Precision circuit packaging substrate based on surface protection and its processing technology
By using the combination of conventional copper foil and corrosion-resisted layer in single-sided buried technology, the problems of high cost and complex process of ultra-thin copper materials are solved, and efficient buried layer formation and plate surface flatness are achieved, suitable for small Line width, small line spacing, high density wiring products.
Patent Information
- Application Number
- CN202210325646.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-03-30
AI Technical Summary
In the existing single-sided buried wire technology, the use of ultra-thin copper materials is costly and complex in process, which leads to excessive erosion of the buried wire layer lines, affecting the flatness of the board surface, and cannot meet the small line width, small line distance, and high-density wiring products. processing requirements.
The carrier layer is made using conventional copper foil and a resist layer is formed on its surface. The buried wire layer is formed through electroplating and subsequent processes. The difference in thermal expansion coefficient between the frame and the copper foil is used to maintain the tight state of the copper foil, reduce material costs and control bite Erode the end point to ensure flatness of the plate.
It reduces material costs, improves product yield and flatness, is suitable for double-sided panels and multi-layer boards, meets the minimum line width/line distance 8/8um design requirements, simplifies the process flow and reduces costs.
Smart Images

Figure CN114698270B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a packaging substrate, and in particular to a precision circuit packaging substrate based on surface protection and a processing technology thereof. Background Art
[0002] With the development of electronic technology and people's requirements for miniaturization and high precision of electronic products, the requirements for packaging substrates are getting higher and higher. The existing masking process can no longer meet the processing requirements of small line width, small line spacing and high-density wiring products. Therefore, the application requirements of semi-additive method, buried wire and other processes are getting higher and higher; but in the existing single-sided buried wire technology, the carrier uses an ultra-thin copper (such as 3-5μm thick copper foil) structure. This special material has a high cost and a complicated manufacturing process. In addition, when removing the ultra-thin copper at the bottom of the buried wire product after depaneling, the control of the amount of bite is relatively strict, which can easily lead to excessive line bite of the buried wire layer. There will be a relatively obvious height difference between the copper surface and the insulating medium layer, which reduces the flatness of the entire board surface; thus greatly limiting the promotion and application of the buried wire process.
[0003] Application Contents
[0004] In order to overcome the above-mentioned defects, the present application provides a processing technology for a precision circuit packaging carrier based on surface protection. In the processing technology, conventional copper foil is used to make the carrier layer, and an anti-corrosion layer is formed on the surface of the copper foil, thereby reducing the material production cost, controlling the end point of the buried wire layer circuit corrosion, and thus ensuring the flatness of the circuit board surface.
[0005] The technical solution adopted by this application to solve its technical problems is:
[0006] A processing technology for a precision circuit packaging substrate based on surface protection includes the following steps:
[0007] Step 1: Preparation of a carrier: prepare two conventional copper foils, and glue the two copper foils together to form a carrier, that is, the carrier includes a first copper foil layer and a second copper foil layer, and the two outer surfaces of the carrier are defined as outer surfaces, and the two inner surfaces of the carrier are defined as inner surfaces, and the two inner surfaces are glued together;
[0008] Step 2: Preparation of the anti-corrosion layer: a layer of tin is plated on at least one outer surface of the carrier to form an anti-corrosion layer, and a bare pattern circuit area is formed on the anti-corrosion layer, and a non-pattern circuit area on the outer surface of the carrier is covered with a photosensitive layer;
[0009] Step 3: Preparation of the first buried wire layer:
[0010] 3.1 Electroplating: Electroplating is used to form the embedded first buried wire layer on the exposed pattern circuit area on the anti-corrosion layer of the carrier;
[0011] 3.2 De-filming: De-film the electroplated product to remove the photosensitive layer, exposing the graphic circuit and its spacing space;
[0012] Step 4: Post-processing
[0013] 4.1 Add-on layer production: Fill the first buried wire layer with insulating medium to form an insulating medium layer;
[0014] 4.2 Production of the second buried wire layer:
[0015] ① Blind hole processing: Processing blind holes in the insulating dielectric layer;
[0016] ②Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer and the blind hole;
[0017] ③ Fabrication of graphic circuits: fabricating a second buried wiring layer on the seed layer;
[0018] 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer;
[0019] 4.4 Removing the carrier: firstly, the first copper foil layer and the second copper foil layer are separated, and then the first copper foil layer or the second copper foil layer is removed by etching to obtain a product with an anti-corrosion layer;
[0020] 4.5 Removal of the anti-corrosion layer: Use tin stripping liquid to remove the anti-corrosion layer in the product to obtain a product with a buried wire layer on one side.
