Metallized aramid honeycomb material, preparation method and application thereof

The method of forming an iron-nickel coating through cleaning, activation and chemical plating solves the complex problem of preparing existing electromagnetic shielding honeycomb core materials, realizes the metallization of aramid honeycomb, and obtains a product with excellent corrosion resistance, air permeability and shielding performance. Metallized aramid honeycomb material.

CN114672794BActive Publication Date: 2024-10-29LUOYANG INST OF CUTTING EDGE TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011568899.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-29
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

The existing electromagnetic shielding honeycomb core material preparation method is complicated and cannot meet the modern needs of breathability and electromagnetic wave shielding at the same time.

Method used

Using cleaning, activation and electroless plating methods, an iron-nickel coating is formed on the surface of the aramid honeycomb to achieve metallization of the aramid paper honeycomb, resulting in metallization with good corrosion resistance, good air permeability, high plane compression strength and excellent shielding performance. Aramid paper honeycomb material.

Benefits of technology

The preparation process of the honeycomb core material is simplified, the corrosion resistance, air permeability and shielding performance of the material are improved, and the requirements for air permeability and electromagnetic wave shielding are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a metallized aramid honeycomb material, a preparation method and application thereof. The preparation method comprises step S1, cleaning the aramid honeycomb to obtain a clean aramid honeycomb; step S2, activating the clean aramid honeycomb to obtain an active aramid honeycomb; step S3, placing the active aramid honeycomb in a chemical iron-nickel plating solution for chemical plating to form an iron-nickel coating on the inner surface of the active aramid honeycomb. The above cleaning can remove small solid particles such as dust attached to the surface of the aramid honeycomb and stains such as mineral oil or grease adhered to the pore wall; the activation treatment can make it easier to deposit an iron-nickel coating on the surface of the aramid honeycomb; and finally, chemical plating is performed to form a uniform iron-nickel coating on the surface of the active aramid honeycomb, thereby realizing the metallization of the aramid paper honeycomb. The preparation method of the metallized aramid honeycomb material of the present application is simple, and the obtained metallized aramid paper honeycomb material has good corrosion resistance, good air permeability, high plane compression strength and excellent shielding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electromagnetic shielding technology, and in particular to a metallized aramid honeycomb material, a preparation method and application thereof. Background Art

[0002] With the continuous development and improvement of research technology, various types of shielding materials have been developed and applied one after another. The electromagnetic shielding materials currently used can be divided into airtight and breathable types according to their air permeability. For instruments and equipment such as chassis with vents, which require ventilation and air permeability while shielding electromagnetic waves, air-permeable electromagnetic shielding materials must be selected. At present, the commonly used air-permeable electromagnetic shielding materials are mainly metal mesh and waveguide windows; and foam metal with excellent shielding performance, light weight and air permeability is a new type of electromagnetic shielding material developed in recent years. It not only has the good conductivity or magnetism of metal materials, but also because of its porous structure inside, electromagnetic waves can have multiple reflection losses inside its pores, so that it has higher electromagnetic wave shielding ability than two-dimensional metal mesh, and can even achieve the shielding effect of waveguide windows.

[0003] Electromagnetic shielding refers to blocking the electromagnetic wave propagation path from the electromagnetic pollution source to the designated area, thereby reducing or eliminating the adverse effects of the pollution source on sensitive equipment, devices or human body in the designated area. According to the different working principles of shielding, it can be divided into three categories: electrostatic shielding, magnetic shielding and electromagnetic shielding. Among them, electrostatic shielding and magnetic shielding are just two special types of electromagnetic shielding.

[0004] The shielding ability and effect of various shielding materials on external electromagnetic waves are usually expressed in shielding effectiveness (SE). The unit of SE is decibel (dB). The shielding effectiveness of electromagnetic materials is calculated using the Schelkunoff formula:

[0005] SE=SE R +SE A +SE M .

[0006] Where SE R is the reflection loss, SE A is the absorption loss, SE M It is multiple reflection loss. Reflection loss is caused by the impedance mismatch between the shielding material and the space medium, and is the result of the interaction between the charged particles in the material and the electromagnetic field; absorption loss is caused by the heat loss generated by the interaction between the magnetic dipole or electric dipole and the electromagnetic field; and multiple reflection loss is caused by the inhomogeneity inside the shield.

[0007] As a special composite material structure, aramid paper honeycomb core material has the characteristics of high specific strength, good shock absorption, and good thermal insulation. Its continuous porous structure can also make electromagnetic waves absorb, reflect and scatter multiple times in the honeycomb core layer. In addition, paper honeycombs are cheap and have high economic benefits. In view of the above advantages of honeycomb core materials, honeycomb core materials are not only widely used in civil and construction fields, but also occupy an important position in aviation and aerospace fields.

[0008] In addition, due to the advantages of honeycomb such as high specific stiffness and low relative density, the honeycomb sandwich structure has strong design and simple processing and molding, and has been increasingly widely used in aerospace and rail transportation. Considering the large-scale use of honeycomb sandwich structures in the main structure of aircraft cabins, the rational development of honeycomb core materials with electromagnetic shielding functions can effectively protect the precision instruments and passengers in the aviation flight cabin from electromagnetic interference, realize the structural and functional integrated design of aviation core materials, and improve the space utilization of honeycomb core materials as a whole, thereby achieving the purpose of intelligent lightweight design and functional integrated application of core materials. With the rapid development of electronic science and cutting-edge technology, the application of honeycomb sandwich composite materials with shielding properties in modern electronic countermeasure technology is no longer limited to the fields of national defense aircraft and ship equipment, but has expanded to civil technologies such as communication base stations, vehicle-mounted, and indoor radar covers.

