Micron SiC hollow tube and preparation method and application thereof
By removing the two-dimensional carbon material template during vapor deposition and heat treatment, and preparing micron SiC hollow tubes, the problems of small specific surface area and limited catalytic performance of SiC support are solved, and higher catalytic activity and adsorption separation performance are achieved.
Patent Information
- Application Number
- CN202411034018.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing SiC support has a low specific surface area and limited supported catalyst amount, resulting in fewer active sites and limited catalytic performance of composite materials.
By arranging the two-dimensional carbon materials at intervals in the vapor deposition equipment, a silicon carbon precursor is passed into the vapor deposition, and then heat treatment is performed in an air atmosphere to remove the two-dimensional carbon material template to form a micron SiC hollow tube to increase the specific surface area of the material and catalytic activity.
The micron SiC hollow tube prepared by this method has a larger specific surface area, provides more active sites, improves catalytic efficiency and adsorption separation performance, is simple to operate, reasonable design, and meets application needs in different fields.
Smart Images

Figure CN118957746A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micron material development and relates to a micron SiC hollow tube and a preparation method and application thereof. Background Art
[0002] Silicon carbide (SiC) has stable chemical properties, small thermal expansion coefficient, high hardness, excellent thermal conductivity, and excellent antioxidant properties in high-temperature oxygen environments. Its application fields are very wide, mainly including: power electronics, refractory materials, new energy, semiconductor devices, etc. SiC not only has two crystal forms: α-SiC (hexagonal system) and β-SiC (cubic system), but also has a variety of multi-level structures, such as: SiC whiskers, SiC nanowires, nanobelts, hollow SiC microspheres, etc. The unique performance characteristics of SiC have made it a catalyst carrier that has received a lot of attention in recent years. SiC can cope with harsh preparation processes and reaction conditions, and the structure and morphology of SiC can be customized by controlling the synthesis path, and it has a generally adjustable surface area, making it an ideal choice for carriers in many catalytic conversions. In addition, the catalyst loaded with precious metals on SiC has strong stability and can show good catalytic effects under high temperature, high pressure and complex atmosphere; it has strong antioxidant properties and can resist the erosion of oxidants, and the catalyst has a long service life; the loading process is simple to operate, energy-saving and environmentally friendly;
[0003] However, most of the current SiC is in the form of solid rods, needles and bamboo nodes, with a low specific surface area and a limited amount of loaded catalyst, resulting in fewer active sites in the composite material and limited catalytic performance. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a micron SiC hollow tube and a preparation method and application thereof, thereby solving the technical problems in the prior art that the SiC carrier has a low specific surface area and a limited amount of loaded catalyst, resulting in fewer active sites in the composite material and limited catalytic performance.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a micron SiC hollow tube comprises the following steps:
[0007] S1: The two-dimensional carbon material is arranged at intervals and fixed in a vapor deposition device, and a silicon-carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC;
[0008] S2: In an air atmosphere, heat-treating the two-dimensional carbon material loaded with SiC to obtain the micron SiC hollow tube.
[0009] Preferably, the silicon-carbon precursor is a mixed gas of SiCl4, CH4 and H2 or CH3Cl3Si and H2.
[0010] Preferably, the spacing distance between the two-dimensional carbon materials is 5 to 10 mm.
[0011] Preferably, the two-dimensional carbon material is carbon nanotube fiber or carbon fiber.
[0012] Preferably, during the vapor deposition process, the deposition temperature is 1050-1300° C. and the deposition time is 2-4 hours.
[0013] Preferably, the heat treatment temperature is 400-500°C.
[0014] Preferably, the heat treatment time is 2 to 4 hours.
[0015] A micron SiC hollow tube is prepared by the above method.
[0016] Preferably, the hollow inner diameter is 20 to 25 μm.
