Metallocene, catalyst containing the same, synthesis and application thereof

By designing a multi-substituted cyclopentadiene and five-membered heterocyclic metallocene catalyst, the problem of insufficient selectivity and activity of existing catalysts in polyolefin synthesis is solved, and efficient control of heavy olefin polymerization and oligomer selection is achieved. Improvement of sex.

CN114702531BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110000205.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-01
Publication Date
2024-12-06
Estimated Expiration
2041-01-01

AI Technical Summary

Technical Problem

Existing metallocene catalysts have problems of insufficient selectivity and activity in controlling polyolefin synthesis, especially in poor performance in heavy olefin polymerization and oligomer selectivity.

Method used

A multi-substituted cyclopentadiene and five-membered heterocyclic metallocene catalyst was designed to regulate the electron and space effects of the catalyst through specific synthesis methods and structural optimization, and improve the catalytic performance and selectivity. The catalyst consists of substituted acid chloride, five-membered heterocycle and metal atoms, synthesized by a series of reaction steps and combined with organoboride and alkyl metals for olefin polymerization.

Benefits of technology

The yield of trimerization, tetramerization and pentamerization terminal olefin products of heavy olefin polymerization is significantly improved, the formation of hydrogenation saturated products is reduced, the reactivity and selectivity of the catalyst is improved, and the catalytic performance of metallocene is optimized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The present invention discloses an olefin polymerization catalyst. The catalyst comprises a polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, an organic boron compound, an alkyl metal and a solvent; the metallocene is the main catalyst, and the organic boron compound and the alkyl metal are the co-catalysts; the molar ratio of the metallocene, the organic boron compound and the alkyl metal is 1: (0.8-1.4): (10-500); the weight proportion of the solvent in the catalyst is 70-90%. The catalyst of the present invention adopts a new metallocene structure, effectively regulates the electronic and spatial effects of the metallocene, and improves the yield of trimerization, tetramerization and pentamerization terminal olefin products of heavy olefin polymerization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metallocene and its application, in particular to a metallocene with a new structure and its synthesis and application. Background Art

[0002] Polyolefins have become a type of synthetic polymer material widely used in our daily lives. The market demand for traditional polyolefin materials, such as polyethylene and polypropylene, is still increasing. Polyolefin materials with specific functions such as optical properties continue to attract people's interest. Designing efficient transition metal complexes can accurately control olefin coordination polymerization, thereby synthesizing new polyolefin materials that are difficult to synthesize with traditional catalysts. Therefore, the research on designing efficient transition metal complexes to accurately control olefin coordination polymerization has received considerable attention.

[0003] Metallocene catalysts can synthesize a series of high-performance polyolefin products, such as isotactic polypropylene, syndiotactic polypropylene, atactic polypropylene, high-density polyethylene, low-density polyethylene, syndiotactic polystyrene and cyclic olefin copolymers, polybutene, PAO, etc. Metallocene catalysts have significant advantages in controlling the synthesis of polyolefin products. Further optimization of the catalyst structure and synthesis of new metallocene catalysts can synthesize polyolefin products with excellent performance.

[0004] CN1020101897 describes a type of metallocene catalyst structure containing N and O atoms in the side chain, which has high activity for olefin polymerization. CN102245620 also describes a large class of metallocene complexes with a substituent at the 5-position of the indenyl ring and optionally a substituted furanyl or thienyl at the 2-position of the indenyl ring, which improves the absorption efficiency of ethylene or α-olefins and can obtain a rubber component with a high molecular weight, especially an ethylene / propylene copolymer component. CN 105985372A describes a type of metallocene catalyst containing S or O heterocycles, which catalyzes the copolymerization of long-chain α-olefins. CN2016112389522 describes a bridged metallocene compound containing a heterocyclic structure, which is used for the copolymerization of ethylene and α-olefins, and improves the insertion rate of α-olefins. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a metallocene with a new structure, a catalyst containing the metallocene, and the synthesis and application thereof.

[0006] According to the first aspect of the present invention, the present invention provides a metallocene with a novel structure.

[0007] A polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, the general structural formula of which is shown below:

[0008]

[0009] In the formula, X is sulfur, nitrogen or oxygen, preferably sulfur or nitrogen; R 1 , R 2 , R 3 CH 3 , C 2 H 5 , C 3 H 7 , C 6 H 5 etc. alkyl, preferably CH 3 , C 2 H 5 ; M is Zr, Ti or Hf, preferably Zr; Z is Cl, Br, I, CH 3 , C 2 H 5 , C 3 H 7 or C 4 H 9 etc., preferably Cl, Br, I or C 2 H 5 ; m is the valence state of M metal -2.

[0010] According to the second aspect of the present invention, the present invention provides a method for synthesizing the above-mentioned metallocene.