[0009] The hexagonal honeycomb structure that imitates the natural honeycomb is widely used as the core material of the sandwich structure because of its light weight, high strength and high rigidity. When the radar wave enters the sandwich structure from the wave-transmitting layer, the sandwich cavity scatters and absorbs it multiple times, maximally attenuating the radar wave energy and thus achieving broadband and high-intensity shielding and wave-absorbing effects.

[0010] Electromagnetic shielding is a measure used to weaken the electromagnetic field caused by certain emission sources in a certain area of ​​space. In most cases, the shield can be made of metals such as copper, aluminum, and steel, but for constant and lower frequency magnetic fields, ferrite and other materials can also be used as shields. When the electromagnetic wave reaches the surface of the shield, the incident wave is reflected due to the discontinuity of impedance at the interface between air and metal. This reflection does not require the shielding material to have a certain thickness, but only requires discontinuity at the interface; the energy that is not reflected by the surface and enters the shield is attenuated by the shielding material during the forward propagation process in the body, which is the so-called absorption. The remaining energy that has not yet attenuated in the shield, when it is transmitted to the other surface of the material, encounters the interface of metal-air impedance discontinuity, will be reflected again, and return to the shield. This reflection may be reflected multiple times at the interface between the two metals. In short, the attenuation of electromagnetic waves by electromagnetic shielding is mainly based on the reflection and absorption of electromagnetic waves.

[0011] The Chinese patent application with application number 201710266357.8 discloses an electromagnetic shielding honeycomb core material, its preparation method and implantation tooling. In the cavity of each honeycomb unit of the present invention, there are 1 to 5 layers of parallel electromagnetic shielding membranes; the steps of implanting the electromagnetic shielding membranes are as follows: selecting a honeycomb matrix; manufacturing an electromagnetic shielding membrane blank; implanting the electromagnetic shielding membrane blank. The implantation tooling of the invention is composed of an upper handle and a lower implantation rod connected. Due to the limitation of its tooling, the invention cannot be industrialized and applied in batches.

[0012] The Chinese patent application with application publication number CN108724822A discloses a method for preparing an electromagnetic shielding honeycomb core material, which adopts the method of preparing a graphene / ferrite hybrid material, and uniformly attaching the graphene / ferrite hybrid particles to a fabric carrier by magnetic deposition to form a graphene / ferrite hybrid particle electromagnetic shielding fabric. The electromagnetic shielding interlayer is prepared by using prepreg, adhesive film, and electromagnetic shielding fabric. Finally, the electromagnetic shielding interlayer and the honeycomb core material are composited into a sandwich electromagnetic shielding honeycomb structure by gluing. This technology realizes the low-cost design, manufacturing and technical integration and comprehensive utilization of electromagnetic shielding honeycomb core materials, but the operation is complicated. Single-layer graphene / ferrite electromagnetic shielding honeycomb core materials or multi-layer graphene / ferrite electromagnetic shielding honeycomb core materials cannot meet the modern needs of ventilation and air permeability while shielding electromagnetic waves. Summary of the invention

[0013] The main purpose of the present invention is to provide a metallized aramid honeycomb material, a preparation method and application thereof, so as to solve the problem of complex preparation methods of electromagnetic shielding honeycomb core materials in the prior art.

[0014] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a metallized aramid honeycomb material is provided, the method comprising: step S1, cleaning the aramid honeycomb to obtain a clean aramid honeycomb; step S2, activating the clean aramid honeycomb to obtain an active aramid honeycomb; step S3, placing the active aramid honeycomb in a chemical iron-nickel plating solution for chemical plating to form an iron-nickel plating layer on the inner surface of the active aramid honeycomb.

[0015] Furthermore, the above step S1 includes sequentially performing alkali washing and water washing on the aramid honeycomb to obtain a clean aramid honeycomb.

[0016] Furthermore, the alkaline liquid used for the above-mentioned alkaline washing includes NaOH with a concentration of 10-30 g / L and OP emulsifier with a concentration of 1-3 g / L. Preferably, ultrasound is performed during the alkaline washing process. It is further preferred that the ultrasound power is 50-200 W and the ultrasound time is 5-30 min. Preferably, the alkaline washing is performed at 30-70°C.

[0017] Furthermore, the above step S2 includes: sequentially performing an infiltration treatment and a heat treatment on the clean aramid honeycomb in an activation solution to obtain an active aramid honeycomb, wherein the activation solution includes nickel acetate, a first reducing agent and water in a ratio of 1 g: 0.5-1.5 g: 20-40 mL, and preferably the first reducing agent is selected from any one or more of sodium hypophosphite, glucose, formaldehyde, acetaldehyde and sodium hypophosphite.

[0018] Furthermore, the time of the above-mentioned infiltration treatment is 5 to 10 minutes, and the temperature of the heat treatment is preferably 195 to 205° C. and the time of the heat treatment is 30 to 60 minutes.

[0019] Furthermore, before the infiltration treatment, step S2 also includes a process of surface corrosion of the clean aramid honeycomb. Preferably, the surface corrosion process includes: using a corrosive liquid to corrode the clean aramid fiber, the corrosive liquid includes hydrogen peroxide and sulfuric acid in a volume ratio of 1:2-4, preferably the corrosion treatment time is 3-10 minutes, and the mass concentration of sulfuric acid is preferably 90-99%.

