A ball mold matrix manufacturing process
Through forging molding and continuous drive friction welding technology, the problems of environmental pollution and high costs in the production of ball mold matrix are solved, processing efficiency and quality are improved, and market demand is met.
Patent Information
- Application Number
- CN202210204973.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-02
AI Technical Summary
The existing ball mold matrix production process has problems such as environmental pollution, poor labor environment for operators, low production efficiency and high cost of mechanical processing, and it is difficult to keep up with market demand.
The forging molding process and continuous drive friction welding technology are adopted to calculate the parameters of the forging molding mold, select appropriate raw materials, perform forging molding and welding connections, and combine heat treatment and mechanical processing to reduce waste and dust generation and reduce production costs.
It has achieved pollution-free production, improved processing quality and efficiency, reduced raw material waste and production costs, improved workers' working environment, and enhanced market competitiveness.
Smart Images

Figure CN114653876B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ball mold matrix manufacturing technology, and in particular to a ball mold matrix manufacturing technology. Background Art
[0002] A ball mold substrate is required for optical lens processing. The ball mold substrate has a large total market demand, but a small number of single size specifications are required (generally 1-2 pieces of a single size specification). In addition, the SR and SD specifications of the working surface of the substrate are random, with a wide range of values (common SR absolute values 0-6000.000mm SD>1-SD<400mm), an extremely low repetition rate, and is a single-piece customized product with few types of connecting parts and a high size matching rate.
[0003] The existing production of ball mold bases is to use cast iron, brass, aluminum and other metal casting blanks, and carbon steel, brass, aluminum and other metal materials are made of rods. The production is carried out by sand casting and lost foam casting. In the lost foam casting method, the main materials are expandable polystyrene resin and expandable methyl methacrylate resin during the production process, which will cause a large amount of waste gas and waste from the casting blank, causing environmental pollution. Dust is generated during the mechanical processing, which makes the working environment of the operators extremely poor, increases the incidence of occupational diseases such as silicosis, makes procurement difficult, and has a long production cycle, which cannot keep up with market demand. Carbon steel, brass, aluminum and other metal materials are made of rods in the production process, which wastes more than 2 / 3 of the raw materials, has low mechanical processing production efficiency, high cost, and is not competitive in the market. Summary of the invention
[0004] In view of the defects in the prior art, the purpose of the present invention is to provide a ball mold base manufacturing process, which solves the problems of environmental pollution, poor working environment for operators, low machining production efficiency, high cost, and poor market competitiveness caused by the existing ball mold base manufacturing process.
[0005] The technical solution adopted by the present invention is: a ball mold matrix manufacturing process, comprising the following steps:
[0006] S1. Calculate forging die parameters: Calculate the minimum range of the common relationship of the dimensions of the working parts of the ball mold base based on the production data, and take the SH segment and SD segment of the working part of the ball mold base as 10mm, where the SH segment increases by 10mm each level from 0mm, and the SD segment increases by 10mm each level. According to the above data, a list of forming die parameters is drawn up.
[0007] S2. Raw material selection: Select raw materials according to production requirements before cutting, and cut according to the proposed molding die parameter list.
[0008] S3. Forging of the working part of the ball mold base: According to the raw material properties, SH and SD values, determine whether to select a forging die for one-time or multiple forming, and heat the blank before forging.
[0009] S4. Ball mold base connection: Welding is carried out according to the shape of the ball mold base, and the working part and the connecting part of the ball mold base are connected by continuous drive friction welding.
[0010] S5. Heat treatment: perform joint annealing treatment on the connection position between the working part and the connection part of the ball mold base to eliminate joint stress.
[0011] S6. Machining: Use machining to remove burrs and process them into finished products that meet production requirements.
[0012] In the above process, the open forming mold can be combined with the SH segment number and the mold can be made according to the maximum machinable SD with machining allowance. The forming mold can be used to place the blank quickly, safely and accurately in the appropriate position of the forming mold. The mold investment is small, and the dimensional wear and tear can be repaired multiple times, with the lowest cost.
[0013] Furthermore, in S2, the blanking material is a round plate with a thickness of 15-30 mm.
