A preparation method of polyamide masterbatch carrier resin and polyamide masterbatch

By using copolyamide as the carrier resin, the melting point and fluidity are regulated, and combined with dispersant, the problem of poor dispersion uniformity of colorant in polyamide fibers is solved, and the fiber performance and the quality of the raw liquid colored polyamide fibers are improved.

CN114685818BActive Publication Date: 2024-11-26CHINESE TEXTILE ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011628179.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-31
Publication Date
2024-11-26
Estimated Expiration
2040-12-31

AI Technical Summary

Technical Problem

Polyamide fibers have poor dispersion uniformity of colorant during melt spinning, resulting in low fiber performance, especially when the colorant particle size is small, the dispersion state is worse, which affects the quality of the raw liquid colored polyamide fiber.

Method used

Copolyamide is used as the carrier resin, and by regulating the copolymerization ratio of caprolactam and nylon 66 salt and the copolymerization ratio of branching agent, copolyamides with low melting point and excellent fluidity are prepared, combined with an appropriate amount of dispersing agent to realize the colorant in the carrier resin. evenly dispersed.

Benefits of technology

Improve the processing performance and fiber performance of polyamide masterbatch, ensure uniform dispersion of colorants in copolyamide, improve the quality of the raw liquid colored polyamide fiber, especially maintain good dispersion when the particle size of the colorant is small. Effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114685818B_ABST
    Figure CN114685818B_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a polyamide masterbatch carrier resin and a polyamide masterbatch. By using copolyamide as the carrier resin and utilizing the low melting point and good fluidity of the copolyamide, uniform dispersion of a colorant in the carrier resin is achieved, and the problem that a colorant with a smaller particle size is difficult to disperse in a polyamide melt and has poor uniformity is overcome, thereby obtaining a polyamide masterbatch capable of preparing high-quality fine-denier polyamide colored fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material synthesis, and particularly relates to a preparation method of a polyamide masterbatch carrier resin and a polyamide masterbatch. Background Art

[0002] Polyamide 6 fiber has excellent properties such as moisture absorption, skin-friendly, wear resistance, high strength, chemical stability, good resilience, etc., and is widely used in clothing, industry and military fields. When processed into textiles, solution-dyed polyamide fiber can save the dyeing process, reduce a large amount of wastewater and carbon dioxide emissions, save energy and reduce consumption, and has outstanding environmental friendliness. It can effectively solve the outstanding problems of high energy consumption, high water consumption and high COD emissions faced by the traditional printing and dyeing industry from the source, and has great potential for future development.

[0003] At present, the most commonly used method for producing solution-dyed polyamide fibers is the masterbatch blending method. The masterbatch is blended with the polyamide matrix before spinning, and the polyamide fiber is melt-spinned to achieve the solution dyeing of the polyamide fiber. It is simple, flexible and has low production cost. The key to this technology is whether the masterbatch is evenly mixed with the matrix and whether the colorant component can be evenly dispersed in the spinning melt. Therefore, the quality of the masterbatch directly determines the quality of the solution-dyed polyamide fiber. However, since polyamide has a linear macromolecular chain structure and a high degree of molecular chain entanglement, it has a high relative viscosity and poor fluidity in the molten state, making it difficult to disperse the colorant in the polyamide melt, poor dispersion uniformity, poor spinnability, and other problems such as short component spinning cycle, difficult fiber refinement, and low fiber performance. It greatly affects the quality of the solution-dyed polyamide fiber. The higher melting point leads to the fact that the colorant cannot be well dispersed in the carrier resin during the melt spinning process, which reduces the performance of the solution-dyed polyamide fiber. Especially when the colorant particle size is small, its dispersion state is worse, and the fiber performance is further reduced.

[0004] Therefore, the present invention is specially proposed. Summary of the invention

[0005] In view of the defects of the prior art, the present invention provides a method for preparing a polyamide masterbatch carrier resin and a polyamide masterbatch. By using copolyamide as the carrier resin and utilizing the low melting point and good fluidity of the copolyamide, the uniform dispersion of the colorant in the carrier resin is achieved, and the colorant can still be evenly dispersed when the particle size is small, thereby overcoming the problems of difficulty in dispersing the colorant in the polyamide melt and poor dispersion uniformity, and obtaining a polyamide masterbatch that can be used to prepare high-quality fine-denier polyamide colored fibers.