[0020] Further, in the above step S3, the chemical iron-plating nickel solution includes a soluble nickel salt, a soluble ferrous salt and a second reducing agent, wherein the soluble nickel salt is selected from any one or more of nickel sulfate, nickel acetate and nickel hypophosphite, the soluble ferrous salt is selected from any one or more of ammonium ferrous sulfate hexahydrate and ferrous chloride tetrahydrate, and the second reducing agent is selected from any one or more of hypophosphite, sodium borohydride, borane and hydrazine; preferably, the concentration of the soluble nickel salt is 0.04-0.09 mol / L, the soluble The concentration of the ferrous salt is 0.01-0.06 mol / L, and the concentration of the second reducing agent is 0.005-0.01 mol / L; the pH value of the chemical iron-nickel plating solution is preferably 8.0-11.5, preferably, the temperature of the chemical plating is 90°C, and the time is 30-60 min, and the chemical iron-nickel plating solution also includes a catalyst, and the catalyst is selected from any one or more of malonic acid, succinic acid, aminoacetic acid, propionic acid, and sodium fluoride, and the concentration of the catalyst is 0.001-0.005 mol / L.

[0021] According to another aspect of the present invention, a metallized aramid honeycomb material is provided. The material is prepared by any one of the above-mentioned preparation methods.

[0022] According to another aspect of the present invention, a metallized aramid honeycomb material is provided, which comprises an aramid honeycomb substrate and an iron-nickel coating, wherein the iron-nickel coating is arranged on the inner surface and the outer surface of the aramid honeycomb substrate, and preferably the mass ratio of the aramid honeycomb substrate to the iron-nickel coating is 100-10:1, and the thickness of the iron-nickel coating is preferably 10-30 μm, and the iron-nickel coating contains phosphorus, and preferably the mass ratio of iron, nickel and phosphorus is 0.4-0.9:0.1-0.6:0.05-0.1.

[0023] According to yet another aspect of the present invention, there is provided an electromagnetic shielding structure, comprising an electromagnetic shielding honeycomb core material, wherein the electromagnetic shielding honeycomb core material is any one of the above-mentioned metallized aramid honeycomb materials.

[0024] By applying the technical solution of the present invention, firstly, cleaning is performed to remove small solid particles of impurities such as dust attached to the surface of the aramid honeycomb and stains such as mineral oil or grease adhering to the pore wall, and then activation treatment is performed to make it easier to deposit an iron-nickel coating on the surface of the aramid honeycomb. Finally, chemical plating is performed to form a uniform iron-nickel coating on the surface of the active aramid honeycomb, thereby realizing the metallization of the aramid paper honeycomb. From the above description, it can be seen that the preparation method of the metallized aramid honeycomb material of the present application is simple, and the metallization of the aramid paper honeycomb can be completed by cleaning, activation and chemical plating, thereby obtaining a metallized aramid paper honeycomb material with good corrosion resistance, good air permeability, high planar compression strength and excellent shielding performance. DETAILED DESCRIPTION

[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0026] As described in the background of this application, electromagnetic shielding honeycomb core materials can simultaneously meet the requirements of air permeability and electromagnetic wave shielding. However, some electromagnetic shielding honeycomb core materials in the prior art cannot meet the requirements of air permeability due to their structural design. In addition, the preparation methods of electromagnetic shielding honeycomb core materials in the prior art are too complicated. In order to solve the above problems, this application provides a metallized aramid honeycomb material, its preparation method and application.

[0027] In a typical embodiment of the present application, a method for preparing a metallized aramid honeycomb material is provided, and the preparation method comprises: step S1, cleaning the aramid honeycomb to obtain a clean aramid honeycomb; step S2, activating the clean aramid honeycomb to obtain an active aramid honeycomb; step S3, placing the active aramid honeycomb in a chemical iron-nickel plating solution for chemical plating to form an iron-nickel plating layer on the inner surface of the active aramid honeycomb.

[0028] The preparation method of the metallized aramid honeycomb material of the present application is firstly to clean to remove small solid particles of impurities such as dust attached to the surface of the aramid honeycomb and stains such as mineral oil or grease adhered to the pore wall, and then to activate to make it easier to deposit the iron-nickel coating on the surface of the aramid honeycomb. Finally, chemical plating is performed to form a uniform iron-nickel coating on the surface of the active aramid honeycomb, thereby realizing the metallization of the aramid paper honeycomb. From the above description, it can be seen that the preparation method of the metallized aramid honeycomb material of the present application is simple, and the metallization of the aramid paper honeycomb can be completed by cleaning, activation and chemical plating, so as to obtain a metallized aramid paper honeycomb material with good corrosion resistance, good air permeability, high planar compression strength and excellent shielding performance.

[0029] In the above cleaning step, the commonly used methods for removing small particles and grease in the prior art can be used. In order to achieve a better cleaning effect on the stains such as mineral oil or grease adhering to the aramid honeycomb cell wall, it is preferred that the above step S1 includes sequentially alkali washing and water washing of the aramid honeycomb to obtain a clean aramid honeycomb. After the alkali washing, water washing is performed to remove the residual alkali solution.

[0030] The above-mentioned alkali washing can use the alkali solution commonly used for alkali washing in the prior art. In order to achieve a better cleaning effect for aramid honeycombs, the alkaline solution used for the above-mentioned alkali washing preferably includes NaOH with a concentration of 10~30g / L and OP emulsifier of 1~3g / L. It is preferred to perform ultrasound during the alkali washing process, and it is further preferred that the ultrasonic power is 50~200W and the ultrasonic time is 5~30min. It is preferred that the alkali washing is performed at 30~70°C. The use of 10~30g / L sodium hydroxide solution and 1~3g / L OP emulsifier can enhance the effect of removing mineral oil or grease, wherein the emulsifier can also significantly reduce the surface tension of the grease, making it more dispersed in the water. Furthermore, the preferred ultrasonic treatment can further enhance the effect of removing small solid particle impurities such as dust from diffusing into the water.