[0011] A method for synthesizing a polysubstituted cyclopentadienyl five-membered heterocyclic metallocene comprises the following contents:

[0012] (1) Add the substituted acid chloride and the substituted five-membered heterocycle to a solvent, stir evenly, cool to -40 to 0°C, then add a catalyst, stir and react for 10 to 24 hours; separate the reaction materials to obtain the product Pa (number Pa);

[0013] (2) adding the Pa product obtained in step (1) and hexamethylenetetramine to acetic anhydride, stirring and reacting for 24 to 48 hours at a reaction temperature of 80 to 100°C; adding alkali solution, stirring and reacting for 1 to 4 hours; separating the organic matter by extraction technology; then adding the extract and a strong acid catalyst to a solvent, stirring and reacting at a reaction temperature of room temperature to 50°C for a reaction time of 1 to 4 hours; separating to obtain the product Pb;

[0014] (3) adding the product Pb obtained in step (2) to diethyl ether to prepare a solution Ep; adding lithium aluminum hydride to diethyl ether to prepare a lithium aluminum hydride diethyl ether solution Es; cooling the solution Es to -20 to -40°C; adding the solution Ep dropwise to the solution Es, heating to room temperature to 40°C, and reacting for 1 to 2 hours; separating and obtaining the product Pc by extraction-vacuum distillation technology;

[0015] (4) adding the product Pc obtained in step (3) and a strong acid catalyst to a solvent, heating and refluxing for 0.5 to 2 hours, and obtaining the product Pd by separation;

[0016] (5) dissolving the product Pd prepared in step (4) in a solvent, cooling to -40 to 0°C, adding alkyl lithium dropwise, stirring and reacting for 0.5 to 3 hours at a temperature of room temperature to 40°C; then adding chloride, stirring and reacting for 24 to 48 hours at a temperature of room temperature to 40°C, and obtaining a solution S;

[0017] (6) The solvent in the solution S obtained in step (5) is drained, methyl chloride is added to dissolve, the solid-liquid is separated, and the solution is concentrated by distillation to obtain the product CpM.

[0018] Furthermore, the substituted acyl chloride structure in step (1) is R-CH 2 -CO-Cl, R is various alkyl groups and aromatic hydrocarbons. Specifically, the substituted acyl chloride structure can be acetyl chloride, propionyl chloride, butyryl chloride, phenylacetyl chloride or phenylpropionyl chloride. The structure of the five-membered heterocyclic ring is , R (R1, R2) are various alkyl and aromatic hydrocarbons. The solvent is at least one of benzene, toluene, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide, etc., preferably benzene (0.8765g / cm 3 ) or toluene.

[0019] Furthermore, the catalyst in step (1) is anhydrous aluminum chloride or anhydrous tin chloride, preferably anhydrous tin chloride. The extraction-reduced pressure distillation is a conventional technology in the art, and the extraction agent used in the extraction process is at least one of dichloromethane, chloroform, dichloroethane, benzene, toluene, etc., preferably benzene.

[0020] Furthermore, in step (1), the molar ratio of the substituted acid chloride, the substituted five-membered heterocycle and the catalyst is 1:(0.8-1.2):(0.01-0.1), and the weight ratio of the substituted five-membered heterocycle to the solvent is 1:(4-10). The reaction is stirred for 10-24 hours in step (1). The separation in step (1) adopts conventional operations in the art, such as extraction-decompression distillation technology.

[0021] The alkali solution in step (2) is an aqueous solution of alkali, and the alkali is sodium hydroxide, sodium tert-butoxide, sodium bicarbonate, etc., preferably sodium hydroxide. The extractant is dichloromethane, chloroform, dichloroethane, benzene, toluene, etc., preferably dichloromethane. The strong acid catalyst is methanesulfonic acid, ethylsulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, hydrochloric acid, sulfuric acid, etc., preferably methanesulfonic acid.

[0022] In step (2), the concentration of the alkali solution is 1 to 4 mol / L. The molar ratio of Pa, hexamethylenetetramine and acetic anhydride is 1:(0.8 to 1.6):(1.2 to 2.0), and the molar ratio of alkali to acetic anhydride is 1:(5 to 10). The molar ratio of Pa product to strong acid catalyst is 1:(0.1 to 0.5). The weight ratio of Pa product to solvent is generally 1:(4 to 10). The separation of the reaction materials in step (2) adopts conventional operations in the art, such as extraction-vacuum distillation technology.

[0023] In step (3), the concentration of the obtained solution Ep is 1-3 mol / L. The concentration of the lithium aluminum hydride ether solution is generally 0.1-0.3 mol / L. The molar ratio of the product Pb to lithium aluminum hydride is 1:(0.2-0.4).

[0024] The strong acid catalyst in step (4) is methanesulfonic acid, ethylsulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid (172 g / mol), hydrochloric acid, sulfuric acid, etc., preferably p-toluenesulfonic acid. The solvent is chloroform, carbon tetrachloride, benzene, toluene, etc., preferably benzene. Further, the molar ratio of Pc to the strong acid catalyst is 1: (0.02-0.05), and the weight ratio of Pc to the solvent is 1: (10-18). The separation in step (4) adopts operations well known in the art, such as extraction-decompression distillation technology.