[0017] The above-mentioned micron SiC hollow tube is used as a catalyst carrier.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The present invention discloses a method for preparing a micron SiC hollow tube. The method prepares a micron SiC hollow tube through two main steps. First, a two-dimensional carbon material is arranged at intervals and fixed in a vapor deposition device, and then a silicon-carbon precursor is introduced for vapor deposition. At high temperature, the silicon-carbon precursor is cracked and reacts with the two-dimensional carbon material to form a two-dimensional carbon material loaded with SiC. Then the two-dimensional carbon material loaded with SiC is placed in an air atmosphere for heat treatment. During this process, the two-dimensional carbon material is oxidized and removed as a template, while SiC is retained to form a micron SiC tube with a hollow structure. The hollow tubular structure has a larger specific surface area than the solid material, which means that more active sites can be exposed on the surface of the material, thereby improving its catalytic activity. In the fields of catalysis, adsorption, separation, etc., this structural advantage is particularly obvious. At present, there are few methods for preparing SiC micron hollow tubes. The present invention provides a novel and feasible approach. Through the two-step method of vapor deposition and heat treatment, the morphology and structure of the SiC hollow tube can be accurately controlled to meet the application needs of different fields. Micron-sized SiC hollow tubes can provide more active sites and improve catalytic efficiency. Their large specific surface area is conducive to the adsorption and separation of target substances in gas or liquid. Therefore, the method of the present invention is simple to operate and reasonably designed, and micron-sized SiC hollow tubes can be effectively obtained.
[0020] Further, the silicon-carbon precursor is a mixed gas of SiCl4, CH4 and H2 or CH3Cl3Si, wherein SiCl4 (silicon tetrachloride), H2 and CH4 (methane) can react chemically at high temperature to generate SiC (silicon carbide) during the vapor deposition process. This reaction provides a direct way to prepare SiC, and due to the uniformity of vapor deposition, it helps to form a uniform SiC layer. CH3Cl3Si (methyltrichlorosilane) has a 1:1 carbon-silicon stoichiometric ratio, can be cracked at high temperature and reacted with the participation of hydrogen to form SiC, and the Si-Cl bond and Si-CH3 bond in its molecular structure are easy to break and reorganize at high temperature, which is conducive to the formation of SiC. Using a mixed gas of SiCl4 and CH4 or CH3Cl3Si as a silicon-carbon precursor, the growth rate, morphology and purity of SiC can be controlled by adjusting parameters such as the ratio of the gas, flow rate, and deposition temperature. This controllability makes the preparation process more accurate and reliable. Using a mixed gas of SiCl4 and CH4 or CH3Cl3Si as a precursor may have lower costs and higher yields compared to other methods.
[0021] Furthermore, the spacing distance between the two-dimensional carbon materials is 5 to 10 mm. During the vapor deposition process, the silicon-carbon precursor gas needs to be fully diffused to the surface of the two-dimensional carbon material for reaction. The appropriate spacing distance (5 to 10 mm) can ensure that the gas can flow freely between the materials and reduce the uneven reaction caused by limited gas diffusion. The wider spacing distance helps the gas to quickly reach and cover the surface of the two-dimensional carbon material, improve the reaction efficiency and the deposition rate of SiC, and at the same time, it also helps to reduce the reaction difference caused by the gas concentration gradient. In the subsequent heat treatment process, the two-dimensional carbon material is oxidized and removed as a template, while SiC is retained to form a hollow tube. The appropriate spacing distance helps to maintain the stability of the material during the heat treatment process and avoid deformation or rupture of the hollow tube caused by mutual extrusion between materials. The setting of the spacing distance can also affect the morphology and size of the SiC hollow tube. By adjusting the spacing distance and the deposition process, precise control of parameters such as the diameter and wall thickness of the hollow tube can be achieved to meet the application requirements of different fields. Although the spacing distance itself does not directly affect the specific surface area of the SiC hollow tube, the appropriate spacing distance helps to maintain the integrity of the material during the preparation process, thereby ensuring the specific surface area and number of active sites of the final product, which is of great significance for improving the catalytic activity and adsorption performance of the material. A wider spacing distance can reduce the mutual interference and agglomeration of two-dimensional carbon materials during heat treatment, which helps to improve the structural stability and thermal stability of the SiC hollow tube. The spacing distance of 5 to 10 mm makes it easy to arrange and fix the two-dimensional carbon material in the vapor deposition equipment, reducing the complexity and difficulty of the preparation process.