[0031] The activation treatment method of the aramid honeycomb can be based on the commonly used activation methods of fibers in the prior art, such as the activation method using precious metal catalysis such as silver salt or palladium salt. In order to save costs and simplify the operation steps, in one embodiment, the above step S2 includes: sequentially performing an infiltration treatment and a heat treatment on the clean aramid honeycomb in an activation solution to obtain an activated aramid honeycomb, and the above activation solution includes nickel acetate, a first reducing agent and water in a ratio of 1g:0.5~1.5g:20~40mL. Through the treatment of the above activation solution, the nickel salt in the activator can be decomposed into elemental nickel to form a catalytic active center for chemical nickel plating on the surface of the aramid honeycomb, so that the subsequent chemical nickel plating can obtain a nickel-phosphorus coating that is firmly bonded to the aramid honeycomb and is smooth and uniform.

[0032] The first reducing agent in the activation solution of the present application can be selected from any one of the water-soluble reducing agents in the prior art. In order to uniformly activate the surface of the aramid honeycomb and improve the activation effect, the first reducing agent is preferably selected from any one or more of sodium hypophosphite, glucose, formaldehyde, acetaldehyde and sodium hypophosphite. The reducing agent is a small molecule compound that is easily adsorbed on the surface of the substrate and can remain stable in a room temperature aqueous solution. It can react with the aramid honeycomb more uniformly, so that the coating formed by subsequent chemical plating is dense and uniform, and thus has good corrosion resistance.

[0033] In order to improve both the activation effect and the activation efficiency, the time of the infiltration treatment is 5-10 minutes, and the preferred heat treatment temperature is 195-205°C and the heat treatment time is 30-60 minutes. When the treatment time is lower than the above preferred time range, the activation effect is not ideal; when the treatment time is longer than the preferred time, the treatment effect is not significantly improved.

[0034] Subsequent chemical plating is mainly to chemically plate a metal layer on the inner or outer surface of the aramid honeycomb. In order to improve the adhesion of the plated metal, in one embodiment, before the infiltration treatment, the above step S2 also includes a process of surface corrosion of the clean aramid honeycomb, also known as surface roughening. Preferably, the surface corrosion process includes: using a corrosive liquid to corrode the clean aramid fiber, the corrosive liquid includes hydrogen peroxide and sulfuric acid in a volume ratio of 1:2~4, preferably the corrosion treatment time is 3~10min, and the mass concentration of sulfuric acid is preferably 90~99%. The surface of the aramid fiber is roughened by surface corrosion treatment, which is conducive to the formation of multiple surface active points, so that the coating can be formed faster during subsequent chemical plating, and the adhesion of the coating is stronger. Within the above preferred parameter range, the occurrence of excessive or insufficient corrosion is minimized.

[0035] The method of chemical plating to form an iron-nickel metal layer can be referred to the chemical plating method of the metal layer in the prior art. In one embodiment, in the above step S3, the chemical iron-nickel plating solution includes a soluble nickel salt, a soluble ferrous salt and a second reducing agent, wherein the soluble nickel salt is selected from any one or more of nickel sulfate, nickel acetate and nickel hypophosphite, the soluble ferrous salt is selected from any one or more of ammonium ferrous sulfate hexahydrate and ferrous chloride tetrahydrate, and the second reducing agent is selected from any one or more of hypophosphite, sodium borohydride, borane and hydrazine. By using the above reagents, a dense and uniform iron-nickel plating layer can be formed on the surface of the aramid honeycomb, thereby preparing a metallized aramid paper honeycomb material with good corrosion resistance, high plane compression strength and excellent shielding performance. Furthermore, when nickel hypophosphite is selected as the source of nickel and hypophosphite, phosphorus and nickel will co-precipitate during the chemical plating process, so the chemically plated iron-nickel coating is an iron-nickel-phosphorus alloy coating in which phosphorus is dispersed. By controlling the phosphorus content between 1% and 15%, the obtained alloy coating is dense and non-porous, and its corrosion resistance is much better than that of electroplated nickel. In addition, the use of nickel hypophosphite avoids the introduction of sulfate ions and can minimize the accumulation of alkali metal ions, thereby avoiding the reaction of sulfate with metal ions to produce stable salts, resulting in impurities in the coating, which in turn affects the performance of the coating.

[0036] Those skilled in the art can adjust the thickness of the formed metal layer and the nickel-iron composition thereof according to the concentration of the soluble nickel salt and the concentration of the soluble ferrous salt used. In order to achieve more ideal corrosion resistance and electromagnetic shielding performance, the concentration of the soluble nickel salt is preferably 0.04-0.09 mol / L, the concentration of the soluble ferrous salt is 0.01-0.06 mol / L, and the concentration of the second reducing agent is 0.005-0.01 mol / L; the pH value of the chemical iron-nickel plating solution is preferably 8.0-11.5, and the temperature of the chemical plating is preferably 90°C and the time is 30-60 min. By optimizing the reagent concentration, reaction conditions, etc., the thickness, composition and other parameters of the coating can be well controlled, so that the prepared metallized aramid honeycomb material has better mechanical properties and application performance.

[0037] In one embodiment, the chemical iron-nickel plating solution preferably further comprises a catalyst, the catalyst being selected from any one or more of malonic acid, succinic acid, aminoacetic acid, propionic acid, and sodium fluoride, and the concentration of the catalyst being 0.001 to 0.005 mol / L. The selection of the catalyst can accelerate the reaction speed of chemical plating. The concentration of the catalyst is controlled to achieve a better catalytic effect without wasting reagents.