[0025] The chloride salt in step (5) is zirconium chloride, hafnium chloride, titanium chloride, etc. Preferably zirconium chloride. The solvent in step (5) is diethyl ether, tetrahydrofuran, etc. Preferably tetrahydrofuran. Further, the molar ratio of Pd to butyl lithium and zirconium chloride is 1: (1.8-2.4): (0.4-0.6). The weight ratio of Pd to solvent is 1: (8-20).

[0026] The alkyl lithium described in step (5) includes ethyl lithium, propyl lithium, butyl lithium, etc. Butyl lithium is preferred. The concentration of the alkyl lithium solution is 2-4 mol / L.

[0027] In step (6), the weight ratio of S to dichloromethane is 1:(10-20). The chloromethane is one of dichloromethane, chloroform and carbon tetrachloride.

[0028] According to the third aspect of the present invention, the third aspect of the present invention also provides an olefin polymerization catalyst, which contains the multi-substituted cyclopentadienyl five-membered heterocyclic metallocene described above.

[0029] The olefin polymerization catalyst comprises a polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, an organic boron compound, an alkyl metal and a solvent; the metallocene is the main catalyst, the organic boron compound and the alkyl metal are the co-catalysts; the molar ratio of the metallocene, the organic boron compound and the alkyl metal is 1: (0.8-1.4): (10-500). Preferably, it is 1: (0.9-1.3): (20-100). The weight proportion of the solvent in the catalyst is 70-90%.

[0030] Furthermore, the organic boron compound is selected from BF 3 , B(CF 3 ) 3 、[MePhNH][B(CF 3 ) 3 ]、[(Me) 2 PhNH][B(CF 3 ) 4 ]、[R 2 NH][B(CF 3 ) 3 ]、[R 3 N][B(CF 3 ) 3 ]、[R 3 NH][B(CF 3 ) 4 ]、[Ph 3 C][B(CF 3 ) 2 ]、[NH 3 ][B(CH 3 ) 3 ]、[Ph(Me) 2 N][B(C 6 F 5 ) 3 ]、[Ph(Me) 2 NH][B(C 6 F 5 ) 4 ], wherein R=C 2 -C 10 The organoboron compound is preferably [(Me) 2 PhNH][B(CF 3 ) 4 ]、[R 3 NH][B(CF 3 ) 4 ] or [Ph(Me) 2 NH][B(C 6 F 5 ) 4 ], more preferably [Ph(Me) 2NH][B(C 6 F 5 ) 4 ].

[0031] Further, the alkyl metal includes at least one of alkyl magnesium, alkyl aluminum, and alkyl zinc. The alkyl magnesium is selected from at least one of the group consisting of diethyl magnesium, dipropyl magnesium, diisopropyl magnesium, and dibutyl magnesium; the alkyl aluminum is selected from at least one of the group consisting of trimethyl aluminum, triethyl aluminum, tripropyl aluminum, triisopropyl aluminum, tributyl aluminum, and tri-tert-butyl aluminum; the alkyl zinc is selected from at least one of diethyl zinc, dipropyl zinc, diisopropyl zinc, dibutyl zinc, and di-tert-butyl zinc. Preferably, the alkyl metal is tributyl aluminum and tri-tert-butyl aluminum, and more preferably tri-tert-butyl aluminum.

[0032] Furthermore, the solvent may be at least one of benzene, toluene, n-octane, n-decane, alkylate, and the like.

[0033] According to a fourth aspect of the present invention, the present invention also provides an olefin polymerization reaction, wherein the above-mentioned olefin polymerization catalyst is used.

[0034] Specifically, the olefin polymerization reaction includes the following steps: introducing olefin and catalyst into an autoclave, and performing polymerization reaction under polymerization reaction conditions.

[0035] Furthermore, the conditions for the oligomerization reaction are as follows: the reaction temperature is 40 to 100° C., preferably 60 to 80° C., and the reaction time is 1 to 8 hours, preferably 2 to 4 hours.