[0014] Furthermore, in S2, the raw materials are cut by sawing machine before cutting.
[0015] Furthermore, in S2, the ball mold base connecting part and the ball mold base working part can be made of the same material or different materials according to the weldability of the materials.
[0016] Furthermore, in S3, the blank is heated by a medium frequency power supply, wherein the heating temperature is 700-950 degrees.
[0017] Furthermore, in S3, the blank is heated and then forged using a press.
[0018] Further, in S4, welding is performed according to the shape of the ball mold substrate, the spindle speed of the friction welding machine is 2000 r / min, and the friction pressure and the upset pressure are 45 KN and 100 KN respectively.
[0019] Furthermore, in S4, the friction time of friction welding is 25 s, and the holding time is 5-10 s.
[0020] Furthermore, in S5, the heat treatment temperature is 760 degrees, the holding time is 90 minutes, and the temperature is cooled to 200 degrees with the furnace cooling and then air-cooled.
[0021] The beneficial effects of the present invention are as follows: the present invention solves the problems of the existing integral casting ball mold base using sand casting, combustion pollution during lost foam casting, and large investment and high cost of lost foam mechanical processing and lost foam closed molding molds. The mold investment of open molding is small, and the dimensional wear and tear can be repaired many times, and the cost is relatively the lowest. There is no casting pollution emission in the production and manufacturing, and the thermoplastic forging molding of metals and the thermoplastic welding properties of dissimilar materials are fully utilized and friction welding is used to achieve the purpose of saving precious materials; in addition, the ball mold base produced by the present invention adopts forging molding, which has the characteristics of low cost, less processes, saving raw materials, etc., can improve the processing quality, precision and efficiency, and the operation and control are simple and flexible, which can fundamentally solve the environmental pollution emissions generated in the production process of this type of products from the supply and demand relationship. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0023] Figure 1 A three-dimensional flow chart of the ball mold matrix manufacturing process provided by an embodiment of the present invention.
[0024] Figure 2 A spherical mold base structure diagram of a spherical mold base provided in an embodiment of the present invention.
[0025] Figure 3 The working part structure of the ball mold base of the ball mold base provided by the embodiment of the present invention Figure 1 .
[0026] Figure 4 The working part structure of the ball mold base of the ball mold base provided by the embodiment of the present invention Figure 2 .
[0027] Figure 5 The working part structure of the ball mold base of the ball mold base provided by the embodiment of the present invention Figure 3 .
[0028] Reference numerals: ball mold base working part 100 , ball mold base connecting part 200 . DETAILED DESCRIPTION
[0029] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.
[0030] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.
[0031] like Figures 1 to 5 As shown, an embodiment of the present invention provides a ball mold matrix manufacturing process, comprising the following steps:
[0032] Step 1. Calculate forging die parameters: Calculate the minimum range of the common relationship of the dimensions of the working parts of each ball mold base based on production data. Usually, the SH absolute value of the common ball mold base is 0-70mm. Therefore, the SH segment and SD segment of the working part 100 of the ball mold base are 10mm, where the SH segment increases by 10mm per level from 0mm, and the SD segment increases by 10mm per level. According to the above data, a list of molding die parameters is drawn up, and the molding die cavity is made according to the shape of the working part of the ball mold base, so that the molding die can be reused many times. In actual application, the SR parameter is calculated based on the SD and SH values.
[0033] Step 2. Raw material selection: Cut the materials according to the proposed molding die parameter list, and select the raw materials according to the production requirements before cutting. According to the production requirements, the physical properties of the materials need to be considered, and the raw materials for cutting are round plates with a thickness of 15-30mm. The round plates can be cut to the corresponding size using sawing equipment. In addition, the connecting part of the ball mold base and the working part of the ball mold base can be made of the same or different materials according to the weldability of the materials, such as cast iron, brass, aluminum, etc.
[0034] Step 3. Forging the working part of the ball mold base: According to the raw material properties, SH and SD values, determine the one-time or multiple-time forming and select the forging die, heat the blank and then forge it; the blank is heated by a medium frequency power supply, and the heating temperature is 700-950 degrees.