[0021] Preferably, in step 1: a frame is also prepared, and the first copper foil layer and the second copper foil layer are bonded together through the frame, specifically: at a temperature of 80-120°C, glue is coated on the upper and lower surfaces of the frame, and then two pieces of copper foil are respectively attached to the upper and lower surfaces of the frame to form a carrier, the frame is an annular structure with a hollow interior, the width of the frame is 5-15 mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16-18ppm / °C.
[0022] Preferably, the step 1 is specifically as follows: after a layer of glue is evenly coated around one of the copper foils near the edge area, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to solidify to form a carrier.
[0023] Preferably, the above step 4.4 specifically includes the following process:
[0024] ① Edge milling: perform edge milling 2-5mm away from the inner side of the frame to separate the first copper foil layer from the second copper foil layer;
[0025] ②Frame processing: After the milling frame is etched, the residual glue and impurities are removed to obtain a reusable frame;
[0026] ③Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
[0027] Preferably, the above step 4.4 specifically includes the following process:
[0028] ① Edge milling: perform edge milling 2-5mm from the inner side of the connection between the first copper foil layer and the second copper foil layer to separate the first copper foil layer from the second copper foil layer;
[0029] ②Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
[0030] Preferably, the step 2 specifically includes the following process:
[0031] ① Pretreatment: Clean and roughen the outer surface of the carrier;
[0032] ② Anti-corrosion layer preparation: Tin plating is performed on the entire outer surface of the carrier to form an anti-corrosion layer, and the thickness of the anti-corrosion layer is controlled to be 0.5-2.0 μm;
[0033] ③Production of graphic circuit area: Through lamination, exposure and development, the graphic circuit area to be produced is exposed, and the non-graphic circuit area is covered with a photosensitive layer that resists electroplating.
[0034] Preferably, the step 2 specifically includes the following process:
[0035] ① Pretreatment: Clean and roughen the outer surface of the carrier;
[0036] ② Pattern circuit area production: Through lamination, exposure and development, the pattern circuit area to be produced is exposed, and the non-pattern circuit area is covered with a photosensitive layer that resists electroplating;
[0037] ③ Preparation of anti-corrosion layer: Tin-plating the surface of the exposed pattern circuit area to form an anti-corrosion layer, the thickness of which is controlled to be 0.5-2.0 μm.
[0038] Preferably, the pattern circuit area production specifically includes the following processes:
[0039] ① Lamination: Make a photosensitive layer, and evenly apply a photosensitive layer on the outer surface of the carrier by lamination or coating;
[0040] ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution;
[0041] ③ Development: The photosensitive layer in the unreacted area is removed, and the area where the photopolymerization reaction occurs is retained, that is, the graphic circuit area 18 to be produced is exposed, and the non-graphic circuit area is covered with the anti-plating photosensitive layer 15.
[0042] Preferably, the step 4.1 specifically includes the following process:
[0043] ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding force between the circuit and the insulating medium and improve product performance;
[0044] ②Filling with insulating medium: forming an insulating medium layer on the graphic circuit layer through lamination or vacuum lamination combined with baking process;
[0045] In step 4.2, in step ①, a blind hole is made by laser window opening and laser drilling, and the alignment reference during the production process is a target hole with an inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference during the production process is an inner target; in step 4.2, in step ②, a seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when the pattern is produced, according to the pattern wiring density, an additive method combined with pattern electroplating or a subtractive method combined with whole-board electroplating and etching process is used to carry out pattern layer production.
[0046] The present invention also provides a precision circuit packaging carrier based on surface protection, and the packaging carrier is processed by the above-mentioned processing technology.