[0006] In order to achieve the above object, the first aspect of the present invention provides a polyamide masterbatch, comprising a colorant, a dispersant and a carrier resin, wherein the carrier resin is a copolyamide, and the copolyamide is a copolymer of caprolactam, nylon 66 salt and a branching agent, and the filter press value DF of the polyamide masterbatch is not higher than 0.05MPa·cm 2 / g.

[0007] The copolyamide prepared with caprolactam, nylon 66 salt and lysine as raw materials has a branched structure and has better fluidity and a lower melting point. The melting point of the copolyamide can be adjusted by adjusting the copolymerization ratio of caprolactam and nylon 66 salt, and the branching degree of the copolyamide can be adjusted by adjusting the copolymerization ratio of the branching agent.

[0008] The filter pressure value is not higher than 0.05MPa·cm 2 / g achieves uniform dispersion of colorant powder in the carrier resin,

[0009] Furthermore, the proportions of the colorant, dispersant and carrier resin are as follows:

[0010] Colorant 5-60%;

[0011] Dispersant 1-20%;

[0012] Carrier resin 20~90%.

[0013] Furthermore, the branching agent is at least one of lysine, pyromellitic acid, and aminocaprolactam.

[0014] Preferably, the branching agent is aminocaprolactam.

[0015] Furthermore, the molar ratio of the caprolactam, nylon 66 salt and branching agent is 100:5-30:0.1-1.

[0016] The above ratio is the molar percentage range that can obtain higher fluidity and lower melting point summarized by technicians in a large number of experiments. The copolyamide prepared using this ratio has a lower melting point, is more conducive to melt spinning, and has excellent fluidity. It can achieve sufficient mixing with the colorant under the condition of small colorant particle size, thereby improving mixing uniformity.

[0017] Furthermore, the copolyamide is a copolymer with a branched structure, and its branching degree is 0.05 to 0.5.

[0018] The above-mentioned branching degree range is the branching degree range of the copolyamide that can obtain a lower melting point without affecting the fluidity, which is summarized by technicians in a large number of experiments.

[0019] Preferably, the branching degree of the copolyamide is 0.2 to 0.5.

[0020] The copolyamide having the above preferred branching degree can further improve the dispersibility of the colorant and achieve more uniform dispersion of the colorant.

[0021] Furthermore, the melt index of the copolyamide is not less than 40 g / 10 min (220° C., 2.16 kg).

[0022] The higher the melt index, the better its flow properties. The melt index of copolyamide is not less than 40g / 10min (220°C, 2.16kg), which indicates that it has good flow properties.

[0023] Further, the colorant can be selected from carbon black, pigment white 6, pigment brown 3, pigment blue 5, pigment blue 15, pigment blue 15:1, pigment blue 15:3, pigment blue 15:4, pigment blue 15:6, pigment blue 16, pigment blue 28, pigment blue 29, pigment blue 60, pigment violet 19, pigment violet 23, pigment violet 29, pigment red 101, pigment red 102, pigment red 108, pigment red 112, pigment red 122, pigment red 146, pigment red 149, pigment red 170, pigment red 171, pigment red 172, pigment red 175, pigment red 176, pigment red 177, pigment red 178, pigment red 179, pigment red 185, pigment red 202, pigment red 207, pigment red 208, pigment red 214, pigment red 241, pigment red 242, pigment red 254, pigment red 255, pigment red 26 3. At least one of pigment red 264, pigment red 272, pigment yellow 6, pigment yellow 13, pigment yellow 14, pigment yellow 17, pigment yellow 21, pigment yellow 37, pigment yellow 77, pigment yellow 74, pigment yellow 81, pigment yellow 97, pigment yellow 107, pigment yellow 110, pigment yellow 120, pigment yellow 129, pigment yellow 138, pigment yellow 139, pigment yellow 147, pigment yellow 148, pigment yellow 150, pigment yellow 151, pigment yellow 155, pigment yellow 168, pigment yellow 174, pigment yellow 180, pigment yellow 187, pigment yellow 192, pigment yellow 195, pigment yellow 196, pigment yellow 197, pigment orange 34, pigment orange 36, pigment orange 43, pigment orange 61, pigment orange 64, pigment orange 68, pigment orange 70, pigment orange 73, pigment green 5, pigment green 7, pigment green 36, and pigment green 50.