[0035] Step 4. Ball mold base connection: The working part of the ball mold base is connected to the connecting part by continuous drive friction welding. Under the action of constant or increasing pressure and torque, the relative movement between the welding contact end faces is used to generate friction heat and plastic deformation heat on the friction surface and its vicinity, so that the temperature of the vicinity rises to a temperature range close to but generally lower than the melting point, the deformation resistance of the material is reduced, the plasticity is improved, and the oxide film on the interface is broken. Under the action of the upsetting pressure, the material produces plastic deformation and flow, and solid-state welding is achieved through molecular diffusion and recrystallization at the interface. When performing friction welding, the spindle speed of the friction welding machine is 2000r / min, the friction pressure and upsetting pressure are 45KN and 100KN respectively, the friction time of friction welding is 25s, and the pressure holding time is 5-10s. In addition, the end face diameter of the joint should be 20mm.
[0036] Step 5. Heat treatment: perform joint annealing treatment on the connection position between the working part 100 and the connection part 200 of the ball mold base to eliminate joint stress; during the heat treatment process, the heat treatment temperature is 760 degrees, the insulation time is 90 minutes, and the temperature is cooled to 200 degrees with the furnace and then air-cooled.
[0037] Step 6. Mechanical processing: Use mechanical equipment to remove burrs and process them into finished products that meet production requirements.
[0038] In the above process, the open forming mold is combined with the SH segment number, and the mold is made according to the maximum machinable SD with a processing allowance. The blank placement locator is made in conjunction with the forming mold and the blank SD, so that the blank can be placed in the appropriate position of the forming mold quickly, safely and accurately. The mold investment is small, and the dimensional wear and tear can be repaired multiple times, with the lowest cost, which solves the problem of large mold investment and high cost of existing closed forming molds.
[0039] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A ball mold matrix manufacturing process, characterized in that; The steps include: S1. Calculate forging die parameters: Calculate the minimum range of the common relationship of the dimensions of the working parts of the ball mold base according to the production data, and take the SH segment and SD segment of the working part of the ball mold base as 10mm, where the SH segment increases by 10mm each step from 0mm, and the SD segment increases by 10mm each step. According to the above data, a list of forming die parameters is drawn up; S2. Raw material selection: Cut the working part of the ball mold base according to the proposed molding die parameter list and product specification requirements, and select the raw materials according to production requirements before cutting; S3. Forging of the working part of the ball mold base: Determine the selection of a forging die for one-time or multiple-time forming according to the raw material properties, SH and SD values, and heat the blank before forging; S4. Ball mold base connection: welding according to the shape of the ball mold base, using continuous drive friction welding to connect the working part of the ball mold base with the connecting part; S5. Heat treatment: annealing the joint between the working part and the connecting part of the ball mold base to eliminate joint stress; S6. Machining: Use machining to remove burrs and process them into finished products that meet production requirements.
2. The ball mold matrix manufacturing process according to claim 1, characterized in that; In S2, the blanking material is a round plate with a thickness of 15-30 mm.
3. The ball mold matrix manufacturing process according to claim 1, characterized in that; In S2, the raw materials are cut by sawing machine and then cut.
4. The ball mold matrix manufacturing process according to claim 1, characterized in that: In S2, the connecting part of the ball mold base and the working part of the ball mold base are made of the same material or different materials according to the weldability of the materials.
5. The ball mold matrix manufacturing process according to claim 1, characterized in that; In S3, the blank is heated by a medium frequency power supply, wherein the heating temperature is 700-950 degrees.
6. The process for manufacturing a ball mold matrix according to claim 1, characterized in that: In S3, the blank is heated and then forged using a press.
7. The ball mold matrix manufacturing process according to claim 1, characterized in that; In S4, the spindle speed of the friction welding machine is 2000r / min, and the friction pressure and upsetting pressure are 45KN and 100KN respectively.
8. The ball mold matrix manufacturing process according to claim 1, characterized in that; In S4, the friction time of friction welding is 25s and the holding time is 5-10s.
9. The process for manufacturing a ball mold matrix according to claim 1, characterized in that: In S5, the heat treatment temperature is 760 degrees, the holding time is 90 minutes, and the temperature is cooled to 200 degrees with the furnace and then air-cooled.