[0047] The beneficial effects of this application are:
[0048] 1) Compared with the existing technology, the present application uses conventional copper foil to replace the high-cost ultra-thin copper, which greatly reduces the material cost, and the frame used can be reused, so the overall cost is very low. By utilizing the difference between the thermal expansion coefficients of the frame and the copper foil, the copper foil layer in the carrier is in a taut state, which improves the quality of the carrier and thus improves the yield of product manufacturing;
[0049] 2) During the processing, the whole board tinning scheme or the pattern tinning method can be flexibly selected in combination with product grade requirements and cost factors. If the whole board tinning scheme is adopted, the buried wire layer and the insulating layer are on the same horizontal line after tin stripping; if the pattern tinning scheme is adopted, the height difference between the buried wire layer and the insulating layer after tin stripping can be controlled to ≤2μm, so the buried wire layer circuit is protected by the tin layer, and the buried wire layer will not be attacked through the tin when the carrier copper foil is removed. The height difference between the copper surface and the substrate can be controlled, ensuring the flatness of the whole board surface. The buried wire layer circuit is protected by the tin layer, the process flow is simple, and the process cost is low;
[0050] 3) This processing technology is suitable for double-sided boards and multi-layer boards, and can meet the minimum line width / line spacing 8 / 8um design requirements. During the processing, double-sided processing can be performed on the carrier part, which improves product production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a schematic diagram of the structure of the present application without a frame carrier;
[0052] Figure 2 This is a schematic diagram of the structure of the frame carrier component in this application;
[0053] Figure 3 This is a schematic diagram of the structure of the carrier component after the entire plate is electroplated with a tin layer in this application;
[0054] Figure 4 This is a schematic diagram of the structure of the carrier component after the photosensitive layer is attached in this application;
[0055] Figure 5 This is a schematic diagram of the structure of the carrier component after the first buried wire layer is formed in the present application;
[0056] Figure 6 This is a schematic diagram of the structure of the carrier member in this application after removing the photosensitive layer;
[0057] Figure 7 It is a schematic diagram of the structure of the n-layer board in this application;
[0058] Figure 8 This is a schematic diagram of the structure of the n-layer board after removing the carrier member in this application;
[0059] Fig. 9 This is a schematic diagram of the structure of the n-layer board after the copper foil layer is removed in this application;
[0060] Fig.10 This is a schematic diagram of the structure of the n-layer board after the anti-etching layer is removed in this application;
[0061] In the figure: 10-carrier, 11-first copper foil layer, 12-second copper foil layer, 13-frame, 14-anti-corrosion layer, 15-photosensitive layer, 16-first buried wire layer, 17-insulating dielectric layer, 18-graphic circuit area, 21-second buried wire layer, 22-external graphic circuit layer. DETAILED DESCRIPTION
[0062] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0063] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the following drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0064] Embodiment: A processing technology for a precision circuit packaging substrate based on surface protection comprises the following steps:
[0065] Step 1: Preparation of carrier 10: Figure 1 Or as shown in 2, two conventional copper foils are prepared, and the two copper foils are glued together to form a carrier 10, that is, the carrier 10 includes a first copper foil layer 11 and a second copper foil layer 12, the two outer surfaces of the carrier 10 are defined as outer surfaces, and the two inner surfaces of the carrier 10 are defined as inner surfaces, and the two inner surfaces are glued together; the first copper foil layer 11 and the second copper foil layer 12 both have a first surface and a second surface relative to each other, the second surfaces of the first copper foil layer and the second copper foil layer are glued together, the two second surfaces are the inner surfaces of the carrier, the first surfaces of the first copper foil layer and the second copper foil layer are far away from each other, the two first surfaces are the outer surfaces of the carrier, and the outer surfaces are used for subsequent circuit production;
[0066] Step 2: Preparation of the anti-corrosion layer 14: Figure 3 As shown, a layer of tin is plated on at least one outer surface of the carrier 10 to form an anti-corrosion layer 14, and a bare pattern circuit area 18 is formed on the anti-corrosion layer 14, and a non-pattern circuit area on the outer surface of the carrier 10 is covered with a photosensitive layer 15, as shown in FIG. Figure 4As shown; the anti-corrosion layer 14 is a tin layer, and the circuit is made on any outer surface of the carrier member 10 for single-sided processing, and the circuit can also be made on two outer surfaces at the same time, and double-sided processing is performed to improve the production efficiency of the carrier;
[0067] Step 3: Making the first buried wiring layer 16: that is, making the surface embedded wiring.