[0038] In another typical embodiment of the present application, a metallized aramid honeycomb material is provided. The metallized aramid honeycomb material is prepared by any of the above-mentioned preparation methods.

[0039] The metallized aramid honeycomb material prepared by the preparation method of the present application can controllably form a dense and uniform metal coating on the surface of the aramid honeycomb, thereby obtaining a metallized aramid paper honeycomb material with good corrosion resistance, good air permeability, high planar compression strength, and excellent shielding performance.

[0040] In another typical embodiment of the present application, a metallized aramid honeycomb material is provided, which includes an aramid honeycomb substrate and an iron-nickel coating, wherein the iron-nickel coating is disposed on the inner and outer surfaces of the aramid honeycomb substrate, and preferably the mass ratio of the aramid honeycomb substrate to the iron-nickel coating is 100-10:1, and the thickness of the iron-nickel coating is preferably 10-30 μm, and the iron-nickel coating preferably contains phosphorus, and preferably the mass ratio of iron, nickel and phosphorus is 0.4-0.9:0.1-0.6:0.05-0.1. A metallized aramid honeycomb material having the above structure. The shielding effect of eddy current is utilized, that is, when a high-frequency electromagnetic wave is incident, the Joule heat generated by the eddy current consumes the energy of the incident electromagnetic field by utilizing the certain resistance of the metal material, thereby achieving a shielding effect. In addition, it also has the characteristics of good corrosion resistance, good air permeability, high planar compression strength and excellent shielding performance.

[0041] In another typical embodiment of the present application, an electromagnetic shielding structure is provided, including an electromagnetic shielding honeycomb core material, wherein the electromagnetic shielding honeycomb core material is any of the above-mentioned metallized aramid honeycomb materials. The electromagnetic shielding structure using the metallized aramid honeycomb material of the present application as the electromagnetic shielding honeycomb core material has the characteristics of strong structural stability, good air permeability and excellent shielding effect.

[0042] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0043] Embodiment 1:

[0044] (1) Cleaning

[0045] Aramid paper honeycomb (300mm*300mm*5mm) was placed in alkaline solution and treated at 50°C and 120W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 20g / L NaOH and 2g / L OP emulsifier.

[0046] (2) Microetching

[0047] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0048] (3) Activation

[0049] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 60 minutes, and then washed with deionized water to remove the residual activation solution.

[0050] (4) Chemical iron-nickel plating

[0051] The activated aramid paper honeycomb was chemically plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the chemical iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.04 mol / L ammonium ferrous sulfate hexahydrate, 0.005 mol / L sodium borohydride, 0.005 mol / L sodium fluoride, pH 9.0, temperature 90°C, and treatment time 60 min.

[0052] Embodiment 2:

[0053] (1) Cleaning

[0054] Aramid paper honeycomb (300mm*300mm*15mm) was placed in alkaline solution and treated at 50°C and 150W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 30g / L NaOH and 2g / L OP emulsifier.

[0055] (2) Microetching

[0056] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0057] (3) Activation

[0058] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 50 minutes, and then washed with deionized water to remove the residual activation solution.

[0059] (4) Chemical iron-nickel plating

[0060] The activated aramid paper honeycomb was electrolessly plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the electroless iron and nickel plating solution were as follows: 0.05 mol / L nickel hypophosphite, 0.05 mol / L ammonium ferrous sulfate hexahydrate, 0.008 mol / L sodium borohydride, pH 9.5, temperature 90°C, and treatment time 60 min.

[0061] Embodiment 3:

[0062] (1) Cleaning

[0063] Aramid paper honeycomb (300mm*300mm*20mm) was placed in alkaline solution and treated at 50°C and 160W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 10g / L NaOH and 1g / L OP emulsifier.

[0064] (2) Microetching

[0065] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0066] (3) Activation

[0067] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 60 minutes, and then washed with deionized water to remove the residual activation solution.

[0068] (4) Chemical iron-nickel plating

[0069] The activated aramid paper honeycomb was electrolessly plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the electroless iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.04 mol / L ammonium ferrous sulfate hexahydrate, 0.005 mol / L sodium borohydride, pH 9.0, temperature 90°C, and 60 min.

[0070] Embodiment 4:

[0071] (1) Cleaning

[0072] Aramid paper honeycomb (300mm*300mm*25mm) was placed in an alkaline solution and treated at 50°C and an ultrasonic power of 170W for 10 minutes to remove impurities on the surface of the honeycomb pores. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 20g / L NaOH and 1g / L OP emulsifier.

[0073] (2) Microetching

[0074] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0075] (3) Activation

[0076] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 40 minutes, and then washed with deionized water to remove the residual activation solution.

[0077] (4) Chemical iron-nickel plating

[0078] The activated aramid paper honeycomb was electrolessly plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the electroless iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.06 mol / L ammonium ferrous sulfate hexahydrate, 0.01 mol / L sodium borohydride, 0.005 mol / L sodium fluoride, pH 10.0, temperature 90°C, and 60 min.

[0079] Embodiment 5:

[0080] (1) Cleaning

[0081] Aramid paper honeycomb (300mm*300mm*30mm) was placed in alkaline solution and treated at 50°C and 160W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 10g / L NaOH and 1g / L OP emulsifier.

[0082] (2) Microetching

[0083] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0084] (3) Activation

[0085] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 60 minutes, and then washed with deionized water to remove the residual activation solution.

[0086] (4) Chemical iron-nickel plating

[0087] The activated aramid paper honeycomb was electrolessly plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the electroless iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.04 mol / L ammonium ferrous sulfate hexahydrate, 0.005 mol / L sodium borohydride, pH 11.5, temperature 90°C, and 60 min.