[0036] Compared with the prior art, the catalyst and preparation method of the present invention have the following beneficial effects:

[0037] The catalyst of the present invention adopts a novel metallocene structure, effectively regulates the electronic and spatial effects of metallocene, and can significantly improve the yield of trimerization, tetramerization and pentamerization terminal olefin products of heavy olefin polymerization. Specifically, the five-membered heterocyclic ring increases the aromaticity of cyclopentadiene. At the same time, the presence of heteroatoms causes the electron cloud of the aromatic ring to shift, which helps to stabilize the alkyl or hydrogen atoms on the metallocene, promote the exposure of the cationic center, thereby promoting the coupling of macromolecular olefins with the cationic center, and realizing chain initiation and chain growth. The presence of substituents further promotes the movement of electrons to zirconium metal, reduces the positive charge of zirconium metal, is conducive to β-H elimination reaction, realizes chain termination, and prevents the appearance of olefin polymers. The effective adjustment of the three factors optimizes the catalytic performance of metallocene and improves the selectivity of oligomers such as trimerization, tetramerization and pentamerization of heavy olefin polymerization. At the same time, the steric hindrance and power supply effect prevent the bimolecular dehydrogenation reaction of metallocene, effectively reduces the generation of hydrogenation saturated products of olefin reactants, and improves the reaction activity of the catalyst. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0039] The organic solvent used in the experiment was purified on a Mikaelona SolvPurer A3 / G3 solvent purification system, and the purification of organic solvents is an operation well known to those skilled in the art. The required anhydrous and oxygen-free operation was carried out in a Mikaelona Super (1220 / 750) glove box. The product analysis was performed using an Agilent 7890A gas chromatograph. The element detection of the catalyst was performed using a ZSX100e X-ray fluorescence spectrometer produced by Rigaku Corporation of Japan.

[0040] The reagents and solvents used in the examples were from J&K and were chemically pure.

[0041] Example 1

[0042] (1) Add 92g propionyl chloride (92.5g / mol) and 95g 2,3-dimethylpyrrole (95g / mol) to 736g benzene (0.8765g / cm3), stir evenly, cool to -20℃, and then drop 13g anhydrous tin chloride (260g / mol). Stir and react for 20h. Use extraction-vacuum distillation technology to separate the product Pa1 (151g / mol). The yield is 91%.

[0043] (2) Add 75.5 g of the Pa1 product obtained in step (1) and 91 g of hexamethylenetetramine (140 g / mol) to 92 g of acetic anhydride (102 g / mol), stir and react for 20 h at a reaction temperature of 90 ° C. Add 56 mL of 2 mol / L sodium hydroxide and stir and react for 3 h. Separate the organic matter by extraction technology. Then add the extract and 14.4 g of methanesulfonic acid (96 g / mol) to 608 g of dichloromethane, stir and react at a reaction temperature of 30 ° C for 2 h. Use extraction-vacuum distillation technology to separate the product Pb1. The yield is 88%.

[0044] (3) Add 41 g of the product Pb1 (163 g / mol) obtained in step (2) to 125 mL of ether to prepare a solution Ep1. The concentration of Ep1 is 2 mol / L. Add 2.9 g of lithium aluminum hydride (38 g / mol) to 375 mL of ether to prepare a lithium aluminum hydride ether solution with a concentration of 0.2 mol / L. Cool the solution to -30°C. Add Ep1 dropwise to the lithium aluminum hydride ether solution. Heat to 30°C and react for 2 h. Use extraction-vacuum distillation technology to separate the product P1c. The yield is 84%.

[0045] (4) 41 g of the product Pc1 (165 g / mol) obtained in step (3) and 1.2 g of benzenesulfonic acid (158 g / mol) were added to 615 g of benzene and heated under reflux for 1.5 h. The product Pd1 was isolated by extraction-vacuum distillation. The yield was 89%.

[0046] (5) 18 g of the product Pd1 (147 g / mol) prepared in step (4) was dissolved in 270 g of tetrahydrofuran, cooled to -40°C, and 131 mL of a 2 mol / L butyl lithium hexane solution was added dropwise, and the mixture was stirred for 2 h at a reaction temperature of 30°C. Then 14.6 g of zirconium chloride (233 g / mol) was added, and the mixture was stirred for 30 h at a reaction temperature of 30°C to obtain a solution S.

[0047] (6) The solvent in the solution S1 obtained in step (4) was drained, 560 g of dichloromethane was added to dissolve, the solid-liquid separation was carried out, and the product CpM1 was obtained by distillation and concentration. The yield was 94%. The total yield of CpM1 was 56%.

[0048] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0049]

[0050] Among them, R1, R2, and R3 are CH 3 ; X is nitrogen; M is Zr; Z is Cl; m is 2.

[0051] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is N2C20ZrCl2H24, and the theoretical weight percentage composition is 6.17wt%N: 52.86wt%C: 20.04wt%Zr: 15.64wt%Cl: 5.29wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0052] Example 2

[0053] (1) Add 92 g of propionyl chloride (92.5 g / mol) and 114 g of 2,3-dimethylpyrrole (95 g / mol) to 920 g of benzene (0.8765 g / cm 3 ), stirred evenly, cooled to -20°C, and then 26g of anhydrous tin chloride (260g / mol) was added dropwise. Stirred and reacted for 20h. The product Pa2 (151g / mol) was separated by extraction-vacuum distillation technology. The yield was 88%.

