High-strength outdoor tent fabric and preparation method thereof
Through the cross-linking reaction of gamma ray irradiation treatment and the closed isocyanate cross-linking agent, combined with modified basalt fibers, the mechanical properties of outdoor tent fabrics are improved, the problem of cracks in existing fabrics is solved, and the service life of the tent is extended.
Patent Information
- Application Number
- CN202210485349.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-05-06
AI Technical Summary
The mechanical properties of existing outdoor tent fabrics are poor, resulting in easy cracks during use and folding, affecting the service life of the tent.
The fiber is treated with gamma ray irradiation, and the crosslinking reaction between the blocked isocyanate crosslinking agent and epoxy resin is combined with modified basalt fibers and ammonium polyphosphate to enhance the bonding strength between the base cloth and the glue coating, and improve the mechanics of the fabric. performance.
It significantly improves the mechanical properties of the fabric, including tensile strength, peel strength and fold resistance, extending the service life of the tent.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of outdoor tents, and in particular to a high-strength outdoor tent fabric and a preparation method thereof. Background Art
[0002] When going camping outdoors, a tent is a must-have equipment. The tent must have multiple outdoor functions such as sunshade, ventilation, windproof, rainproof, and warmth. Outdoor tents must adapt to various weather environments, so there are higher requirements for the tents produced by the company. The existing tents need to add multiple coatings on the base fabric of the tent to enhance the function of the tent itself, so that the produced tents are more practical and can have effective sunshade, ventilation, windproof, rainproof, and warmth functions.
[0003] In the prior art, generally, the thermal insulation effect of the fabric is improved by increasing the thickness and number of layers of the coating. Increasing the thickness of the coating will increase the weight and rigidity of the coating, thereby affecting the mechanical properties of the fabric. Cracks are easily generated after bending, and tents usually need to be folded and placed after each use, which seriously affects the service life of the tent. Summary of the invention
[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a high-strength outdoor tent fabric and a preparation method thereof, so as to solve the technical problem that the existing tent fabric has poor mechanical properties.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A method for preparing a high-strength outdoor tent fabric, the specific preparation steps are as follows:
[0007] (1) Pretreatment of base fabric: Place the polyester base fabric in an irradiation room and perform γ-ray irradiation treatment. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric;
[0008] (2) Preparation of coating: epoxy resin, blocked isocyanate crosslinking agent, tributyl phosphate and alumina powder are stirred and mixed evenly, and then modified basalt fiber, ammonium polyphosphate and decabromodiphenylethane are added thereto, stirred and mixed evenly, and then ultrasonically defoamed to obtain coating;
[0009] (3) Fabric preparation: The glue obtained in step (2) is evenly scraped onto the outer layer of the pretreated polyester base fabric, and then dried and cooled to obtain the outdoor tent fabric.
[0010] Preferably, in step (1), the irradiation dose is 20-40 kGy, and the irradiation dose rate is 1-5 kGy / h.
[0011] Preferably, in step (2), the mass ratio of the epoxy resin, blocked isocyanate crosslinking agent, tributyl phosphate, alumina powder, modified basalt fiber, ammonium polyphosphate and decabromodiphenylethane is 80-100:4-8:1-3:2-3:10-15:5-10:3-6.
[0012] Preferably, in step (2), the method for preparing the modified basalt fiber comprises the following steps:
[0013] (01) Grinding and crushing the basalt fiber, then immersing it in an alkali solution, washing and drying it, and then heat treating it at 300-400°C for 2-3h to obtain the pretreated basalt fiber;
[0014] (02) The pretreated basalt fiber is dispersed in a methanol solvent, and then a polyurethane resin and a silane coupling agent are added thereto. The mixture is heated, stirred and refluxed for reaction. After the reaction is completed, the reaction product is washed and dried to obtain the modified basalt fiber.
[0015] Preferably, in step (01), the alkali solution is a sodium hydroxide solution, and the concentration of the alkali solution is 1-2 mol / L.
[0016] Preferably, in step (02), the mass ratio of the pretreated basalt fiber, the polyurethane resin and the silane coupling agent is 10-20:8-12:4-8.
