A design method for all-solid waste foam lightweight filler

By using calcium carbide slag as an alkaline exciter, combined with the Sheffe secondary regression model and I-optimal design method, the problem of low operating risks and economic benefits of alkaline exciters in the prior art is solved, and the light foam is simplified The mix ratio design of mass fillers achieves effective control of flow value and compressive strength, saving material and time.

CN114743605BActive Publication Date: 2024-11-12SHANDONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210277977.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-21
Publication Date
2024-11-12
Estimated Expiration
2042-03-21

AI Technical Summary

Technical Problem

The prior art has operating risks, low economic benefits, high energy consumption when treating GGBS with alkaline exciters, and fails to affect mechanical or durable properties when changing the workingability of the slurry, resulting in the fluidity and pressure resistance of foam concrete. The strength is difficult to control and requires a lot of material and time to prepare and test.

Method used

Calcium slag is used as a green alkali excitation alternative material. By determining the volume ratio of calcium slag, water, granulated blast furnace slag and foam, using Sheffe quadratic regression model and I-optimal design method, the experiment was designed and performed, and the data was analyzed to establish Regression model of flow value and compressive strength simplifies mix design and saves material and time.

Benefits of technology

It realizes that while ensuring the workingability and compressive strength of the slurry, the mix ratio design process is simplified, manpower and material resources are saved, the accuracy of the regression results is ensured, and material loss and test cycle are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114743605B_ABST
    Figure CN114743605B_ABST
Patent Text Reader

Abstract

The present invention discloses a fully solid waste foam lightweight filler and a design method thereof. The present invention uses only two types of solid waste, namely granulated blast furnace slag and carbide slag; at the same time, the present invention uses two key values ​​of foam lightweight soil quality detection, namely flow value and compressive strength, as target parameters, and uses a statistical mixture design method to establish regression models of flow value and compressive strength respectively. The model proposed by the present invention can give the corresponding flow value and 3-day, 7-day, and 28-day compressive strength according to the material ratio parameters within a certain accuracy range, providing a specific numerical reference for the experimenter, thereby saving a lot of time and cost spent in mix design and mechanical property testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste utilization, and specifically relates to a design method for a fully solid waste foam lightweight filler. Background Art

[0002] Granulated blast furnace slag (GGBS) has similar hydration characteristics to cement, but because its self-hydration process is very slow and highly dependent on the material properties of GGBS, some alkaline hydroxides, soluble silicates or sulfates are usually required to accelerate the hydration of GGBS. Some commonly used alkaline activators (such as sodium hydroxide, water glass, etc.) have strong hygroscopicity and corrosiveness, which will increase the operating risks of material preparation personnel to a certain extent. At the same time, the use of such highly alkaline activators in the alkaline slag system has problems such as short coagulation time, low economic benefits, and high product energy consumption. Calcium carbide slag is a by-product of acetylene, polyvinyl chloride and polyvinyl alcohol produced by the hydrolysis reaction of calcium carbide (calcium carbide). The annual output is close to 500 tons and the overall utilization rate is less than 10%, resulting in waste of land resources and secondary pollution of the stacking environment. Calcium carbide slag is mainly composed of calcium hydroxide (content ≥80%), and the pH value is much lower than that of activators such as sodium hydroxide (pH <12.5). It can be used to make practical and safe alkaline solutions and has great potential to become a green alkali activating alternative material. For the alkali-activated system using carbide slag to activate GGBS, no admixture has been developed that can change the workability of the slurry without affecting other mechanical or durability properties. Therefore, the fluidity of foamed concrete in this system can only be controlled by adjusting the water-cement ratio or the mineral admixture ratio. While ensuring that the fresh slurry meets the workability requirements, different mineral admixture ratios and water-cement ratios will also change the defoaming rate, setting time, size and density of the foam soil, etc., and have a significant impact on the compressive strength of the hardened specimen. However, the process from preparing a mix ratio that meets the workability requirements to verifying the compressive strength of the specimens at a fixed curing age usually requires a lot of materials and time. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a design method for all-solid waste foam lightweight filler. The present invention proposes a simplified mix design method for the complicated steps of foam lightweight soil mix design, aiming to save material loss and test cycle during the adaptation process.