[0022] Further, the two-dimensional carbon material is carbon nanotube fiber or carbon fiber, and both carbon nanotube fiber and carbon fiber have the characteristics of high strength and high toughness, which enables them to withstand high temperature and stress during vapor deposition and heat treatment when used as a supporting template, and ensure the integrity of the SiC hollow tube structure. In particular, carbon nanotube fiber, its super strong mechanical properties make it possible to significantly improve the strength of the prepared SiC hollow tube. Both carbon nanotube fiber and carbon fiber have good thermal stability and can maintain structural stability under high temperature environment, which is crucial for subsequent heat treatment steps. Since carbon nanotube fiber and carbon fiber have a large specific surface area and uniform fiber structure, silicon-carbon precursor gas can be more easily uniformly deposited on its surface to form a uniform SiC layer. During the heat treatment process, carbon nanotube fiber and carbon fiber can be relatively easily removed as a template because the interface between them and SiC is relatively clear, which helps to reduce mechanical damage and chemical erosion during the removal process, thereby maintaining the integrity of the SiC hollow tube.
[0023] Furthermore, in the process of vapor deposition, the deposition temperature is 1050-1300°C and the deposition time is 2-4h. Within this temperature range, the silicon-carbon precursor gas can be fully cracked and react chemically with the two-dimensional carbon material to generate SiC. The higher temperature helps to accelerate the reaction rate and improve the deposition efficiency. High deposition temperature helps to improve the crystal integrity of SiC crystals, reduce crystal defects, and improve the mechanical properties, thermal stability and chemical stability of the material, which is crucial for the preparation of high-performance SiC hollow tubes and other materials. The deposition temperature has an important influence on the morphology and size of SiC. By adjusting the deposition temperature, the growth rate and deposition thickness of SiC can be controlled, thereby achieving precise control of the morphology and size of materials such as SiC hollow tubes. The length of the deposition time directly affects the degree of reaction between the silicon-carbon precursor gas and the two-dimensional carbon material. The deposition time of 2-4 hours can ensure that the reaction is fully carried out, so that SiC forms a uniform and dense coating on the surface of the two-dimensional carbon material. Appropriate deposition time can improve the deposition efficiency while ensuring the deposition quality. Too short deposition time may lead to incomplete reaction, while too long deposition time may increase cost and energy consumption. The deposition time is also closely related to the deposition thickness of SiC. By adjusting the deposition time, the deposition thickness of SiC can be controlled to meet the material thickness requirements of different application fields. By precisely controlling the deposition temperature and deposition time, the vapor deposition process can be optimized and the stability and repeatability of the preparation process can be improved, which is of great significance for realizing industrial production.
[0024] Furthermore, the heat treatment temperature is 400-500°C, which can effectively achieve the thermal decomposition of the two-dimensional carbon material used as a template inside SiC. In addition to the direct thermal decomposition of the two-dimensional carbon material, this temperature range can also promote the interface reaction between SiC and the two-dimensional carbon material. These reactions include the diffusion of carbon elements in SiC, the local phase change of SiC or the formation of new phases, which effectively improves the reaction activity of the micron SiC hollow tube.