[0017] Preferably, in step (02), the silane coupling agent is selected from one or more of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0018] Preferably, in step (02), the reflux reaction temperature is 70-90° C., and the reflux reaction time is 2-3 h.
[0019] Preferably, in step (3), the drying temperature is 120-150° C., the drying time is 3-5 min, and the thickness of the glue after drying is 0.8-1.5 mm.
[0020] The present invention also provides high-strength outdoor tent fabric prepared by the above preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention uses high-energy gamma rays with strong penetrating power to stimulate the activity of the fiber surface, generating a large number of free radicals on the fiber surface. The blocked isocyanate crosslinking agent can coexist stably with the resin containing active groups for a long time at room temperature. After heat treatment, the isocyanate crosslinking agent releases -NCO groups and reacts with hydroxyl, carboxyl, amino and other groups on the resin molecular chain to form crosslinks, thereby improving the bonding strength between the base fabric and the coating, and further improving the mechanical properties of the fabric. In addition, under the action of high-energy rays, the epidermis and core layer of the fiber are crosslinked, and the main strength of the fiber is improved through crosslinking, further improving the mechanical properties of the fabric.
[0023] (2) The present invention first pre-treats the basalt fiber to improve the surface roughness of the basalt fiber, so that more hydroxyl groups are exposed on the surface, providing more active sites for grafting polyurethane. By grafting polyurethane onto the basalt fiber, on the one hand, it is beneficial for the basalt fiber to be evenly dispersed in the coating to avoid the problem of uneven dispersion. On the other hand, it improves the bonding strength between the basalt fiber and the base fabric, reduces the loss of tear strength of the coating layer, and improves the folding resistance of the fabric. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0025] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0026] The polyester base fabric used in this embodiment is an untreated and dyed white base fabric, and the product specification is 250D;
[0027] Epoxy resin was purchased from Zaoqiang County Yingtao Composite Materials Co., Ltd., model E44;
[0028] The blocked isocyanate crosslinker was purchased from Hefei Dibang Nanotechnology Co., Ltd., model JL-1001;
[0029] Polyurethane resin was purchased from Jiangsu Polys Biotechnology Co., Ltd., model number 9009-54-5.
[0030] Example 1
[0031] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0032] (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. The irradiation dose is 20 kGy and the irradiation dose rate is 2 kGy / h. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric.
[0033] (2) Preparation of coating: 80 g of epoxy resin, 5 g of blocked isocyanate crosslinking agent, 2 g of tributyl phosphate and 3 g of alumina powder were stirred and mixed uniformly, and then 10 g of modified basalt fiber, 5 g of ammonium polyphosphate and 4 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0034] The preparation method of modified basalt fiber comprises the following steps:
[0035] 10g of basalt fiber was ground and then immersed in 1mol / L sodium hydroxide solution, washed and dried, and then heat treated at 300℃ for 2h to obtain pretreated basalt fiber.
[0036] 10 g of pretreated basalt fiber was dispersed in 200 mL of methanol solvent, and then 8 g of polyurethane resin and 4 g of silane coupling agent KH560 were added thereto, and the mixture was heated, stirred and refluxed at 80° C. for 2 h. After the reaction was completed, the reaction product was washed and dried to obtain modified basalt fiber;
[0037] (3) Fabric preparation: The glue is evenly coated on the outer layer of the pretreated polyester base fabric and dried at 120°C for 4 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0038] Example 2
[0039] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0040] (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. The irradiation dose is 24 kGy and the irradiation dose rate is 3 kGy / h. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric.