[0004] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0005] A design method for all-solid waste foam lightweight filler, characterized by comprising the following steps:

[0006] (1) Identify the factors in the mixture, define the factor boundary constraints, and determine the key characteristics and target response of the product: and select appropriate statistical algorithms;

[0007] The factors in the mixture are determined by volume ratio of carbide slag, water, granulated blast furnace slag and foam;

[0008] (2) Design and implementation: First, carbide slag, water, granulated blast furnace slag and foam are mixed according to different volume ratios to obtain a pure slurry; a foaming agent and water are mixed and foamed under high pressure to obtain foam; foam is added to the pure slurry to obtain a slurry; before the specimen is poured, the wet density and flow value of the slurry are tested; after pouring, the 7d compressive strength and 28d compressive strength of the slurry are tested; through the test, the flow value, 7d compressive strength and 28d compressive strength of the slurry under different volume ratios of carbide slag, water, granulated blast furnace slag and foam are obtained;

[0009] (3) Analyze data and evaluate model: By analyzing the data, the regression model of flow value, 7d and 28d compressive strength is obtained; and the value recommendations of each parameter are given according to different wet densities;

[0010] (4) According to the parameter value recommendations given in step (3), the mix parameters are initially proposed; the laboratory mix ratio is obtained through flow value test and strength test;

[0011] (5) After determining the laboratory mix ratio, convert it into the construction mix ratio based on the moisture content of the materials at the construction site.

[0012] Furthermore, the factors in the mixture are granulated blast furnace slag, carbide slag, water and foam; to ensure the rationality of the experiment, the mass of carbide slag is limited to 5-30% of the solid mass, and the water-cement mass ratio is 0.5-0.8; before entering the model, the parameters of each component should be converted into the percentage of the component in the total volume according to its actual density.

[0013] Furthermore, the key characteristics and target response quantities of the product are determined as follows: the flow value of the fresh slurry is controlled to meet the flow value control range of 160-190mm recommended by the "Technical Code for Bubble Mixed Lightweight Soil Filling Engineering" (TJG F10-01-2011), and the 7d and 28d compressive strengths meet the engineering strength requirements.

[0014] Furthermore, the Sheffe quadratic regression model and the I-optimal design method were selected, and Design Expert 13.0 was used for model design, testing, and residual analysis.

[0015]

[0016] Furthermore, the foaming agent is a protein anion composite foaming agent; and the foaming liquid is prepared at a mass ratio of foaming agent: water = 1:49.

[0017] Furthermore, the specific steps for preparing the slurry are: first, mix the carbide slag with water, stir at a low speed of 145±5rm for 30s, then add the mineral powder, stir at a low speed for 60s, and then stir at a high speed of 285±10rm for 60s; prepare the foaming liquid, and mix the compressed air with the foaming liquid in a foaming machine; after preparing the net slurry, add the weighed foam in batches, and stir at a low speed until there is no white foam on the surface and the slurry is uniform.

[0018] Furthermore, in order to prevent the foam structure from being destroyed during the stirring process, a hand-held stirrer equipped with a cross-shaped stirring rod was selected.

[0019] Furthermore, the conditions for testing the 7d and 28d compressive strength are as follows: prepare 100mm×100mm×100mm specimens, form 6 specimens for each operation, and place them at 20±1℃ and relative humidity greater than 90% for curing until demolding, wherein the group mixed with carbide slag is demolded after curing for 48h, and the group containing only mineral powder is demolded after curing until the specimen hardens; the specimens after demolding are placed in plastic sealed bags and cured at 20±1℃ to the age; the compressive strength test follows GB / T 11969-2008, for the formed specimens, three standard specimens are taken from each group at each age, and the 7d and 28d compressive strength are tested.