[0024] In order to meet the conditions for preparing fine-denier colored polyamide fibers, the particle size of the colorant powder in the above scheme is not greater than 700 nm.

[0025] Furthermore, the dispersant is at least one of ethylene-acrylic acid copolymer wax, ethylene-acrylic acid based ionomer wax, and low melting point polyamide wax, and the solid content of the dispersant is 1%-20%.

[0026] Preferably, the dispersant is low melting point polyamide wax.

[0027] A second aspect of the present invention provides a method for preparing a polyamide masterbatch carrier resin, the preparation method comprising the following steps:

[0028] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer;

[0029] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer;

[0030] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer;

[0031] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices;

[0032] In the step S1, the temperature of the hydrolysis ring-opening copolymerization reaction is 220-260° C. and the pressure is 1-4 MPa; in the step S2, the temperature of the prepolymerization reaction is 230-270° C. and the pressure is 0.1-0.6 MPa; in the step S3, the temperature of the postpolymerization reaction is 230-260° C. and the pressure is -20-20 kPa.

[0033] When the polyamide masterbatch carrier resin is prepared using the above preparation method, the branching agent can generate a structure with no less than 3 reactive functional groups in step S1, and caprolactam and nylon 66 salt use this as the branching point of the macromolecular chain to obtain a copolyamide with a branched structure.

[0034] The above preparation method is obtained by technicians based on a large number of experiments. It is a preparation method that can prepare copolyamides with stable branching degree and melt index that meet the requirements. The copolyamide prepared using this preparation method has better flow properties, lower melting point, and more stable product performance.

[0035] The beneficial effects of the present invention are as follows: the branched structure of the copolyamide can further reduce the melting point of the copolyamide and further improve its fluidity; and the melting point of the copolyamide is regulated by regulating the copolymerization ratio of caprolactam and nylon 66 salt, and the branching degree of the copolyamide is regulated by regulating the copolymerization ratio of the branching agent to obtain a copolyamide carrier resin with the best mixing effect with a colorant; the polyamide masterbatch carrier resin is used to prepare the polyamide masterbatch, so that the colorant is uniformly dispersed in the copolyamide with a smaller particle size, and the processing performance of the polyamide masterbatch is improved; further, by using a dispersant with good compatibility with the polyamide, while promoting the dispersion effect of the colorant, the fluidity of the melt processing is further improved, and the polyamide masterbatch with excellent performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the accompanying drawings described below are only some embodiments. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0037] Figure 1 It is the melt flow curve of polyamide 6 and copolyamide.

[0038] Figure 2 DSC curves of polyamide 6 and copolyamide.

[0039] Figure 3 This is a 10,000x scanning electron microscope photo of the cross section of the copolyamide masterbatch. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is clearly and completely described below in conjunction with some embodiments. It can be understood by those skilled in the art that the following implementation is only used to explain the technical principle of the present invention and is not intended to limit the scope of protection of the present invention. For example, although the present application describes the steps of the method of the present invention in a specific order, these orders are not restrictive. Without departing from the basic principles of the present invention, those skilled in the art can perform the steps in different orders.

[0041] Embodiment 1

[0042] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0043] Caprolactam: 100;

[0044] Nylon 66 salt: 5;

[0045] Branching agent lysine: 0.1.

[0046] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0047] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260°C, and the reaction pressure is 4MPa;

[0048] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 270° C., and the reaction pressure is 0.6 MPa;

[0049] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 260° C., and the reaction pressure is 20 KPa;

[0050] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0051] The degree of branching of the copolyamide prepared using the above protocol is 0.1.

[0052] Embodiment 2

[0053] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0054] Caprolactam: 100;

[0055] Nylon 66 salt: 30;

[0056] Branching agent aminocaprolactam: 1.

[0057] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0058] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260°C, and the reaction pressure is 4MPa;

[0059] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 270° C., and the reaction pressure is 0.6 MPa;

[0060] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 260° C., and the reaction pressure is 20 KPa;

[0061] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0062] The degree of branching of the copolyamide prepared using the above protocol is 0.47.

[0063] Embodiment 3

[0064] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0065] Caprolactam: 100;

[0066] Nylon 66 salt: 24;

[0067] Branching agent aminocaprolactam: 0.7.