[0041] (2) Preparation of coating: 85 g of epoxy resin, 6 g of blocked isocyanate crosslinking agent, 1 g of tributyl phosphate and 2 g of alumina powder were stirred and mixed uniformly, and then 12 g of modified basalt fiber, 8 g of ammonium polyphosphate and 5 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0042] The preparation method of modified basalt fiber comprises the following steps:
[0043] 15g of basalt fiber was ground and then immersed in a 1mol / L sodium hydroxide solution, washed and dried, and then heat treated at 350°C for 2h to obtain pretreated basalt fiber;
[0044] 12 g of pretreated basalt fiber was dispersed in 200 mL of methanol solvent, and then 10 g of polyurethane resin and 6 g of silane coupling agent KH550 were added thereto, and the mixture was heated, stirred and refluxed at 85° C. for 2 h. After the reaction was completed, the reaction product was washed and dried to obtain modified basalt fiber;
[0045] (3) Fabric preparation: The glue is evenly coated on the outer layer of the pretreated polyester base fabric and dried at 130°C for 4 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0046] Example 3
[0047] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0048] (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. The irradiation dose is 30 kGy and the irradiation dose rate is 3 kGy / h. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric.
[0049] (2) Preparation of coating: 90 g of epoxy resin, 5 g of blocked isocyanate crosslinking agent, 2 g of tributyl phosphate and 3 g of alumina powder were stirred and mixed uniformly, and then 15 g of modified basalt fiber, 8 g of ammonium polyphosphate and 6 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0050] The preparation method of modified basalt fiber comprises the following steps:
[0051] 15g of basalt fiber was ground and then immersed in a 2mol / L sodium hydroxide solution, washed and dried, and then heat treated at 380°C for 3h to obtain pretreated basalt fiber;
[0052] 15 g of pretreated basalt fiber was dispersed in 200 mL of methanol solvent, and then 12 g of polyurethane resin and 5 g of silane coupling agent KH560 were added thereto, and the mixture was heated, stirred and refluxed at 90° C. for 2 h. After the reaction was completed, the reaction product was washed and dried to obtain modified basalt fiber;
[0053] (3) Fabric preparation: The glue is evenly coated on the outer layer of the pretreated polyester base fabric and dried at 140°C for 4 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0054] Example 4
[0055] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0056] (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. The irradiation dose is 40 kGy and the irradiation dose rate is 5 kGy / h. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric.
[0057] (2) Preparation of coating: 100 g of epoxy resin, 8 g of blocked isocyanate crosslinking agent, 2 g of tributyl phosphate and 3 g of alumina powder were stirred and mixed uniformly, and then 14 g of modified basalt fiber, 8 g of ammonium polyphosphate and 5 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0058] The preparation method of modified basalt fiber comprises the following steps:
[0059] 15g of basalt fiber was ground and then immersed in a 2mol / L sodium hydroxide solution, washed and dried, and then heat treated at 400°C for 2h to obtain pretreated basalt fiber.
[0060] 15 g of pretreated basalt fiber was dispersed in 200 mL of methanol solvent, and then 10 g of polyurethane resin and 6 g of silane coupling agent KH560 were added thereto, and the mixture was heated, stirred and refluxed at 80° C. for 2 h. After the reaction was completed, the reaction product was washed and dried to obtain modified basalt fiber;
[0061] (3) Fabric preparation: The glue is evenly coated on the outer layer of the pretreated polyester base fabric and dried at 150°C for 3 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0062] Comparative Example 1
[0063] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0064] (1) Preparation of coating: 90 g of epoxy resin, 5 g of blocked isocyanate crosslinking agent, 2 g of tributyl phosphate and 3 g of alumina powder were stirred and mixed uniformly, and then 15 g of modified basalt fiber, 8 g of ammonium polyphosphate and 6 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0065] The preparation method of modified basalt fiber comprises the following steps:
[0066] 15g of basalt fiber was ground and then immersed in a 2mol / L sodium hydroxide solution, washed and dried, and then heat treated at 380°C for 3h to obtain pretreated basalt fiber;
[0067] 15 g of pretreated basalt fiber was dispersed in 200 mL of methanol solvent, and then 12 g of polyurethane resin and 5 g of silane coupling agent KH560 were added thereto, and the mixture was heated, stirred and refluxed at 90° C. for 2 h. After the reaction was completed, the reaction product was washed and dried to obtain modified basalt fiber;
[0068] (2) Fabric preparation: The glue is evenly coated on the outer layer of the polyester base fabric and dried at 140°C for 4 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0069] Comparative Example 2
[0070] A method for preparing high-strength outdoor tent fabric comprises the following preparation steps:
[0071] (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. The irradiation dose is 30 kGy and the irradiation dose rate is 3 kGy / h. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric.