[0088] Embodiment 6:

[0089] (1) Cleaning

[0090] Aramid paper honeycomb (300mm*300mm*40mm) was placed in alkaline liquid and treated at 50°C and 200W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline liquid. The alkaline liquid contained: 30g / L NaOH and 2g / L OP emulsifier.

[0091] (2) Microetching

[0092] Micro-etching is prepared by using hydrogen peroxide and 98.3% sulfuric acid in a volume ratio of 1:4. Put the washed aramid paper honeycomb into the micro-etching solution for about 5 minutes, then take it out, wash it with water, rinse the surface with deionized water, rinse the surface with deionized water again, and then dry it (105°C, 1.5h).

[0093] (3) Activation

[0094] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 60 minutes, and then washed with deionized water to remove the residual activation solution.

[0095] (4) Chemical iron-nickel plating

[0096] The activated aramid paper honeycomb was electrolessly plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the electroless iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.06 mol / L ammonium ferrous sulfate hexahydrate, 0.01 mol / L sodium borohydride, pH 11.0, temperature 90°C, and 60 min.

[0097] Example 7

[0098] The difference from Example 1 is that the concentration of the OP emulsifier in the cleaning step is 3 g / L.

[0099] Example 8

[0100] The difference from Example 1 is that the ultrasonic power in the cleaning step is 50W.

[0101] Example 9

[0102] The difference from Example 1 is that the ultrasonic time in the cleaning step is 5 minutes.

[0103] Example 10

[0104] The difference from Example 1 is that the ultrasonic time in the cleaning step is 30 minutes.

[0105] Embodiment 11

[0106] The difference from Example 1 is that the alkaline washing temperature in the cleaning step is 30°C.

[0107] Example 12

[0108] The difference from Example 1 is that the alkaline washing temperature in the cleaning step is 70°C.

[0109] Embodiment 13

[0110] The difference from Example 1 is that the volume ratio of hydrogen peroxide to sulfuric acid in the micro-etching step is 1:2.

[0111] Embodiment 14

[0112] The difference from Example 1 is that the micro-etching time in the micro-etching step is 3 minutes.

[0113] Embodiment 15

[0114] The difference from Example 1 is that the micro-etching time in the micro-etching step is 10 minutes.

[0115] Example 16

[0116] The difference from Example 1 is that in the activation step, an activation solution with a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:0.5:30 is used.

[0117] Embodiment 17

[0118] The difference from Example 1 is that in the activation step, an activation solution with a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1.5:30 is used.

[0119] Embodiment 18

[0120] The difference from Example 1 is that an equal weight of glucose is used to replace sodium hypophosphite in the activation step.

[0121] Embodiment 19

[0122] The difference from Example 1 is that an equal weight of acetaldehyde is used to replace sodium hypophosphite in the activation step.

[0123] Embodiment 20

[0124] The difference from Example 1 is that the activation treatment is carried out for 5 minutes.

[0125] Embodiment 21

[0126] The difference from Example 1 is that the heat treatment temperature during the activation treatment is 205°C.

[0127] Embodiment 22

[0128] The difference from Example 1 is that the heat treatment temperature during the activation treatment is 195°C.

[0129] Embodiment 23

[0130] The difference from Example 1 is that the heat treatment time during the activation treatment is 30 minutes.

[0131] Embodiment 24

[0132] The difference from Example 1 is that nickel sulfate of equal concentration is used instead of nickel hypophosphite in the chemical iron-nickel plating step.

[0133] Embodiment 25

[0134] The difference from Example 1 is that in the chemical iron-nickel plating step, nickel acetate of equal concentration is used instead of nickel hypophosphite.

[0135] Embodiment 26

[0136] The difference from Example 1 is that the concentration of nickel hypophosphite in the chemical iron-nickel plating step is 0.04 mol / L.

[0137] Embodiment 27

[0138] The difference from Example 1 is that the concentration of nickel hypophosphite in the chemical iron-nickel plating step is 0.09 mol / L.

[0139] Embodiment 28

[0140] The difference from Example 1 is that in the chemical iron-nickel plating step, borane of equal concentration is used instead of sodium borohydride.

[0141] Embodiment 29

[0142] The difference from Example 1 is that in the chemical iron-nickel plating step, hypophosphite of equal concentration is used instead of sodium borohydride.

[0143] Embodiment 30

[0144] The difference from Example 1 is that the concentration of ammonium ferrous sulfate hexahydrate in the chemical iron-nickel plating step is 0.01 mol / L.

[0145] Embodiment 31

[0146] The difference from Example 1 is that the chemical plating treatment time is 30 minutes.

[0147] Embodiment 32

[0148] The difference from Example 1 is that the concentration of sodium fluoride in the chemical iron-nickel plating step is 0.001 mol / L.

[0149] Embodiment 33

[0150] The difference from Example 1 is that in the chemical iron-nickel plating step, an equal concentration of boroaminoacetic acid is used instead of sodium fluoride.

[0151] Embodiment 34

[0152] The difference from Example 1 is that in the chemical iron-nickel plating step, malonic acid of equal concentration is used instead of sodium fluoride.

[0153] Embodiment 35

[0154] (1) Cleaning

[0155] Aramid paper honeycomb (300mm*300mm*5mm) was placed in alkaline solution and treated at 50°C and 120W ultrasonic power for 10 minutes to remove impurities on the surface of the honeycomb pore wall. The surface of the material was then rinsed with clean water to remove the residual alkaline solution, which contained 20g / L NaOH and 2g / L OP emulsifier.