[0068] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0069] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260°C, and the reaction pressure is 4MPa;

[0070] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 270° C., and the reaction pressure is 0.6 MPa;

[0071] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 260° C., and the reaction pressure is 20 KPa;

[0072] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0073] The degree of branching of the copolyamide prepared using the above protocol is 0.35.

[0074] Embodiment 4

[0075] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0076] Caprolactam: 100;

[0077] Nylon 66 salt: 5;

[0078] Branching agent: pyromellitic acid: 0.1.

[0079] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0080] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 220°C, and the reaction pressure is 1MPa;

[0081] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 230° C., and the reaction pressure is 0.1 MPa;

[0082] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 230° C., and the reaction pressure is -20 KPa;

[0083] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0084] The degree of branching of the copolyamide prepared using the above protocol is 0.05.

[0085] Embodiment 5

[0086] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0087] Caprolactam: 100;

[0088] Nylon 66 salt: 20;

[0089] Branching agent aminocaprolactam: 1.

[0090] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0091] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 220°C, and the reaction pressure is 2MPa;

[0092] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 230° C., and the reaction pressure is 0.4 MPa;

[0093] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 230° C., and the reaction pressure is -20 KPa;

[0094] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0095] The degree of branching of the copolyamide prepared using the above protocol is 0.3.

[0096] Embodiment 6

[0097] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0098] Caprolactam: 100;

[0099] Nylon 66 salt: 24;

[0100] Branching agent lysine: 0.7.

[0101] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0102] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 220°C, and the reaction pressure is 1MPa;

[0103] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 230° C., and the reaction pressure is 0.1 MPa;

[0104] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 230° C., and the reaction pressure is -20 KPa;

[0105] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0106] The degree of branching of the copolyamide prepared using the above protocol is 0.26.

[0107] Embodiment 7

[0108] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0109] Caprolactam: 100;

[0110] Nylon 66 salt: 14;

[0111] Branching agent aminocaprolactam: 0.3.

[0112] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0113] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 240°C, and the reaction pressure is 3MPa;

[0114] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260° C., and the reaction pressure is 0.4 MPa;

[0115] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 245° C., and the reaction pressure is 5 KPa;

[0116] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0117] The degree of branching of the copolyamide prepared using the above protocol is 0.2.

[0118] Embodiment 8

[0119] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0120] Caprolactam: 100;

[0121] Nylon 66 salt: 20;

[0122] Branching agent lysine: 1.

[0123] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0124] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 220°C, and the reaction pressure is 4MPa;

[0125] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260° C., and the reaction pressure is 0.6 MPa;

[0126] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 230° C., and the reaction pressure is 20 KPa;

[0127] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0128] The degree of branching of the copolyamide prepared using the above protocol is 0.35.

[0129] Embodiment 9

[0130] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0131] Caprolactam: 100;

[0132] Nylon 66 salt: 9;

[0133] Branching agent: pyromellitic acid: 0.1.

[0134] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0135] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 240°C, and the reaction pressure is 3MPa;

[0136] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260° C., and the reaction pressure is 0.4 MPa;

[0137] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 245° C., and the reaction pressure is 5 KPa;

[0138] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0139] The degree of branching of the copolyamide prepared using the above protocol is 0.06.

[0140] Embodiment 10

[0141] As an embodiment of the present invention, this embodiment provides a method for preparing a polyamide masterbatch carrier resin. In this embodiment, the raw material ratio (molar ratio) used is as follows:

[0142] Caprolactam: 100;

[0143] Nylon 66 salt: 28;

[0144] Branching agent aminocaprolactam: 1.

[0145] Specifically, the preparation method of the polyamide masterbatch carrier resin is as follows:

[0146] S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer, the reaction temperature is 240°C, and the reaction pressure is 3MPa;

[0147] S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer, the reaction temperature is 260° C., and the reaction pressure is 0.4 MPa;

[0148] S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer, the reaction temperature is 245° C., and the reaction pressure is 5 KPa;

[0149] S4, pelletizing, extracting and drying the copolyamide final polymer obtained in step S3 in sequence to obtain copolyamide slices.

[0150] The copolyamide prepared using the above protocol has a branching degree of 0.5.

[0151] Embodiment 11

[0152] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0153] Colorant 30%;

[0154] Dispersant 10%;

[0155] Carrier resin 60%;

[0156] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 8.