[0054] (2) Add 75.5 g of the Pa product obtained in step (1) and 112 g of hexamethylenetetramine (140 g / mol) to 102 g of acetic anhydride (102 g / mol), stir and react for 20 h at a reaction temperature of 90 ° C. Add 50 mL of 2 mol / L sodium hydroxide and stir and react for 3 h. Separate the organic matter by extraction technology. Then add the extract and 24 g of methanesulfonic acid (96 g / mol) to 755 g of dichloromethane, stir and react at a reaction temperature of 30 ° C for 2 h. Use extraction-vacuum distillation technology to separate the product Pb2. The yield is 81%.

[0055] (3) Add 41 g of the product Pb2 (163 g / mol) obtained in step (2) to 83 mL of ether to prepare a solution Ep2. The concentration of Ep2 is 3 mol / L. Add 3.8 g of lithium aluminum hydride (38 g / mol) to 1000 mL of ether to prepare a lithium aluminum hydride ether solution with a concentration of 0.1 mol / L. Cool the solution to -30°C. Add Ep2 dropwise to the lithium aluminum hydride ether solution. Heat to 30°C and react for 2 h. Use extraction-vacuum distillation technology to separate the product Pc2. The yield is 79%.

[0056] (4) 41 g of the product Pc2 (165 g / mol) obtained in step (3) and 2 g of benzenesulfonic acid (158 g / mol) were added to 738 g of benzene and heated under reflux for 1.5 h. The product Pd2 was separated by extraction-vacuum distillation technology. The yield was 91%.

[0057] (5) 18 g of the product Pd2 (147 g / mol) prepared in step (4) was dissolved in 360 g of tetrahydrofuran, cooled to -40°C, and 150 mL of a 2 mol / L butyl lithium hexane solution was added dropwise, and the mixture was stirred for 2 h at a reaction temperature of 30°C. Then 17.5 g of zirconium chloride (233 g / mol) was added, and the mixture was stirred for 30 h at a reaction temperature of 30°C to obtain a solution S.

[0058] (6) The solvent in the solution S2 obtained in step (4) was drained, 700 g of dichloromethane was added to dissolve, the solid-liquid separation was carried out, and the product CpM2 was obtained by distillation and concentration. The yield was 93%. The total yield of CpM2 was 47%.

[0059] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0060]

[0061] Among them, R1, R2, and R3 are CH 3 ; X is nitrogen; M is Zr; Z is Cl; m is 2.

[0062] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is N2C20ZrCl2H24, and the theoretical weight percentage composition is 6.17wt%N: 52.86wt%C: 20.04wt%Zr: 15.64wt%Cl: 5.29wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0063] Example 3

[0064] (1) Add 92g propionyl chloride (92.5g / mol) and 76g 2,3-dimethylpyrrole (95g / mol) to 368g benzene (0.8765g / cm3), stir evenly, cool to -20℃, and then drop 2.6g anhydrous tin chloride (260g / mol). Stir and react for 20h. Use extraction-vacuum distillation technology to separate the product Pa3 (151g / mol). The yield is 79%.

[0065] (2) Add 75.5 g of the Pa3 product obtained in step (1) and 56 g of hexamethylenetetramine (140 g / mol) to 61 g of acetic anhydride (102 g / mol), stir and react for 20 h at a reaction temperature of 90 ° C. Add 60 mL of 2 mol / L sodium hydroxide and stir and react for 3 h. Separate the organic matter by extraction technology. Then add the extract and 4.8 g of methanesulfonic acid (96 g / mol) to 302 g of dichloromethane, stir and react, the reaction temperature is 30 ° C, and the reaction time is 2 h. Use extraction-vacuum distillation technology to separate the product Pb3. The yield is 78%.

[0066] (3) Add 41 g of the product Pb3 (163 g / mol) obtained in step 2 to 250 mL of ether to prepare solution Ep3. The concentration of Ep3 is 1 mol / L. Add 1.9 g of lithium aluminum hydride (38 g / mol) to 167 mL of ether to prepare a lithium aluminum hydride ether solution with a concentration of 0.3 mol / L. Cool the solution to -30°C. Add Ep dropwise to the lithium aluminum hydride ether solution. Heat to 30°C and react for 2 h. Use extraction-vacuum distillation technology to separate the product Pc3. The yield is 74%.

[0067] (4) 41 g of the product Pc3 (165 g / mol) obtained in step (3) and 0.8 g of benzenesulfonic acid (158 g / mol) were added to 410 g of benzene and heated under reflux for 1.5 h. The product Pd3 was separated by extraction-vacuum distillation technology. The yield was 81%.

[0068] (5) 18 g of the product Pd3 (147 g / mol) prepared in step (4) was dissolved in 144 g of tetrahydrofuran, cooled to -40°C, and 112 mL of a 2 mol / L butyl lithium hexane solution was added dropwise, and the mixture was stirred for 2 h at a reaction temperature of 30°C. Then 11.6 g of zirconium chloride (233 g / mol) was added, and the mixture was stirred for 30 h at a reaction temperature of 30°C to obtain a solution S.