[0156] (2) Activation

[0157] The micro-etched aramid paper honeycomb was infiltrated with an activation solution having a concentration of nickel acetate (g): sodium hypophosphite (g): water (ml) = 1:1:30 for about 10 minutes, then heat treated at 200°C for 60 minutes, and then washed with deionized water to remove the residual activation solution.

[0158] (3) Chemical iron-nickel plating

[0159] The activated aramid paper honeycomb was chemically plated with iron and nickel in an alkaline solution at 90°C, wherein the composition and process conditions of the chemical iron and nickel plating solution were as follows: 0.06 mol / L nickel hypophosphite, 0.04 mol / L ammonium ferrous sulfate hexahydrate, 0.005 mol / L sodium borohydride, 0.005 mol / L sodium fluoride, pH 9.0, temperature 90°C, and treatment time 60 min.

[0160] Embodiment 36

[0161] The difference from Example 1 is that in the activation step, the heat treatment temperature is 220°C.

[0162] Embodiment 37

[0163] The difference from Example 1 is that in the activation step, the heat treatment temperature is 180°C.

[0164] Embodiment 38

[0165] The difference from Example 1 is that in the activation step, the heat treatment time is 15 minutes.

[0166] Embodiment 39

[0167] The difference from Example 1 is that in the activation step, the heat treatment time is 75 minutes.

[0168] Embodiment 40

[0169] The difference from Example 1 is that in the chemical iron-nickel plating step, the concentration of nickel hypophosphite is 0.02 mol / L.

[0170] Embodiment 41

[0171] The difference from Example 1 is that in the chemical iron-nickel plating step, the concentration of nickel hypophosphite is 0.13 mol / L.

[0172] Embodiment 42

[0173] The difference from Example 1 is that in the chemical iron-nickel plating step, the concentration of ammonium ferrous sulfate hexahydrate is 0.09 mol / L.

[0174] The performance of the metallized aramid honeycomb material prepared in the above embodiment was tested.

[0175] (1) Corrosion resistance test:

[0176] Specific test content: observe the distribution of the metal layer on the honeycomb hole wall, and then conduct corrosion resistance test through salt spray test. And observe whether it is easy to fall off, whether the corrosion products of the material are loose, etc. For example, when evaluating the corrosion resistance of different materials through salt spray test, the weight loss method is usually used.

[0177] The gravimetric method is the most basic and most effective quantitative evaluation method in the study of material corrosion resistance. Although the gravimetric method has the disadvantage of being unable to study the corrosion mechanism of materials, by measuring the change in the weight of the material before and after corrosion, the corrosion resistance of the material can be characterized more accurately and reliably. Because of this, it has been widely used in corrosion research and is the basis for the comparison of many modern electrochemical, physical and chemical analysis and evaluation methods. The weight loss method can usually be considered.

[0178] The corrosion resistance of the material is characterized by the salt spray test combined with the weight loss test. According to the requirements of ASTMB117, the sample is placed at an angle of 15-30 degrees, and a 5% NaCl solution is used for atomization spraying, and the test temperature is 35°C. The salt spray test requires that the volume of the salt spray chamber must be large enough, and the salt spray must not be sprayed directly onto the test surface.

[0179] (2) Compression strength test

[0180] Take GB / T 1453-2005 test method as an example:

[0181] A. Sample preparation: Cut the sample honeycombs into sizes between 60mm*60mm*5mm and 60mm*60mm*40mm.

[0182] B. Testing equipment: universal material testing machine.

[0183] C. Compression fixture: A fixed flat platen and a platen with a spherical seat (automatic centering) should be used to introduce force into the specimen. The platen can be well centered and no eccentric load is applied. The platen surface should exceed the specimen shape. If the platen hardness is insufficient or in order to protect the platen surface, a harder flat plate (parallel to the surface) can be inserted between the fixture and each end face of the corresponding platen.

[0184] Test method: When testing the flat compression strength, adjust the spherical support so that the upper pad is parallel to the lower pressure plate of the testing machine, then load evenly and continuously until failure, read the failure load, and record the failure form. The recommended loading speed is 0.5mm / min.

[0185] E. Failure Mode: Uniform failure of the sample honeycomb is the only acceptable failure mode. Compression failure limited to one corner or one edge is invalid.

[0186] F. Data processing: keep 3 decimal places, ultimate strength, P = F / A. Where P is the unflattened compressive strength, MPa; F is the ultimate load before failure, N; A is the cross-sectional area of ​​the specimen, mm 2 .

[0187] (3) Shielding efficiency test

[0188] According to GJB6190-2008, the shielding effectiveness of shielding materials is tested in the electromagnetic compatibility test shielding room within the range of 10MHz~10GHz. Test. Since the amplitude value (unit: dB) displayed by the spectrum analyzer, the shielding room can directly measure the receiving field strength with and without shielding materials, and the shielding effectiveness of the shielding material can be obtained by subtracting the two.

[0189] The above test results are recorded in Table 1.

[0190] Table 1

[0191]

[0192] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0193] The preparation method of the metallized aramid honeycomb material of the present application is firstly to clean to remove small solid particles of impurities such as dust attached to the surface of the aramid honeycomb and stains such as mineral oil or grease adhered to the pore wall, and then to activate to make it easier to deposit the iron-nickel coating on the surface of the aramid honeycomb. Finally, chemical plating is performed to form a uniform iron-nickel coating on the surface of the active aramid honeycomb, thereby realizing the metallization of the aramid paper honeycomb. From the above description, it can be seen that the preparation method of the metallized aramid honeycomb material of the present application is simple, and the metallization of the aramid paper honeycomb can be completed by cleaning, activation and chemical plating, so as to obtain a metallized aramid paper honeycomb material with good corrosion resistance, good air permeability, high planar compression strength and excellent shielding performance.