[0157] Furthermore, the colorant is carbon black with a particle size of 20 nm, and the dispersant is low melting point polyamide wax with a solid content of 10%.

[0158] The carbon black, copolyamide and dispersant low melting point polyamide wax are uniformly mixed in a high-speed mixer and melt-mixed in a twin-screw extruder. The specific extrusion parameters are as follows:

[0159] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 260℃ 260℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0160] The extruder screw speed was 240 rpm.

[0161] The polyamide black masterbatch is obtained by extrusion granulation through the extruder.

[0162] Embodiment 12

[0163] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0164] Colorant 20%;

[0165] Dispersant 1%;

[0166] Carrier resin 79%.

[0167] The carrier resin is the polyamide masterbatch carrier resin prepared in Example 5.

[0168] Furthermore, the colorant is phthalocyanine blue 15:3 with a particle size of 200 nm, and the dispersant is ethylene-acrylic acid copolymer wax with a solid content of 1%.

[0169] Phthalocyanine blue 15:3, copolyamide and dispersant ethylene-acrylic acid copolymer wax are uniformly mixed in a high-speed mixer, and then melt-mixed in a twin-screw extruder. The specific extrusion parameters are as follows:

[0170] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 250℃ 250℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0171] The extruder screw speed was 240 rpm.

[0172] The polyamide blue masterbatch was obtained by extrusion granulation using the extruder.

[0173] Embodiment 13

[0174] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0175] Colorant 60%;

[0176] Dispersant 20%;

[0177] Carrier resin 20%.

[0178] The carrier resin is the polyamide masterbatch carrier resin prepared in Example 2.

[0179] Furthermore, the colorant is Pigment Red 254 with a particle size of 100 nm, and the dispersant is a low melting point polyamide wax with a solid content of 20%.

[0180] Pigment Red 254, copolyamide and dispersant low melting point polyamide wax are mixed evenly in a high-speed mixer and melt-kneaded in a twin-screw extruder. The specific extrusion parameters are as follows:

[0181] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 260℃ 260℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0182] The extruder screw speed was 240 rpm.

[0183] The polyamide red masterbatch was obtained by extrusion granulation using the extruder.

[0184] Embodiment 14

[0185] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0186] Colorant 5%;

[0187] Dispersant 5%;

[0188] Carrier resin 90%.

[0189] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 8.

[0190] Furthermore, the colorant is Pigment Green 50 with a particle size of 700 nm, and the dispersant is ethylene-acrylic acid copolymer wax with a solid content of 5%.

[0191] Pigment Green 50, copolyamide and dispersant ethylene-acrylic acid copolymer wax are mixed evenly in a high-speed mixer and melt-kneaded in a twin-screw extruder. The specific extrusion parameters are as follows:

[0192] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 260℃ 250℃ 240℃ 220℃ 190℃ 190℃ 210℃ 250℃

[0193] The extruder screw speed was 240 rpm.

[0194] The polyamide green masterbatch is obtained by extrusion granulation through the extruder.

[0195] Embodiment 15

[0196] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0197] Colorant 40%;

[0198] Dispersant 10%;

[0199] Carrier resin 50%.

[0200] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 3.

[0201] Furthermore, the colorant is Pigment Red 179 with a particle size of 240 nm, and the dispersant is a low melting point polyamide wax with a solid content of 10%.

[0202] Pigment Red 179, copolyamide and dispersant low melting point polyamide wax are mixed evenly in a high-speed mixer and melt-kneaded in a twin-screw extruder. The specific extrusion parameters are as follows:

[0203] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 250℃ 250℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0204] The extruder screw speed was 240 rpm.

[0205] The polyamide red masterbatch was obtained by extrusion granulation using the extruder.

[0206] Embodiment 16

[0207] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0208] Colorant 25%;

[0209] Dispersant 5%;

[0210] Carrier resin 70%.

[0211] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 6.

[0212] Furthermore, the colorant is Pigment Yellow 148 with a particle size of 160 nm, and the dispersant is ethylene-acrylic acid based ionomer wax with a solid content of 5%.

