Method for calculating temperature loss during the production of ultra-low carbon steel in RH refining furnace
By dividing the temperature drop during the treatment process of the RH-TB refining furnace into three parts and establishing a temperature model formula, the end temperature is calculated based on the vacuum chamber interval time, which solves the problem of inaccurate temperature control of the RH-TB refining furnace and achieves higher automation. Control, reduce accidents and waste, and improve product quality and production efficiency.
Patent Information
- Application Number
- CN202210193232.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The temperature control of the RH-TB refining furnace during the molten steel treatment process is inaccurate, resulting in frequent steel leakage or pouring stoppage accidents, affecting the quality of the cast slab, and manual operation is difficult, resulting in operational errors and waste.
Divide the temperature drop during the treatment process into three parts, establish a temperature model formula, judge the temperature drop speed based on the vacuum chamber interval time, automatically calculate the end temperature, and improve the accuracy and automation of temperature control.
Reduce manual operation errors, reduce accident rates, improve the degree of automation, reduce the labor intensity of skilled workers, achieve staff reduction, increase efficiency, and improve product quality.
Smart Images

Figure BDA0003525093980000031
Abstract
Description
Technical Field
[0001] The invention relates to the field of iron and steel metallurgy, and in particular to a method for calculating temperature loss in a process of producing ultra-low carbon steel in an RH refining furnace. Background Art
[0002] When the RH-TB refining furnace processes molten steel, there are many factors that affect the temperature. At present, all temperature-related calculations and controls are manually operated by the furnace master, which is very difficult. The casting machine has very high requirements for the temperature of the molten steel during the casting process. When the temperature is higher than the target temperature, it is necessary to take speed reduction measures to avoid steel leakage accidents, which will have a serious impact on the quality of the ingot. When the temperature is lower than the target temperature, it is easy to stop pouring accidents. Therefore, once the furnace master makes an inaccurate judgment on the temperature, it will bring very serious consequences. Based on this, a method for calculating the temperature loss during the processing of ultra-low carbon steel produced by the RH-TB furnace is developed, which can improve the accuracy of temperature control, reduce costs and increase efficiency, and improve product quality. Summary of the invention
[0003] The object of the present invention is to provide a method for calculating the temperature loss in the process of producing ultra-low carbon steel in an RH refining furnace, which can improve the automation control level of the TH-TB furnace, reduce costs, increase efficiency, and improve production capacity.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The method for calculating the temperature loss during the production of ultra-low carbon steel in the RH refining furnace includes the following methods:
[0006] 1) The temperature drop of the treatment process is divided into three parts:
[0007] Early stage of treatment: start treatment until the pressure is less than 0.2kPa;
[0008] Mid-treatment period: pressure < 0.2 kPa until the molten steel is calm;
[0009] Late stage of treatment: molten steel is calmed until the treatment is completed;
[0010] 2) Establish temperature model formula: T 终点温度 =T 开始处理温度 -T 前期温降 -T 中期温降 -T 后期温降 ;
[0011] 3) Determine the temperature drop before, during and after treatment based on the vacuum chamber interval time:
[0012] a) When the vacuum chamber interval time is greater than 60 minutes, the temperature drop rate from the start of treatment to the pressure less than 0.2 kPa is A℃ / min, the temperature drop rate from the pressure less than 0.2 kPa to the molten steel being calmed is A-1.8℃ / min, and the temperature drop rate from the molten steel being calmed to the end of treatment is A-2.0℃ / min;
[0013] b) When 60min≥vacuum chamber interval time≥30min, the temperature drop rate from the start of treatment to pressure <0.2kPa is B℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is B-1.4℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is B-1.6℃ / min;
[0014] c) When 30min>vacuum chamber interval time>15min, the temperature drop rate from the start of treatment to pressure<0.2kPa is C℃ / min, the temperature drop rate from pressure<0.2kPa to molten steel calming is C-1℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is C-1.2℃ / min;
[0015] d) When the vacuum chamber interval time is ≤15min, the temperature drop rate from the start of treatment to pressure <0.2kPa is D℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is D-0.9℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is D-1.1℃ / min;
[0016] e) When the interval time between two consecutive vacuum chambers is ≤15min, the temperature drop rate from the start of treatment to pressure <0.2kPa is E℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is E-0.7℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is E-0.9℃ / min;
[0017] f) When the interval time of the vacuum chamber is ≤15min for three or more tanks in a row, the temperature drop rate from the start of treatment to pressure <0.2kPa is F℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is F-0.6℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is F-0.8℃ / min.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention discloses a method for calculating temperature loss in a processing process of producing ultra-low carbon steel in an RH refining furnace, which can reduce manual operation errors, accidents and waste, improve the degree of automation, effectively solve the instability of technical operations, reduce the labor intensity of technical workers, and achieve the purpose of reducing staff and increasing efficiency. DETAILED DESCRIPTION
[0020] The following examples are used to specifically illustrate the present invention. These examples are only general descriptions of the present invention and do not limit the present invention.