[0194] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a metallized aramid honeycomb material, characterized in that: The preparation method comprises: Step S1, cleaning the aramid honeycomb to obtain a cleaned aramid honeycomb; Step S2, activating the clean aramid honeycomb to obtain an activated aramid honeycomb; Step S3, placing the active aramid honeycomb in a chemical iron-nickel plating solution for chemical plating to form an iron-nickel plating layer on the inner surface of the active aramid honeycomb; In step S3, the chemical iron-plating nickel solution includes a soluble nickel salt, a soluble ferrous salt and a second reducing agent, wherein the soluble nickel salt is selected from any one or more of nickel sulfate, nickel acetate and nickel hypophosphite, the soluble ferrous salt is selected from any one or more of ammonium ferrous sulfate hexahydrate and ferrous chloride tetrahydrate, and the second reducing agent is selected from any one or more of hypophosphite, sodium borohydride, borane and hydrazine.

2. The preparation method according to claim 1, characterized in that: The step S1 includes sequentially performing alkali washing and water washing on the aramid honeycomb to obtain the clean aramid honeycomb.

3. The preparation method according to claim 2, characterized in that: The alkaline solution used for the alkaline washing includes NaOH with a concentration of 10-30 g / L and OP emulsifier with a concentration of 1-3 g / L.

4. The preparation method according to claim 3, characterized in that: Ultrasound is performed during the alkaline washing process.

5. The preparation method according to claim 4, characterized in that: The ultrasonic power is 50-200W, and the ultrasonic time is 5-30min.

6. The preparation method according to claim 3, characterized in that: The alkali washing is carried out at 30-70°C.

7. The preparation method according to claim 1, characterized in that: The step S2 comprises: sequentially performing an infiltration treatment and a heat treatment on the clean aramid honeycomb in an activation solution to obtain the activated aramid honeycomb, wherein the activation solution comprises nickel acetate, a first reducing agent and water in a ratio of 1 g: 0.5-1.5 g: 20-40 mL.

8. The preparation method according to claim 7, characterized in that: The first reducing agent is selected from any one or more of sodium hypophosphite, glucose, formaldehyde, acetaldehyde and sodium hypophosphite.

9. The preparation method according to claim 7, characterized in that: The time of the infiltration treatment is 5 to 10 minutes.

10. The preparation method according to claim 9, characterized in that: The heat treatment temperature is 195-205° C. and the heat treatment time is 30-60 min.

11. The preparation method according to claim 7, characterized in that: Before the infiltration treatment is performed, the step S2 further includes a process of performing surface corrosion on the clean aramid honeycomb.

12. The preparation method according to claim 11, characterized in that: The surface corrosion process includes: using a corrosion liquid to corrode the clean aramid fiber, and the corrosion liquid includes hydrogen peroxide and sulfuric acid in a volume ratio of 1:2-4.

13. The preparation method according to claim 12, characterized in that: The corrosion treatment time is 3 to 10 minutes.

14. The preparation method according to claim 12, characterized in that: The mass concentration of the sulfuric acid is 90-99%.

15. The preparation method according to claim 1, characterized in that: In step S3, the concentration of the soluble nickel salt is 0.04-0.09 mol / L, the concentration of the soluble ferrous salt is 0.01-0.06 mol / L, and the concentration of the second reducing agent is 0.005-0.01 mol / L.

16. The preparation method according to claim 15, characterized in that: The pH value of the chemical iron-nickel plating solution is 8.0-11.

5.

17. The preparation method according to claim 15, characterized in that: The temperature of the chemical plating is 90° C. and the time is 30 to 60 minutes.

18. The preparation method according to claim 15, characterized in that: The chemical iron-nickel plating solution also includes a catalyst, which is selected from any one or more of malonic acid, succinic acid, aminoacetic acid, propionic acid, and sodium fluoride, and the concentration of the catalyst is 0.001-0.005 mol / L.

19. A metallized aramid honeycomb material, characterized in that: The method is prepared according to any one of claims 1 to 18.

20. The metallized aramid honeycomb material according to claim 19, characterized in that: The metallized aramid honeycomb material comprises an aramid honeycomb matrix and an iron-nickel coating, wherein the iron-nickel coating is arranged on the inner surface and the outer surface of the aramid honeycomb matrix.

21. The metallized aramid honeycomb material according to claim 20, characterized in that: The mass ratio of the aramid honeycomb substrate to the iron-nickel coating is 100-10:

1.

22. The metallized aramid honeycomb material according to claim 20, characterized in that: The thickness of the iron-nickel plating layer is 10-30 μm.

23. The metallized aramid honeycomb material according to claim 20, characterized in that: The iron-nickel plating layer contains phosphorus.

24. The metallized aramid honeycomb material according to claim 23, characterized in that: The mass ratio of iron, nickel and phosphorus is 0.4~0.9:0.1~0.6:0.05~0.

1.

25. An electromagnetic shielding structure, comprising an electromagnetic shielding honeycomb core material, characterized in that: The electromagnetic shielding honeycomb core material is the metallized aramid honeycomb material according to any one of claims 19 to 24.

Citation Information

Patent Citations

  • An electromagnetic shielding honeycomb core material, its preparation method and implantation tooling

    CN106982546B

  • Preparation method of electromagnetic shielding honeycomb core material

    CN108724822A

  • Lightweight square cabinet wall plate with wide frequency shielding function, and preparation method thereof

    CN108274830A

  • Method for preparing surface metallization aramid fibers

    CN109554916A