[0213] Pigment Yellow 148, copolyamide and dispersant ethylene-acrylic acid based ionomer wax are uniformly mixed in a high-speed mixer and melt-mixed in a twin-screw extruder. The specific extrusion parameters are as follows:

[0214] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 250℃ 250℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0215] The extruder screw speed was 240 rpm.

[0216] The polyamide yellow masterbatch was obtained by extrusion granulation using the extruder.

[0217] Embodiment 17

[0218] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0219] Colorant 5%;

[0220] Dispersant 5%;

[0221] Carrier resin 90%.

[0222] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 8.

[0223] Furthermore, the colorant is carbon black with a particle size of 20 nm, and the dispersant is low melting point polyamide wax with a solid content of 10%.

[0224] The carbon black, copolyamide and dispersant low melting point polyamide wax are uniformly mixed in a high-speed mixer and melt-mixed in a twin-screw extruder. The specific extrusion parameters are as follows:

[0225] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 260℃ 260℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0226] The extruder screw speed was 240 rpm.

[0227] The polyamide black masterbatch is obtained by extrusion granulation through the extruder.

[0228] Embodiment 18

[0229] As an embodiment of the present invention, this embodiment provides a polyamide masterbatch, including a carrier resin, a dispersant and a colorant, wherein the mass percentages of the colorant, the dispersant and the carrier resin are:

[0230] Colorant 30%;

[0231] Dispersant 10%;

[0232] Carrier resin 60%;

[0233] The above-mentioned carrier resin is the polyamide masterbatch carrier resin prepared in Example 10.

[0234] Furthermore, the colorant is carbon black with a particle size of 20 nm, and the dispersant is low melting point polyamide wax with a solid content of 10%.

[0235] The carbon black, copolyamide and dispersant low melting point polyamide wax are uniformly mixed in a high-speed mixer and melt-mixed in a twin-screw extruder. The specific extrusion parameters are as follows:

[0236] Temperature Zone Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 District 8 Machine head temperature 240℃ 260℃ 260℃ 240℃ 220℃ 200℃ 200℃ 210℃ 250℃

[0237] The extruder screw speed was 240 rpm.

[0238] The polyamide black masterbatch is obtained by extrusion granulation through the extruder.

[0239] Comparative Example 1

[0240] In this comparative example, polyamide 6 and polyamide 66 were copolymerized at a mass ratio of 1:1 to obtain a random copolymerized polyamide 6 / 66 copolymer.

[0241] Comparative Example 2

[0242] This comparative example uses the same preparation method and raw material ratio as Example 11, but is different from Example 11 in that the carrier resin used in this comparative example is polyamide 6.

[0243] Comparative Example 3

[0244] This comparative example uses the same preparation method and raw material ratio as Example 12. The difference from Example 12 is that the carrier resin used in this comparative example is polyamide 6.

[0245] Comparative Example 4

[0246] This comparative example uses the same preparation method and raw material ratio as Example 13. The difference from Example 13 is that the carrier resin used in this comparative example is polyamide 6.

[0247] Comparative Example 5

[0248] This comparative example uses the same preparation method and raw material ratio as Example 11. The difference from Example 11 is that the carrier resin used in this comparative example is the random copolymer of polyamide 6 and polyamide 66 in Comparative Example 1.

[0249] Comparative Example 6

[0250] This comparative example uses the same preparation method and raw material ratio as Example 12. The difference from Example 12 is that the carrier resin used in this comparative example is the random copolymer of polyamide 6 and polyamide 66 in Comparative Example 1.

[0251] Comparative Example 7

[0252] This comparative example uses the same preparation method and raw material ratio as Example 13. The difference from Example 13 is that the carrier resin used in this comparative example is the random copolymer of polyamide 6 and polyamide 66 in Comparative Example 1.

[0253] Experimental Example 1

[0254] This experimental example tests the branching degree and melt index MF of the polyamide masterbatch carrier resin prepared in the above examples 1 to 10, and the results are as follows:

[0255]

[0256] It can be seen from the above data that the polyamide masterbatch carrier resin is prepared by the method of the present invention in Examples 1 to 10, and the melt index is significantly improved compared with Comparative Example 1 and nylon 6, indicating that the polyamide masterbatch carrier resin of the present invention has better fluidity and stronger processing performance in a molten state. Among them, Example 8 has the same ratio as Example 5, and the degree of branching is also similar, but the melt index of Example 8 is higher than that of Example 5, indicating that the control of temperature and pressure in the preparation method will also have a certain effect on the polyamide masterbatch carrier resin, and the polyamide masterbatch carrier resin obtained by the hydrolysis ring-opening reaction temperature is low and the polymerization reaction temperature is high has a lower degree of branching and better fluidity.

