion exchange water to a ratio of 1:1 to prepare an alkaline chemical solution. The test sample before immersion in the chemical solution was immersed in the alkaline chemical solution for 7 days under an atmosphere of 60°C. Then, the test sample was taken out from the alkaline chemical solution, washed with ion exchange water, and dried at 23°C for 1 hour to obtain a test sample after immersion in the chemical solution.
[0112] For the obtained test samples before and after the immersion in the chemical solution, the peeling after the immersion in the chemical solution and the change rate of the 180° peel strength were evaluated by the following method.
[0113] (Evaluation of peeling after chemical solution immersion)
[0114] After the test sample was immersed in the chemical solution, the double-sided adhesive sheet was observed to see if it peeled off from the stainless steel plate. The case where there was no peeling of the double-sided adhesive sheet was indicated as "none", the case where only the edge of the double-sided adhesive sheet was slightly peeled off was indicated as "edge", and the case where the entire surface of the double-sided adhesive sheet was peeled off was indicated as "complete peeling".
[0115] (Determination of 180° peel strength change rate)
[0116] In an atmosphere of 23°C, according to JIS Z 0237, the double-sided adhesive sheet of the test sample before and after chemical solution immersion was peeled off in the 180° direction at a speed of 300 mm / min using a tensile tester to measure the 180° peel strength. The change rate (%) of the 180° peel strength of the adhesive layer before and after chemical solution immersion was calculated by the following formula.
[0117] Change rate (%) = {(180° peel strength after immersion in alkaline chemical solution) / (180° peel strength before immersion in alkaline chemical solution)-1}×100
[0118] The 180° peel strength change rate was calculated only when the double-sided PSA sheet did not peel or only slightly peeled at the edge in the evaluation of peeling after chemical solution immersion (when judged as “none” or “edge”).
[0119] The case where the peeling after immersion in the chemical solution was evaluated as "none" and the change rate of the 180° peel strength decreased by less than 20% was recorded as ◎, the case where the peeling after immersion in the chemical solution was evaluated as "none" but the 180° peel strength decreased by more than 20%, or the case where the peeling after immersion in the chemical solution was evaluated as "end" was recorded as ○, and the case where the peeling after immersion in the chemical solution was evaluated as "complete peeling" was recorded as ×.
[0120] (3) Determination of shear strength
[0121] The double-sided adhesive sheet was cut into 15 mm × 15 mm pieces, the release film on one side was peeled off, and a 2 kg roller was used to press the surface of a stainless steel (SUS304) plate to prepare a test piece. The release film covering the other adhesive surface of the test piece was peeled off at 23°C, and the test piece was heated at 80°C at 3 kg / cm 2 The test piece was thermally pressed onto the surface of a stainless steel (SUS304) plate at a pressure of 10 seconds to obtain a test sample. The double-sided adhesive sheet of the test sample was peeled off at a speed of 10 mm / min in the direction of the shear stress applied in an atmosphere of 60°C to measure the shear strength.
[0122] The case where the shear strength is 160 [N / 15×15mm] or more is recorded as ◎, the case where the shear strength is less than 160 [N / 15×15mm] and 120 [N / 15×15mm] or more is recorded as ○, the case where the shear strength is less than 120 [N / 15×15mm] and 80 [N / 15×15mm] or more is recorded as Δ, and the case where the shear strength is less than 80 [N / 15×15mm] is recorded as ×.
[0123]
[0124] It should be noted that Examples 6 and 14 were judged as ○ in the evaluation of removability (no residual adhesive in the evaluation of residual adhesive, and the adhesion enhancement rate was 5% or more), but the adhesion enhancement rate exceeded 20%.
[0125]
[0126] Industrial Applicability
[0127] According to the present invention, a PSA sheet having excellent shear strength and slurry resistance at high temperatures and excellent removability that can be re-peeled without residual adhesive can be provided. In addition, according to the present invention, a PSA sheet-attached polishing pad having the PSA sheet can be provided.