[0069] (6) The solvent in the solution S3 obtained in step (4) was drained, 320 g of dichloromethane was added to dissolve, the solid-liquid separation was carried out, and the product CpM3 was obtained by distillation and concentration. The yield was 84%. The total yield of CpM3 was 31%.

[0070] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0071]

[0072] Among them, R1, R2, and R3 are CH 3 ; X is nitrogen; M is Zr; Z is Cl; m is 2.

[0073] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is N2C20ZrCl2H24, and the theoretical weight percentage composition is 6.17wt%N: 52.86wt%C: 20.04wt%Zr: 15.64wt%Cl: 5.29wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0074] Example 4

[0075] The preparation process of CpM4 of the present invention is the same as that of Example 1, except that acetyl chloride is used instead of propionyl chloride, and 2-methylpyrrole is used instead of 2,3-dimethylpyrrole. The total yield of CpM4 is 53%.

[0076] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0077]

[0078] Wherein, R1 and R3 are H; R2 is CH 3 ; X is nitrogen; M is Zr; Z is Cl; m is 2.

[0079] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is N2C16ZrCl2H16, and the theoretical weight percentage composition is 7.03wt%N:48.24wt%C:22.86wt%Zr:17.84wt%Cl:4.02wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0080] Example 5

[0081] The preparation process of CpM5 of the present invention is the same as that of Example 1, except that 2,3-dimethylthiophene is used instead of 2,3-dimethylpyrrole. The total yield of CpM5 is 56%.

[0082] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0083]

[0084] Among them, R1, R2, R3 are CH3; X is sulfur; M is Zr; Z is Cl; m is 2.

[0085] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is S2C20ZrCl2H24, and the theoretical weight percentage composition is 13.06wt%S: 48.98wt%C: 18.57wt%Zr: 14.49wt%Cl: 4.90wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0086] Example 6

[0087] The preparation process of CpM6 of the present invention is the same as that of Example 1, except that butyryl chloride is used instead of propionyl chloride, and 2,3-dimethylthiophene is used instead of 2,3-dimethylpyrrole. The total yield of CpM6 is 48%.

[0088] The obtained metallocene product was characterized by elemental analysis and had the following general structural formula:

[0089]

[0090] Where R1 is CH 3 HC 2 , R2, R3 are CH 3 ; X is sulfur; M is Zr; Z is Cl; m is 2.

[0091] The elemental composition of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is S2C22ZrCl2H28, and the theoretical weight percentage composition is 12.36wt%S: 50.97wt%C: 17.56wt%Zr: 13.71wt%Cl: 5.40wt%H. From the elemental analysis of Table 1, it can be seen that the elemental composition of the synthesized polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is consistent with the theoretical composition, indicating that a zirconium metallocene has been synthesized.

[0092] Table 1 Elemental analysis of metallocene

[0093]

[0094] Example 7

[0095] 4.68 g of metallocene CpM1 (468 g / mol) prepared in Example 1, 10.9 g [Ph(Me) 2 NH][B(C 6 F 5 ) 4 ] (1089 g / mol) and 39.6 g of tributyl aluminum (198 g / mol) were added to 497 g of alkylate oil and stirred evenly to obtain catalyst composition C1.

[0096] The molar ratio of the alkyl metal is 1:1:20, and the weight proportion of the solvent in the catalyst is 90%.

[0097] Example 8

[0098] 4.68 g of metallocene CpM1 (468 g / mol) prepared in Example 1, 14.1 g [Ph(Me) 2 NH][B(C 6 F 5 ) 4 ] (1089 g / mol) and 99 g of tributyl aluminum (198 g / mol) were added to 274 g of alkylate oil and stirred evenly to obtain catalyst composition C2.

[0099] The molar ratio of the alkyl metal is 1:1.3:50, and the weight proportion of the solvent in the catalyst is 70%.

[0100] Example 9

[0101] 4.68 g of metallocene CpM1 (468 g / mol) prepared in Example 1, 9.8 g [Ph(Me) 2 NH][B(C 6 F 5 ) 4] (1089 g / mol) and 198 g of tributyl aluminum (198 g / mol) were added to 850 g of alkylate oil and stirred evenly to obtain catalyst composition C3.

[0102] The molar ratio of the alkyl metal is 1: 0.9: 100, and the weight proportion of the solvent in the catalyst is 80%.

[0103] Example 10

[0104] The preparation process of the catalyst C4 of the present invention is the same as that of Example 7, except that the CpM4 prepared in Example 4 is used.

[0105] Embodiment 11

[0106] The preparation process of the catalyst C5 of the present invention is the same as that of Example 7, except that the CpM5 prepared in Example 5 is used.

[0107] Example 12

[0108] The preparation process of the catalyst C6 of the present invention is the same as that of Example 7, except that the CpM6 prepared in Example 6 is used.