[0021] The method for calculating the temperature loss during the production of ultra-low carbon steel in the RH refining furnace includes the following methods:
[0022] 1) The temperature drop of the treatment process is divided into three parts:
[0023] Early stage of treatment: start treatment until the pressure is less than 0.2kPa;
[0024] Mid-treatment period: pressure < 0.2 kPa until the molten steel is calm;
[0025] Late stage of treatment: molten steel is calmed until the treatment is completed;
[0026] 2) Establish temperature model formula: T 终点温度 =T 开始处理温度 -T 前期温降 -T 中期温降 -T 后期温降 ;
[0027] T 前期温降 = initial temperature drop rate × initial time;
[0028] T 中期温降 = mid-term temperature drop rate × mid-term time;
[0029] T 后期温降 = later temperature drop rate × later time.
[0030] T 开始处理温度 In order to measure it, the endpoint temperature is directly calculated according to the formula according to the different interval time of the vacuum chamber.
[0031] 3) According to the vacuum chamber interval time, the temperature drop before, during and after the treatment is determined as shown in Table 1:
[0032] Table 1 Temperature drop before, during and after treatment based on vacuum chamber interval time
[0033]
[0034] Example 1: A method for calculating temperature loss during the production of ultra-low carbon steel in an RH refining furnace, as follows:
[0035] 1) The temperature of molten steel at the beginning of treatment is 1610℃;
[0036] 2) The interval time for treating molten steel in the vacuum chamber is 35 minutes;
[0037] 3) The temperature drop rate from the start of treatment to the pressure <0.2kPa is B=3, the time from the start of treatment to the pressure less than 0.2kPa is 8min, the time from the pressure less than 0.2kPa to the molten steel being calmed is 10min, and the time from the molten steel being calmed to the end of treatment is 10min;
[0038] 4) According to formula T 终点温度 =T 开始处理温度 -T 前期温降 -T 中期温降 -T 后期温降 calculate:
[0039] T 终点温度 =1610-3×8-1.6×10-1.4×10=1556℃
[0040] 5) Based on the temperature calculated by the formula and the planned removal temperature of the molten steel, the molten steel is heated and cooled.
Claims
1. A method for calculating temperature loss during the production of ultra-low carbon steel in an RH refining furnace, characterized in that: The following methods are included: 1) The temperature drop of the treatment process is divided into three parts: Early stage of treatment: start treatment until the pressure is less than 0.2kPa; Mid-treatment period: pressure < 0.2 kPa until the molten steel is calm; Late stage of treatment: molten steel is calmed until the treatment is completed; 2) Establish temperature model formula: T 终点温度 =T 开始处理温度 -T 前期温降 -T 中期温降 -T 后期温降 ; 3) Determine the temperature drop before, during and after treatment based on the vacuum chamber interval time: a) When the vacuum chamber interval time is greater than 60 minutes, the temperature drop rate from the start of treatment to the pressure less than 0.2 kPa is A℃ / min, the temperature drop rate from the pressure less than 0.2 kPa to the molten steel being calmed is A-1.8℃ / min, and the temperature drop rate from the molten steel being calmed to the end of treatment is A-2.0℃ / min; b) When 60min≥vacuum chamber interval time≥30min, the temperature drop rate from the start of treatment to pressure <0.2kPa is B℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is B-1.4℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is B-1.6℃ / min; c) When 30min>vacuum chamber interval time>15min, the temperature drop rate from the start of treatment to pressure<0.2kPa is C℃ / min, the temperature drop rate from pressure<0.2kPa to molten steel calming is C-1℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is C-1.2℃ / min; d) When the vacuum chamber interval time is ≤15min, the temperature drop rate from the start of treatment to pressure <0.2kPa is D℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is D-0.9℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is D-1.1℃ / min; e) When the interval time between two consecutive vacuum chambers is ≤15min, the temperature drop rate from the start of treatment to pressure <0.2kPa is E℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is E-0.7℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is E-0.9℃ / min; f) When the interval time of the vacuum chamber is ≤15min for three or more tanks in a row, the temperature drop rate from the start of treatment to pressure <0.2kPa is F℃ / min, the temperature drop rate from pressure <0.2kPa to molten steel calming is F-0.6℃ / min, and the temperature drop rate from molten steel calming to the end of treatment is F-0.8℃ / min.
Citation Information
Patent Citations
RH refining furnace chemical heating method suitable for low-carbon aluminum killed steel
CN110527775A