[0068] 3.1 Electroplating: Figure 5 As shown, the embedded first buried wire layer 16 is formed by electroplating on the exposed pattern circuit area 18 on the anti-corrosion layer 14 of the carrier;
[0069] 3.2 De-filming: Figure 6 As shown, the electroplated product is subjected to a film stripping process to remove the photosensitive layer 15, exposing the pattern circuit and its spacing space;
[0070] Step 4: Post-processing
[0071] 4.1 Addition layer manufacturing: filling the first buried wire layer 16 with an insulating medium to form an insulating medium layer 17;
[0072] 4.2 Preparation of the second buried wire layer 21:
[0073] ① Blind hole processing: processing a blind hole in the insulating dielectric layer 17;
[0074] ②Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer 17 and the blind hole;
[0075] ③ Fabrication of graphic circuits: fabricating a second buried wiring layer 21 on the seed layer;
[0076] 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer 22; that is, the preparation of filling the insulating medium and the graphic circuit layer is repeated, and each time steps 4.1 and 4.2 are repeated, a layer of board is added. When the number of repetitions is 0, the formed board is a double-layer board, and when the number of repetitions is greater than or equal to 1, the formed board is a multi-layer board, such as Figure 7 As shown, the third buried wire layer to the n-1th buried wire layer and the insulating dielectric layer therebetween are omitted in the figure;
[0077] 4.4 Removing the carrier 10: Figure 8 As shown, firstly, the first copper foil layer 11 and the second copper foil layer 12 are separated, and then the first copper foil layer 11 or the second copper foil layer 12 is removed by etching to obtain a product having an anti-corrosion layer 14, such as Fig. 9As shown; when single-sided manufacturing is performed, for example, a circuit is made on the outer surface of the first copper foil layer, the carrier 10 is separated, the second copper foil layer 12 is removed, and the first copper foil layer 11 is etched away to obtain a plate with an anti-corrosion layer; when double-sided manufacturing is performed, circuits are made on both the first copper foil layer and the second copper foil layer, the carrier 10 is separated to obtain two plates, and the first copper foil layer or the second copper foil layer is etched away respectively to obtain two plates with an anti-corrosion layer;
[0078] 4.5 Removal of the resist layer 14: Fig.10 As shown, a tin stripping liquid is used to remove the anti-corrosion layer 14 in the product to obtain a product with a buried wire layer on one side. The tin stripping liquid will not attack the copper layer of the circuit, and can effectively control the height difference between the surface embedded circuit layer and the insulating dielectric layer; according to the product design requirements, the following post-processing is performed: solder mask → surface treatment → molding → finished product testing → finished product inspection → packaging and shipment to form a finished board, and the final finished product is the package carrier.
[0079] In one embodiment, in step 1: a frame 13 is also prepared, and the first copper foil layer 11 and the second copper foil layer 12 are bonded together through the frame 13, specifically: at a temperature of 80-120°C, glue is applied to the upper and lower surfaces of the frame 13, and then two pieces of copper foil are respectively bonded to the upper and lower surfaces of the frame to form a carrier 10, the frame 13 is an annular structure with a hollow interior, the width of the frame is 5-15mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16-18ppm / °C. Figure 2 As shown, the carrier component 10 is composed of a first copper foil layer 11, a frame 13 and a second copper foil layer 12. Preferably, the thickness of the conventional copper foil is 17.5 μm or 35 μm. When the temperature returns to room temperature, the copper foil has a larger CTE and shrinks more when cooled to room temperature, so that the copper foil is in a taut state, thereby improving the quality of the carrier component and thus improving the production yield of the product. At this time, the carrier component is completed and the subsequent production process can be single-sided or double-sided processing.