[0257] Experimental Example 2

[0258] This experimental example is to measure the filtration value DF (MPa.cm) of the polyamide masterbatch prepared in the above examples and comparative examples. 2 / g) test, test method: using a filtration performance tester, the filter screen is a filter area of ​​3.8cm 2 The breaking strength (cN / dtex) of the solution-dyed polyamide fiber prepared by blending the polyamide masterbatch prepared in the above embodiment and comparative example with polyamide 6 at a mass ratio of 5:95 was tested in accordance with GB / T14344-2008. The results are shown in the following table:

[0259]

[0260] It can be seen from the table that the filtration pressure values ​​DF of the polyamide masterbatches prepared in Examples 11 to 18 are all less than 0.05 MPa·cm 2 / g, while Comparative Examples 2 to 7 use polyamide 6 or random copolymers of polyamide 6 and polyamide 66 as carrier resins, and their filtration pressure values ​​DF are all higher than 0.05 MPa·cm 2 / g, indicating that the polyamide masterbatch prepared by using the polyamide masterbatch carrier resin of the present invention has a better dispersion state of the colorant; it also indicates that the carrier resin in the comparative example cannot disperse the colorant with a small particle size well, and the colorant cannot be completely and evenly dispersed, resulting in a decrease in its performance.

[0261] Further, Example 11, Comparative Example 2 and Comparative Example 5 use the same process, except that Comparative Example 2 uses a random copolymer of polyamide 6 and polyamide 66 as a masterbatch carrier, Comparative Example 5 uses polyamide 6 as a masterbatch carrier resin, and Example 11 uses the polyamide masterbatch carrier resin of the present invention. It can be seen from the table that the filter pressure value of Example 11 is 0.035 MPa·cm 2 / g, and the fiber breaking strength is 6.1 cN / dtex, which is significantly better than that of Comparative Example 2 and Comparative Example 5, further illustrating that the dispersion state of the colorant in the polyamide masterbatch prepared by the polyamide masterbatch carrier resin of the present invention is better.

[0262] It can also be seen from the above table that both Example 11 and Example 17 use the polyamide masterbatch carrier resin of the present invention to prepare polyamide masterbatch, the difference being that in Example 11, the ratio of colorant to carrier resin is 1:2, while in Example 17, the ratio of colorant to carrier resin is 1:18; Example 11 uses more colorant, and its filter press value DF is still lower than that of Example 17, and the fiber breaking strength is also higher than that of Example 17; This indicates that the use of the polyamide masterbatch carrier resin of the present invention can further improve the dispersibility of the colorant, and can still ensure uniform dispersion of the colorant when the proportion of the colorant is increased, thereby obtaining a polyamide masterbatch with excellent performance.

[0263] It can also be seen from the comparison between Example 11 and Example 18 that Example 11 and Example 18 use the same ratio and method, the difference is that copolyamides with different degrees of branching are used, but the performance of Example 18 is significantly lower than that of Example 11, indicating that too high a degree of branching will reduce the dispersion uniformity of the colorant, thereby causing the performance of the masterbatch to decrease. From the comparison between Example 13 and Example 18, it can be seen that the filter press value DF of the masterbatch prepared using copolyamides with similar degrees of branching does not change much, but the fiber breaking strength decreases significantly with the further increase of the degree of branching, indicating that when the degree of branching is high, the dispersion of the colorant is relatively poor, thereby reducing the mechanical properties of the masterbatch.

[0264] Experimental Example 3

[0265] This experimental example tests the light resistance of the polyamide masterbatches prepared in Examples 11 to 15, and the test results are as follows:

[0266]

[0267] It can be seen from the above table that the color fastness grade of the polyamide masterbatch prepared using the polyamide masterbatch carrier resin of the present invention is ≥4, which is higher than the color fastness requirement for making wearable clothes, indicating that the polyamide masterbatch prepared using the polyamide masterbatch carrier resin of the present invention has better coloring performance and the product is not easy to fade.