[0109] Table 2 Molar composition of catalyst components

[0110]

[0111] Examples 13-16

[0112] The polymerization reaction of 1-decene is carried out in an autoclave equipped with electromagnetic stirring. Before the reaction, the autoclave is cleaned, heated in an oil bath at 140°C and evacuated to negative pressure, and maintained for 0.5 hours. High-purity nitrogen is filled into the autoclave, and then evacuated, and this is repeated three times. The reactor is cooled to the reaction temperature. Oil bath heating and stirring. The liquid 1-decene cylinder and the catalyst feed tank are connected to the metering pump respectively, and 1-decene and the catalyst are introduced into the autoclave through the metering pump. The reaction temperature is 70°C and the reaction time is 2 hours.

[0113] The specific process conditions and reaction results are shown in Table 3.

[0114] Table 3 Process conditions and results

[0115]

[0116] Comparative Example 1

[0117] The existing metallocene catalyst uses n-butylcyclopentadiene zirconium chloride metallocene and methylaluminoxane to catalyze the polymerization of butene. 4.06g of n-butylcyclopentadiene zirconium chloride metallocene and 58g of methylaluminoxane, as well as 14L 1-decene are added to the autoclave respectively, stirred and heated. The reaction conditions are pressure of 3MPa, temperature of 70℃, and time of 2 hours. The conversion rate of 1-decene is 59mol%, C 30 +C 40 +C 50 The overall selectivity was 42 wt%.

[0118] By comparing the catalyst of the present invention with the existing catalyst, it can be found that the activity and the total selectivity of C30+C40+C50 of the catalyst of the present invention are significantly better than those of the existing catalyst.

Claims

1. A heavy olefin oligomerization reaction, characterized in that: The method comprises the following steps: introducing a heavy olefin and an olefin polymerization catalyst into an autoclave, and carrying out a polymerization reaction under oligomerization reaction conditions; Wherein, the olefin polymerization catalyst contains a polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, and the general structural formula of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is shown as follows: , In the formula, X is -NH-, R1, R2, R3 are at least one of H, CH3, C2H5, M is Zr, Z is Cl, Br or I, and m is the valence state of M metal -2.

2. The heavy olefin oligomerization reaction according to claim 1, characterized in that: The synthesis method of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene comprises the following contents: (1) Add the substituted acid chloride and the substituted five-membered heterocycle to a solvent, stir evenly, cool to -40 to 0°C, then add a catalyst, stir and react for 10 to 24 hours; separate the reaction materials to obtain the product Pa; (2) adding the Pa product obtained in step (1) and hexamethylenetetramine to acetic anhydride, stirring and reacting for 24 to 48 hours at a reaction temperature of 80 to 100°C; adding alkali solution, stirring and reacting for 1 to 4 hours; separating the organic matter by extraction technology; then adding the extract and a strong acid catalyst to a solvent, stirring and reacting at a reaction temperature of room temperature to 50°C for a reaction time of 1 to 4 hours; separating to obtain the product Pb; (3) adding the product Pb obtained in step (2) to diethyl ether to prepare a solution Ep; adding lithium aluminum hydride to diethyl ether to prepare a lithium aluminum hydride diethyl ether solution Es; cooling the solution Es to -20 to -40°C; adding the solution Ep dropwise to the solution Es, heating to room temperature to 40°C, and reacting for 1 to 2 hours; separating and obtaining the product Pc; (4) adding the product Pc obtained in step (3) and a strong acid catalyst to a solvent, heating and refluxing for 0.5 to 2 hours, and obtaining the product Pd by separation; (5) dissolving the product Pd prepared in step (4) in a solvent, cooling to -40 to 0°C, adding alkyl lithium dropwise, stirring and reacting for 0.5 to 3 hours at a temperature of room temperature to 40°C; then adding chloride, stirring and reacting for 24 to 48 hours at a temperature of room temperature to 40°C, and obtaining a solution S; (6) draining the solvent from the solution S obtained in step (5), adding methyl chloride to dissolve, separating the solid and the liquid, and concentrating by distillation to obtain the product CpM; Wherein, the substituted acyl chloride structure is R1-CH2-CO-Cl, and the substituted five-membered heterocyclic structure is , R1, R2, R3 and X are as defined in claim 1.

3. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The substituted acyl chloride structure in step (1) is acetyl chloride, propionyl chloride or butyryl chloride.

4. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The solvent in step (1) is at least one of benzene, toluene, tetrahydrofuran, N,N-dimethylformamide and dimethyl sulfoxide.

5. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The catalyst in step (1) is anhydrous aluminum chloride or anhydrous tin chloride.

6. The heavy olefin oligomerization reaction according to claim 2, characterized in that: In step (1), the molar ratio of the substituted acid chloride, the substituted five-membered heterocycle and the catalyst is 1:(0.8-1.2):(0.01-0.1), and the weight ratio of the substituted five-membered heterocycle to the solvent is 1:(4-10).