[0080] In another embodiment, the step 1 is specifically as follows: after a layer of glue is evenly coated around the edge of one of the copper foils, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to form the carrier 10. Figure 1 As shown, the carrier 10 is composed of a first copper foil layer 11 and a second copper foil layer 12. The two copper foils are bonded together only near the edge area by glue to facilitate subsequent board separation. Preferably, glue is applied within a range of about 10 mm near the edge of the copper foil. The thickness of the conventional copper foil is 17.5μm or 35μm.
[0081] When the carrier 10 is composed of the first copper foil layer 11, the frame 13 and the second copper foil layer 12, the above step 4.4 specifically includes the following processes:
[0082] ① Edge milling: edge milling is performed along the distance of 2-5mm from the inner side of the frame 13 to separate the first copper foil layer from the second copper foil layer; that is, the frame portion is removed by edge milling. If it is double-sided molding, it is separated into two boards, i.e., two products, after edge milling. If it is single-sided molding, it is separated into one board and one copper foil after edge milling. The first copper foil layer and the second copper foil layer are connected by the frame, which is more convenient for the board separation process;
[0083] ② Frame processing: the frame 13 after the edge milling processing is etched, the residual glue is removed, and the impurities are removed to obtain a reusable frame 13; the processed frame can be recycled and reused, which reduces the production cost of the product;
[0084] ③Remove the copper foil layer: remove the first copper foil layer or the second copper foil layer by alkaline etching. In this process, the etching solution will not attack the tin layer, thereby effectively preventing the etching solution from attacking the embedded circuits on the surface.
[0085] When the carrier 10 is composed of the first copper foil layer 11 and the second copper foil layer 12, the above step 4.4 specifically includes the following processes:
[0086] ① Edge milling: The first copper foil layer 11 and the second copper foil layer 12 are separated by edge milling at a distance of 2-5 mm from the inner side of the connection point. That is, the connection part of the first copper foil layer 11 and the second copper foil layer 12 is removed by edge milling. If it is double-sided molding, it is separated into two boards, i.e., two products after edge milling. If it is single-sided molding, it is separated into one board and one copper foil after edge milling.
[0087] ②Remove the copper foil layer: remove the first copper foil layer or the second copper foil layer by alkaline etching. In this process, the etching liquid will not attack the tin layer, thereby effectively preventing the etching liquid from attacking the embedded circuits on the surface.
[0088] In one embodiment, the step 2 specifically includes the following process:
[0089] ① Pretreatment: cleaning and roughening the outer surface of the carrier 10;
[0090] ② Preparation of anti-corrosion layer: Tin plating is performed on the entire outer surface of the carrier 10 to form an anti-corrosion layer 14, and the thickness of the anti-corrosion layer 14 is controlled to be 0.5-2.0 μm;
[0091] ③ Pattern circuit area production: Through lamination, exposure, and development, the pattern circuit area 18 to be produced is exposed, and the non-pattern circuit area is covered with a photosensitive layer 15 that resists electroplating. Figure 3 As shown, this solution is to tin the entire board, and the photosensitive layer is pressed onto the surface of the anti-corrosion layer. When the anti-corrosion layer is finally removed, the first buried wire layer and the first insulating medium layer are on the same horizontal line, and the flatness is very good.
[0092] In another embodiment, the step 2 specifically includes the following process:
[0093] ① Pretreatment: cleaning and roughening the outer surface of the carrier 10;
[0094] ② Pattern circuit area production: through lamination, exposure, and development, the pattern circuit area 18 to be produced is exposed, and the non-pattern circuit area is covered with an anti-plating photosensitive layer 15;
[0095] ③ Anti-corrosion layer preparation: Tin-plating the surface of the exposed pattern circuit area to form an anti-corrosion layer 14, the thickness of the anti-corrosion layer is controlled to be 0.5-2.0 μm; Figure 3 As shown, this scheme is graphic electroplating tin, that is, the photosensitive layer is directly pressed onto the outer surface of the carrier, and the tin layer is plated only in the graphic circuit area. When the anti-etching layer is finally removed, the first buried wire layer is recessed in the first insulating dielectric layer, and the height difference between the first buried wire layer and the first insulating dielectric layer is controlled to be ≤2.0μm.