[0268] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modifications to equivalent embodiments of equivalent changes by using the technical content suggested above without departing from the scope of the technical solution of the present invention. The implementation scheme in the above embodiment can also be further combined or replaced. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the solution of the present invention.

Claims

1. A polyamide masterbatch for solution-dyed polyamide fiber, comprising a colorant, a dispersant and a carrier resin, characterized in that: The colorant, dispersant and carrier resin have a ratio of: colorant 5-60%; dispersant 1-20%; carrier resin 20-90%; the dispersant is at least one of ethylene-acrylic acid copolymer wax, ethylene-acrylic acid ionomer wax and low melting point polyamide wax; the particle size of the colorant powder is not greater than 700nm; the filter press value DF of the polyamide masterbatch is not higher than 0.05MPa·cm 2 / g; The carrier resin is a copolyamide with a branched structure, and its branching degree is 0.05-0.

5. The copolyamide is obtained by copolymerizing caprolactam, nylon 66 salt and a branching agent; the molar ratio of the caprolactam, nylon 66 salt and the branching agent is 100:5-30:0.1-1; The branching agent is at least one of lysine, pyromellitic acid, and aminocaprolactam; The melt index of the copolyamide is not less than 40 g / 10 min when tested at 220° C. and 2.16 kg; The preparation method of the carrier resin comprises: S1, transporting the raw materials to a pre-polymerization reactor for hydrolysis and ring-opening copolymerization to obtain a copolyamide prepolymer; S2, transporting the copolyamide precursor prepared in step S1 to a prepolymerization reactor for prepolymerization to obtain a copolyamide prepolymer; S3, transporting the copolyamide prepolymer obtained in step S2 to a post-polymerization reactor for post-polymerization reaction to obtain a copolyamide final polymer; S4, the copolyamide final polymer obtained in step S3 is successively pelletized, extracted and dried to obtain a copolyamide slice; In the step S1, the temperature of the hydrolysis ring-opening copolymerization reaction is 220-260° C. and the pressure is 1-4 MPa; in the step S2, the temperature of the prepolymerization reaction is 230-270° C. and the pressure is 0.1-0.6 MPa; in the step S3, the temperature of the postpolymerization reaction is 230-260° C. and the pressure is -20-20 kPa.

2. The polyamide masterbatch according to claim 1, characterized in that: The branching agent is aminocaprolactam.

3. The polyamide masterbatch according to claim 1, characterized in that: The branching degree of the copolyamide is 0.2-0.

5.

4. The polyamide masterbatch according to any one of claims 1 to 3, characterized in that: The colorant is carbon black, pigment white 6, pigment brown 3, pigment blue 5, pigment blue 15, pigment blue 15:1, pigment blue 15:3, pigment blue 15:4, pigment blue 15:6, pigment blue 16, pigment blue 28, pigment blue 29, pigment blue 60, pigment violet 19, pigment violet 23, pigment violet 29, pigment red 101, pigment red 102, pigment red 108, pigment red 112, pigment red 122, pigment red 146, pigment red 149, pigment red 170, pigment red 171, pigment red 172, pigment red 175, pigment red 176, pigment red 177, pigment red 178, pigment red 179, pigment red 185, pigment red 202, pigment red 207, pigment red 208, pigment red 214, pigment red 241, pigment red 242, pigment red 254, pigment red 255, pigment red 263, pigment red 271, pigment red 272, pigment red 273, pigment red 274, pigment red 275 at least one of pigment red 264, pigment red 272, pigment yellow 6, pigment yellow 13, pigment yellow 14, pigment yellow 17, pigment yellow 21, pigment yellow 37, pigment yellow 77, pigment yellow 74, pigment yellow 81, pigment yellow 97, pigment yellow 107, pigment yellow 110, pigment yellow 120, pigment yellow 129, pigment yellow 138, pigment yellow 139, pigment yellow 147, pigment yellow 148, pigment yellow 150, pigment yellow 151, pigment yellow 155, pigment yellow 168, pigment yellow 174, pigment yellow 180, pigment yellow 187, pigment yellow 192, pigment yellow 195, pigment yellow 196, pigment yellow 197, pigment orange 34, pigment orange 36, pigment orange 43, pigment orange 61, pigment orange 64, pigment orange 68, pigment orange 70, pigment orange 73, pigment green 5, pigment green 7, pigment green 36, and pigment green 50.