7. The heavy olefin oligomerization reaction according to claim 2, characterized in that: In step (1), the reaction is stirred for 10 to 24 hours.

8. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The alkali solution in step (2) is an aqueous solution of alkali, the alkali is at least one of sodium hydroxide, sodium tert-butoxide, and sodium bicarbonate, and the strong acid catalyst is one of methanesulfonic acid, ethylsulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, hydrochloric acid, and sulfuric acid.

9. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The concentration of the alkali solution in step (2) is 1 to 4 mol / L.

10. The heavy olefin oligomerization reaction according to claim 2, characterized in that: In step (2), the molar ratio of Pa, hexamethylenetetramine and acetic anhydride is 1:(0.8-1.6):(1.2-2.0), the molar ratio of the base to the acetic anhydride is 1:(5-10), the molar ratio of the Pa product to the strong acid catalyst is 1:(0.1-0.5), and the weight ratio of the Pa product to the solvent is 1:(4-10).

11. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The concentration of the solution Ep prepared in step (3) is 1-3 mol / L, the concentration of the lithium aluminum hydride ether solution is 0.1-0.3 mol / L, and the molar ratio of the product Pb to lithium aluminum hydride is 1:(0.2-0.4).

12. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The strong acid catalyst in step (4) is methanesulfonic acid, ethylsulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, hydrochloric acid, or sulfuric acid, and the solvent is at least one of chloroform, carbon tetrachloride, benzene, and toluene.

13. The heavy olefin oligomerization reaction according to claim 2, characterized in that: In step (4), the molar ratio of Pc to the strong acid catalyst is 1:(0.02-0.05), and the weight ratio of Pc to the solvent is 1:(10-18).

14. The heavy olefin oligomerization reaction according to claim 2, characterized in that: The solvent in step (5) is one of diethyl ether and tetrahydrofuran, the molar ratio of Pd to alkyl lithium and zirconium chloride is 1:(1.8-2.4):(0.4-0.6), and the weight ratio of Pd to solvent is 1:(8-20).

15. The heavy olefin oligomerization reaction according to claim 2, characterized in that: In step (6), the weight ratio of S to methyl chloride is 1:(10-20), and the methyl chloride is one of dichloromethane, chloroform, and carbon tetrachloride.

16. The heavy olefin oligomerization reaction according to claim 1, characterized in that: The olefin polymerization catalyst comprises a polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, an organic boride, an alkyl metal and a solvent; the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene is a main catalyst, and the organic boride and the alkyl metal are co-catalysts; the molar ratio of the polysubstituted cyclopentadienyl five-membered heterocyclic metallocene, the organic boride and the alkyl metal is 1: (0.8-1.4): (10-500), and the weight proportion of the solvent in the catalyst is 70-90%.

17. The heavy olefin oligomerization reaction according to claim 16, characterized in that: The organic boron compound is selected from at least one of BF3, B(CF3)3, [MePhNH][B(CF3)3], [(Me)2PhNH][B(CF3)4], [R2NH][B(CF3)3], [R3N][B(CF3)3], [R3NH][B(CF3)4], [Ph3C][B(CF3)2], [NH3][B(CH3)3], [Ph(Me)2N][B(C6F5)3], [Ph(Me)2NH][B(C6F5)4], wherein R=C2-C 10 Ph is phenyl and Me is methyl.

18. The heavy olefin oligomerization reaction according to claim 17, characterized in that: The organic boron compound is selected from [(Me)2PhNH][B(CF3)4], [R3NH][B(CF3)4] or [Ph(Me)2NH][B(C6F5)4].

19. The heavy olefin oligomerization reaction according to claim 16, characterized in that: The alkyl metal is selected from at least one of alkyl magnesium, alkyl aluminum and alkyl zinc; the alkyl magnesium is selected from at least one of the group consisting of diethyl magnesium, dipropyl magnesium, diisopropyl magnesium and dibutyl magnesium; the alkyl aluminum is selected from at least one of the group consisting of trimethyl aluminum, triethyl aluminum, tripropyl aluminum, triisopropyl aluminum, tributyl aluminum and tri-tert-butyl aluminum; and the alkyl zinc is selected from at least one of diethyl zinc, dipropyl zinc, diisopropyl zinc, dibutyl zinc and di-tert-butyl zinc.

20. The heavy olefin oligomerization reaction according to claim 19, characterized in that: The alkyl metal is tributylaluminum and tri-tert-butylaluminum.

21. The heavy olefin oligomerization reaction according to claim 16, characterized in that: The solvent is selected from at least one of benzene, toluene, n-octane, n-decane and alkylate oil.

22. The heavy olefin oligomerization reaction according to claim 1, characterized in that: The conditions for the oligomerization reaction are: reaction temperature 40-100° C., and reaction time 1-8 hours.