[0096] The pattern circuit area production specifically includes the following processes:
[0097] ① Lamination: a photosensitive layer 15 is made by evenly coating the outer surface of the carrier 10 with a layer of photosensitive layer 15 by lamination or coating; the photosensitive layer is directly formed on the outer surface of the carrier or on the anti-corrosion layer on the outer surface;
[0098] ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution;
[0099] ③ Development: The photosensitive layer in the unreacted area is removed, and the area where the photopolymerization reaction occurs is retained, that is, the graphic circuit area 18 to be produced is exposed, and the non-graphic circuit area is covered with the anti-plating photosensitive layer 15.
[0100] The step 4.1 specifically includes the following process:
[0101] ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding strength between the circuit and the insulating medium and improve product performance; the graphic circuit layer is the first, second, third... buried wire layer. If the final carrier board is a three-layer board, the graphic circuit layer here is the first buried wire layer and the second buried wire layer. If the final carrier board is a four-layer board, the graphic circuit here is the first, second buried wire layer and the third buried wire layer, and so on.
[0102] ② Filling with insulating medium: forming an insulating medium layer 17 on the graphic circuit layer through a process of pressing or vacuum pressing combined with baking; the process of filling with insulating medium is not limited to the above two methods, as long as it matches the processing characteristics of the insulating medium.
[0103] In step 4.2, in step ①, a blind hole is made by laser windowing and laser drilling, and the alignment reference in the production process is the target hole with the inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference in the production process is the inner target; in step 4.2, in step ②, the seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when making the pattern, according to the pattern wiring density, the additive method is combined with the pattern electroplating or the subtractive method is combined with the whole board electroplating and etching process to carry out the pattern layer addition. Of course, the blind hole processing method is not limited to laser windowing plus laser drilling process or LDD (Laser Direct Drilling); the seed layer production is not limited to the copper deposition process and the sputtering process, and the same conduction function can be achieved; the pattern wiring is not limited to the additive method or the subtractive method, and the pattern production can be achieved, wherein the additive method, the pattern electroplating, the semi-additive method, the subtractive method, the whole board electroplating and etching are all conventional processes in this field, and will not be introduced in detail here.
[0104] like Fig.10 As shown, a precision circuit packaging carrier based on surface protection is obtained by adopting the above processing technology.
[0105] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present application, and these modifications and improvements are all within the scope of protection of the present application. Therefore, the scope of protection of the patent of the present application shall be subject to the attached claims.
Claims
1. A processing technology for a precision circuit packaging substrate based on surface protection, characterized in that: The steps include: Step 1: Preparation of a carrier member (10): preparing two conventional copper foils, and bonding the two copper foils together by glue to form a carrier member (10), that is, the carrier member (10) comprises a first copper foil layer (11) and a second copper foil layer (12), the two outer surfaces of the carrier member (10) are defined as outer surfaces, and the two inner surfaces of the carrier member (10) are defined as inner surfaces, and the two inner surfaces are bonded together; Step 2: Preparation of the anti-corrosion layer (14): a layer of tin is plated on at least one outer surface of the carrier (10) to form an anti-corrosion layer (14), and an exposed pattern circuit area (18) is formed on the anti-corrosion layer (14), and the non-pattern circuit area on the outer surface of the carrier (10) is covered with a photosensitive layer (15); Step 3: Preparation of the first buried wire layer (16): 3.1 Electroplating: forming an embedded first buried wire layer (16) by electroplating on the exposed pattern circuit area (18) on the anti-corrosion layer (14) of the carrier; 3.2 De-filming: De-filming the electroplated product to remove the photosensitive layer (15) to expose the pattern circuit and its spacing space; Step 4: Post-processing 4.1 Addition layer production: filling the first buried wire layer (16) with an insulating medium to form an insulating medium layer (17); 4.2 Preparation of the second buried wire layer (21): ① Blind hole processing: processing a blind hole in the insulating dielectric layer (17); ② Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer (17) and the blind hole; ③ Fabrication of graphic circuits: fabricating a second buried wiring layer (21) on the seed layer; 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer (22); 4.4 Removing the carrier (10): firstly, separating the first copper foil layer (11) and the second copper foil layer (12), and then removing the first copper foil layer (11) or the second copper foil layer (12) by etching, so as