[0025] Furthermore, the heat treatment time is 2 to 4 hours, which is sufficient to achieve thermal decomposition of the two-dimensional carbon material used as a template inside the SiC. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 It is a schematic diagram of a process for preparing a micron SiC hollow tube in the present invention;
[0028] Figure 2 This is a cross-sectional SEM photograph of the micron SiC hollow tube prepared in Example 1 of the present invention;
[0029] Figure 3 This is a surface SEM photograph of the micron SiC hollow tube prepared in Example 1 of the present invention;
[0030] Figure 4 Spectrum of the SEM photograph of the micron SiC hollow tube after heat treatment prepared in Example 2 of the present invention;
[0031] Figure 5 This is the XRD spectrum of the micron SiC hollow tube prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0033] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0034] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0037] like Figure 1 As shown, the present invention provides a method for preparing a micron SiC hollow tube, comprising the following steps:
[0038] S1: The two-dimensional carbon material is arranged at intervals and fixed in a vapor deposition device, and a silicon-carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC;
[0039] The silicon-carbon precursor is a mixed gas of SiCl4 and CH4 or CH3Cl3Si. In addition, hydrogen is introduced as a reaction gas and argon is introduced as a diluent gas during the vapor deposition.
[0040] In addition, the spacing between the two-dimensional carbon materials is 5 to 10 mm. The two-dimensional carbon material is carbon nanotube fiber or carbon fiber. During the vapor deposition process, the deposition temperature is 1050 to 1300° C. and the deposition time is 2 to 4 hours.
[0041] Here, for fixing the two-dimensional carbon material, an "I"-shaped mold can be used, and the two-dimensional carbon material is specifically wound on two parallel sides of the "I" shape, and the spacing between each two-dimensional carbon material is 5 to 10 mm. Then the mold is connected together and placed in a chemical vapor deposition furnace with a fixed graphite base for vapor deposition.
[0042] S2: In an air atmosphere, heat-treating the two-dimensional carbon material loaded with SiC to obtain the micron SiC hollow tube.
[0043] Here, heat treatment can effectively remove the template, the heat treatment temperature is 400-500°C, and the heat treatment time is 2-4h. In addition, the removal of the template in the present invention can also be achieved by a specific tensile machine, specifically: after the vapor deposition is completed, the "I"-shaped deposition mold with fibers is taken out, laid flat on the test bench, and one end is fixed, and the other end is clamped on a puller that can apply force evenly, and the pulling force is set to increase evenly from 0.5 to 5N until a single hollow SiC microtube is pulled out.
[0044] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0045] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0046] Example 1
[0047] A method for preparing a micron SiC hollow tube comprises the following steps:
[0048] S1: The two-dimensional carbon material is fixed in a vapor deposition device with a spacing of 5 mm, and a silicon carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC; wherein the silicon carbon precursor is a mixed gas of SiCl4 and CH4, and hydrogen is introduced as a reaction gas and argon is introduced as a diluent gas. The two-dimensional carbon material is a carbon nanotube fiber. During the vapor deposition process, the deposition temperature is 1050°C and the deposition time is 2 hours.
[0049] S2: In an air atmosphere, the two-dimensional carbon material loaded with SiC is heat treated at 400°C for 2 hours to obtain the micron SiC hollow tube, the inner diameter of which is 20 μm.
[0050] Figure 2 This is a cross-sectional SEM photograph of the micron SiC hollow tube prepared in Example 1 of the present invention. As can be seen from the figure, the inner diameter of the micron SiC hollow tube is 25 μm.
[0051] Figure 3This is a surface SEM photograph of the micron SiC hollow tube prepared in Example 1 of the present invention. It can be seen from the figure that the surface SiC is composed of many stacked pyramid-shaped particles.
[0052] Figure 4 This is a SEM photo spectrum of the micron SiC hollow tube after heat treatment prepared in Example 2 of the present invention. It can be seen from the figure that the inner diameter of the micron SiC hollow tube is 28 μm;
[0053] Figure 5 This is the XRD spectrum of the micron SiC hollow tube prepared in Example 1 of the present invention. It can be seen from the figure that the SiC hollow tube is composed of a single SiC phase and has good crystallinity.
[0054] Example 2
[0055] A method for preparing a micron SiC hollow tube comprises the following steps:
[0056] S1: The two-dimensional carbon material is fixed in a vapor deposition device with a spacing of 10 mm, and a silicon-carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC; wherein the silicon-carbon precursor is a mixed gas of SiCl4 and CH4, and hydrogen is introduced as a reaction gas and argon is introduced as a diluent gas. The two-dimensional carbon material is carbon fiber. During the vapor deposition process, the deposition temperature is 1300°C and the deposition time is 4 hours.