[0128] Description of Reference Numerals
[0129] 1 Adhesive sheet
[0130] 2. Substrate
[0131] 3a, 3b Adhesive layer
[0132] 4 Abrasive pad
[0133] 5 Abrasive pad with adhesive sheet
[0134] 6 Platform (Grinding Machine)
Claims
1. An adhesive sheet, characterized in that: It has at least one adhesive layer, The adhesive layer contains a base polymer, a tackifier resin T1 having a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin T2 having a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less. The base polymer is a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound, In the adhesive layer, the content of the tackifier resin T1 is 10 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the base polymer, and the content of the tackifier resin T2 is 1 part by weight or more and 40 parts by weight or less relative to 100 parts by weight of the base polymer, In the block copolymer, the content of the diblock copolymer is 10 wt % or more and 40 wt % or less, The tackifying resin T2 contains coumarone resin and terpene phenol resin, The content of the coumarone resin is 5 parts by weight or more and 30 parts by weight or less relative to 100 parts by weight of the base polymer in the adhesive layer.
2. The adhesive sheet according to claim 1, characterized in that The softening point of the tackifier resin T1 is 110° C. or higher.
3. The adhesive sheet according to claim 1 or 2, characterized in that: The softening point of the tackifier resin T2 is 120° C. or higher.
4. The adhesive sheet according to claim 1 or 2, characterized in that: The tackifying resin T2 is two or more tackifying resins.
5. The adhesive sheet according to claim 1 or 2, characterized in that: The tackifying resin T1 contains a terpene resin.
6. The adhesive sheet according to claim 1 or 2, characterized in that: The tackifier resin T1 contains a styrene resin.
7. The adhesive sheet according to claim 6, characterized in that In the adhesive layer, the content of the styrene resin is 3 parts by weight or more and 40 parts by weight or less relative to 100 parts by weight of the base polymer.
8. The adhesive sheet according to claim 1 or 2, characterized in that: In the pressure-sensitive adhesive layer, the total content of the tackifier resin T1 and the tackifier resin T2 is 20 parts by weight or more and 80 parts by weight or less relative to 100 parts by weight of the base polymer.
9. The adhesive sheet according to claim 1 or 2, characterized in that: In the adhesive layer, the content of the tackifier resin T3 having a hydroxyl value exceeding 120 mgKOH / g is 5 parts by weight or less based on 100 parts by weight of the base polymer.
10. The adhesive sheet according to claim 1 or 2, characterized in that: The block copolymer is a styrene-isoprene-styrene block copolymer or a styrene-butadiene-styrene block copolymer.
11. The adhesive sheet according to claim 1 or 2, characterized in that: In the block copolymer, the content of the diblock copolymer is 10 wt % or more and 35 wt % or less.
12. The adhesive sheet according to claim 1 or 2, characterized in that: The content of the hard segment part in the block copolymer is 5% by weight or more and 25% by weight or less.
13. The adhesive sheet according to claim 1 or 2, characterized in that: The block copolymer has a weight average molecular weight of 50,000 or more and 600,000 or less.
14. The adhesive sheet according to claim 1 or 2, characterized in that: The block copolymer is a hydrogenated product.
15. The adhesive sheet according to claim 1 or 2, characterized in that: The adhesive layer has a thickness of 20 μm or more and 100 μm or less.
16. The adhesive sheet according to claim 1 or 2, characterized in that: It also has a substrate, with the adhesive layer on one side of the substrate and another adhesive layer on the other side of the substrate.
17. The adhesive sheet according to claim 1 or 2, characterized in that: It also has a substrate having a thickness of 12 μm or more and 300 μm or less.
18. The adhesive sheet according to claim 1 or 2, characterized in that: It is used to fix the polishing cloth, polishing material, and polishing pad to the table of the polishing machine in the process of polishing semiconductor wafers and glass substrates for liquid crystals to a predetermined thickness.
19. A polishing pad with an adhesive sheet, characterized in that: The adhesive sheet according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18 and a polishing pad are laminated.