[0072] (2) Preparation of coating: 90 g of epoxy resin, 5 g of blocked isocyanate crosslinking agent, 2 g of tributyl phosphate and 3 g of alumina powder were stirred and mixed uniformly, and then 15 g of basalt fiber powder, 8 g of ammonium polyphosphate and 6 g of decabromodiphenylethane were added thereto, stirred and mixed uniformly, and then ultrasonically defoamed to obtain coating;
[0073] (3) Fabric preparation: The glue is evenly coated on the outer layer of the pretreated polyester base fabric and dried at 140°C for 4 min. The thickness of the glue after drying is 0.8 mm. After cooling, the outdoor tent fabric is obtained.
[0074] The tent fabrics prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, wherein the tensile strength was tested according to ASTM D638, the peel strength was tested according to HG / T 2581-2009, and the folding resistance was tested according to FZ / T 01143-2018. The test results are shown in the following table:
[0075] Tensile strength (MPa) Peel strength longitudinal (N / 50mm) Folding resistance (times) Example 1 83 169 870 Example 2 88 167 879 Example 3 86 166 857 Example 4 85 168 862 Comparative Example 1 61 142 573 Comparative Example 2 69 153 494
[0076] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A method for preparing high-strength outdoor tent fabric, It is characterized in that The specific preparation steps are as follows: (1) Fabric pretreatment: Place the polyester base in an irradiation room and perform gamma ray irradiation treatment. After the irradiation treatment is completed, take out the base fabric to obtain a pretreated polyester base fabric. (2) Preparation of coating: epoxy resin, blocked isocyanate crosslinking agent, tributyl phosphate and alumina powder are stirred and mixed evenly, and then modified basalt fiber, ammonium polyphosphate and decabromodiphenylethane are added thereto, stirred and mixed evenly, and then ultrasonically defoamed to obtain coating; (3) Fabric preparation: The glue obtained in step (2) is evenly scraped onto the outer layer of the pretreated polyester base fabric, and then dried and cooled to obtain an outdoor tent fabric; In step (2), the mass ratio of the epoxy resin, the blocked isocyanate crosslinking agent, tributyl phosphate, alumina powder, modified basalt fiber, ammonium polyphosphate and decabromodiphenylethane is 80-100:4-8:1-3:2-3:10-15:5-10:3-6; In step (3), the drying temperature is 120-150°C, the drying time is 3-5 minutes, and the thickness of the glue after drying is 0.8-1.5 mm; The preparation method of the modified basalt fiber comprises the following steps: (01) Grinding and crushing the basalt fiber, then immersing it in an alkali solution, washing and drying it, and then heat treating it at 300-400°C for 2-3h to obtain the pretreated basalt fiber; (02) The pretreated basalt fiber is dispersed in a methanol solvent, and then a polyurethane resin and a silane coupling agent are added thereto. The mixture is heated, stirred and refluxed for reaction. After the reaction is completed, the reaction product is washed and dried to obtain the modified basalt fiber.
2. The method for preparing the high-strength outdoor tent fabric according to claim 1, It is characterized in that In step (1), the irradiation dose is 20-40 kGy, and the irradiation dose rate is 1-5 kGy / h.
3. The method for preparing the high-strength outdoor tent fabric according to claim 1, It is characterized in that In step (01), the alkali solution is a sodium hydroxide solution, and the concentration of the alkali solution is 1-2 mol / L.
4. The method for preparing the high-strength outdoor tent fabric according to claim 1, It is characterized in that In step (02), the mass ratio of the pretreated basalt fiber, the polyurethane resin and the silane coupling agent is 10-20:8-12:4-8.
5. The method for preparing the high-strength outdoor tent fabric according to claim 1, It is characterized in that In step (02), the silane coupling agent is selected from one or more of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
6. The method for preparing the high-strength outdoor tent fabric according to claim 1, It is characterized in that In step (02), the reflux reaction temperature is 70-90° C., and the reflux reaction time is 2-3 h.
7. The high-strength outdoor tent fabric prepared by the preparation method according to any one of claims 1 to 6.