[0057] S2: In an air atmosphere, the two-dimensional carbon material loaded with SiC is heat treated at 500°C for 4 hours to obtain the micron SiC hollow tube, the inner diameter of which is 25 μm.
[0058] Example 3
[0059] A method for preparing a micron SiC hollow tube comprises the following steps:
[0060] S1: The two-dimensional carbon material is fixed in a vapor deposition device at an interval of 8 mm, and a silicon carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC; wherein the silicon carbon precursor is a mixed gas of SiCl4 and CH4, and hydrogen is introduced as a reaction gas and argon is introduced as a diluent gas. The two-dimensional carbon material is a carbon nanotube fiber. During the vapor deposition process, the deposition temperature is 1200°C and the deposition time is 3 hours.
[0061] S2: In an air atmosphere, the two-dimensional carbon material loaded with SiC is heat treated at 450°C for 3 hours to obtain the micron SiC hollow tube, the inner diameter of which is 22 μm.
[0062] Example 4
[0063] The carbon nanotube fibers were wound along an "I"-shaped graphite mold with an interval of 5 to 10 mm and evenly spread in two layers; the "I"-shaped mold was placed in a chemical vapor deposition furnace with a fixed graphite base; a SiCl4-CH4-H2-Ar deposition system was used, the deposition equipment was heated to 1050°C, a mixed precursor was introduced, and deposition was performed for 3 hours; after cooling, the "I"-shaped deposition mold with fibers was taken out, laid flat on the test bench, and one end was fixed, and the other end was clamped on a puller that can apply force evenly, with a pulling force of 5N. The structure showed that directly using 5N as a pulling force would cause the fiber to break, and a continuous micron SiC hollow tube could not be obtained.
[0064] Example 5
[0065] Wrap the carbon nanotube fibers along the "I"-shaped graphite mold with an interval of 5mm and spread them evenly in double layers; place the "I"-shaped mold in a chemical vapor deposition furnace with a fixed graphite base; use a CH3Cl3Si-H2-Ar deposition system, heat the deposition equipment to 1150°C, introduce a mixed precursor, and deposit for 2 hours; after cooling, take out the "I"-shaped deposition mold with fibers, lay it flat on the test bench, fix one end of it, and clamp the other end on a puller that can apply force evenly, and increase the pulling force evenly from 3N. When the pulling force reaches 3N, a continuous single micron SiC hollow tube has been completely pulled out.
[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a micron SiC hollow tube, It is characterized in that The following steps are involved: S1: The two-dimensional carbon material is arranged at intervals and fixed in a vapor deposition device, and a silicon-carbon precursor is introduced for vapor deposition to obtain a two-dimensional carbon material loaded with SiC; S2: In an air atmosphere, heat-treating the two-dimensional carbon material loaded with SiC to obtain the micron SiC hollow tube.
2. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that The silicon carbon precursor is SiCl 4 , CH 4 With H 2 A mixed gas or CH 3 Cl 3 Si and H 2 .
3. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that The spacing distance between the two-dimensional carbon materials is 5 to 10 mm.
4. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that The two-dimensional carbon material is carbon nanotube fiber or carbon fiber.
5. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that During the vapor deposition process, the deposition temperature is 1050-1300° C. and the deposition time is 2-4 hours.
6. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that The heat treatment temperature is 400-500°C.
7. The method for preparing a micron SiC hollow tube according to claim 1, It is characterized in that The heat treatment time is 2 to 4 hours.
8. A micron SiC hollow tube, It is characterized in that It is prepared by the method according to any one of claims 1 to 7.
9. A micron SiC hollow tube according to claim 8, It is characterized in that The hollow inner diameter is 20-25 μm.
10. Use of the micron SiC hollow tube according to any one of claims 8 to 9 as a catalyst carrier.