to obtain a product having an anti-corrosion layer (14); 4.5 Removing the anti-corrosion layer (14): using a tin stripping solution to remove the anti-corrosion layer (14) in the product, thereby obtaining a product having a buried wire layer on one side; The step 2 specifically includes the following process: ① Pretreatment: cleaning and roughening the outer surface of the carrier (10); ② Pattern circuit area production: through lamination, exposure, and development, the pattern circuit area (18) to be produced is exposed, and the non-pattern circuit area is covered with an anti-plating photosensitive layer (15); ③ Anti-corrosion layer preparation: Tin-plating the surface of the exposed pattern circuit area to form an anti-corrosion layer (14), wherein the thickness of the anti-corrosion layer is controlled to be 0.5 to 2.0 μm; The pattern circuit area production specifically includes the following processes: ① Lamination: manufacturing a photosensitive layer (15), uniformly coating a layer of photosensitive layer (15) on the outer surface of the carrier (10) by lamination or coating; ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution; ③ Development: removing the photosensitive layer in the unreacted area and retaining the area where the photopolymerization reaction occurs, that is, exposing the pattern circuit area (18) to be produced, and covering the non-pattern circuit area with the anti-plating photosensitive layer (15); The step 4.1 specifically includes the following process: ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding force between the circuit and the insulating medium and improve product performance; ② Filling with insulating medium: forming an insulating medium layer (17) on the pattern circuit layer by lamination or vacuum lamination combined with baking; In step 4.2, in step ①, a blind hole is made by laser window opening and laser drilling, and the alignment reference during the production process is a target hole with an inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference during the production process is an inner target; in step 4.2, in step ②, a seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when the pattern is produced, according to the pattern wiring density, an additive method combined with pattern electroplating or a subtractive method combined with whole-board electroplating and etching process is used to carry out pattern layer production.
2. The processing technology of the precision circuit packaging substrate based on surface protection according to claim 1 is characterized in that: In step 1: a frame (13) is also prepared, and the first copper foil layer (11) and the second copper foil layer (12) are bonded together through the frame (13), specifically: at a temperature of 80 to 120°C, glue is applied to the upper surface and the lower surface of the frame (13), and then two pieces of copper foil are respectively bonded to the upper surface and the lower surface of the frame to form a carrier (10), the frame (13) is an annular structure with a hollow interior, the width of the frame is 5 to 15 mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16 to 18ppm / °C.
3. The processing technology of the precision circuit packaging substrate based on surface protection according to claim 1 is characterized in that: The step 1 specifically comprises: after a layer of glue is evenly coated around the edge area of one of the copper foils, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to solidify to form a carrier (10).
4. The processing technology of the precision circuit packaging substrate based on surface protection according to claim 2 is characterized in that: The above step 4.4 specifically includes the following processes: ① Edge milling: edge milling is performed along the distance 2-5 mm from the inner side of the frame (13) to separate the first copper foil layer from the second copper foil layer; ② Frame processing: etching, removing residual glue and impurities from the frame (13) after edge milling to obtain a reusable frame (13); ③Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
5. The processing technology of the precision circuit packaging substrate based on surface protection according to claim 3 is characterized in that: The above step 4.4 specifically includes the following processes: ① Edge milling: edge milling is performed along the inner side of the connection between the first copper foil layer (11) and the second copper foil layer (12) at a distance of 2-5 mm, so as to separate the first copper foil layer (11) and the second copper foil layer (12); ②Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
6. The processing technology of the precision circuit packaging substrate based on surface protection according to claim 1 is characterized in that: The step 2 specifically includes the following process: ① Pretreatment: cleaning and roughening the outer surface of the carrier (10); ② Preparation of an anti-corrosion layer: Tin plating is performed on the entire outer surface of the carrier (10) to form an anti-corrosion layer (14), wherein the thickness of the anti-corrosion layer (14) is controlled to be 0.5 to 2.0 μm; ③ Pattern circuit area production: through lamination, exposure and development, the pattern circuit area (18) to be produced is exposed, and the non-pattern circuit area is covered with an anti-plating photosensitive layer (15).
7. A precision circuit packaging substrate based on surface protection, characterized in that: The method is manufactured by using the processing technology described in any one of claims 1 to 6.