[0020] Further, in step (4), according to the parameter value suggestions given in step (3), the mix parameters are initially proposed; each parameter is brought into the regression model in step (3) to obtain the flow value and 7d, 28d compressive strength values ​​under the mix ratio; when the flow value and 7d, 28d compressive strength values ​​meet the requirements, the preliminary mix ratio is obtained; if not, the mix parameters are adjusted until they meet the requirements; the preliminary mix ratio obtained in the above steps is tested for flow value, and if it meets the requirements, the benchmark mix ratio can be obtained; if not, the preliminary mix ratio is adjusted until the flow value meets the specification requirements and the benchmark mix ratio is obtained; strength test adjustment is performed on the basis of the benchmark mix ratio, and if it meets the requirements, the laboratory mix ratio is determined, and if not, the calcium carbide slag content is adjusted and the above steps are repeated until the strength requirements are met;

[0021] The requirements are whether the flow value meets the recommended range of 160-190mm in the "Technical Code for Bubble Mixed Light Soil Filling Engineering" (TJG F10-01-2011), and whether the compressive strength meets the engineering strength requirements.

[0022] Furthermore, in step (7), the amount of each material used should be:

[0023] m' GBS =m GBS

[0024] m' CS =m CS

[0025] m' w =m w -(m GBS a+m CS b)

[0026] m' f =m f

[0027] Among them, m` GBS is the mass of granulated blast furnace slag at the construction site; m` CS is the mass of tourmaline slag at the construction site; m` w is the quality of water in the construction site; m` f is the mass of foam at the construction site; m GBS is the mass of laboratory granulated blast furnace slag; m CS is the mass of tourmaline slag in the laboratory; m w is the quality of laboratory water; m f is the mass of the foam in the test room; m GBS a is the moisture content of granulated blast furnace slag at the construction site, m CS b is the moisture content of carbide slag at the construction site.

[0028] The present invention uses only two types of solid waste, namely granulated blast furnace slag and carbide slag. The flow value is the primary control index of the workability of the fresh foam soil slurry. In the mixing process of foam lightweight soil based on the cement system, the flow value can be controlled within the range that meets the standard by adding admixtures. However, for alkali-activated cementitious material systems, no admixtures have been developed that can change the workability of the slurry without affecting other mechanical or durability properties. Therefore, the control of alkali-activated system foam concrete can only be achieved by adjusting the water-cement ratio or the mineral admixture ratio. This process usually consumes a lot of materials and time, and it is necessary to ensure that the sample reaches the minimum strength requirement required for the project after standard curing.

[0029] Mixture Design focuses on exploring the impact of changes in the components of the target mixture on the overall experimental observation value. It allows the inclusion of two or more factors, characterizes the different components in the mixture with relative content (assuming that the measured response value is only affected by the relative content of the factor and has nothing to do with the absolute number), and fits the mathematical equation of the correlation between the components. In the foam concrete system, the actual amount of foam added is usually affected by the fluidity of the slurry, mixing time, and setting time of the foam soil. Mixture design requires that the sum of each component remains at a fixed value, that is, the factor parameter value cannot be changed independently, the proportion of each mixture is between 0-1, and the total amount must be 100%. Therefore, when using wet density as the target value, using the proportion of material per unit volume as the factor for equation regression can better ensure the accuracy of the regression results.

[0030] In order to simplify the mix proportion trial preparation steps and save manpower and material resources consumed in the process of mix proportion adjustment, the present invention uses the two key values ​​of foam lightweight soil quality detection - flow value and compressive strength as target parameters, and uses the statistical mixture design method to establish regression models of flow value and compressive strength respectively. The model proposed in this study can give the corresponding flow value and 3-day, 7-day, and 28-day compressive strength according to the material ratio parameters within a certain accuracy range, providing the experimenters with a specific numerical reference, thereby saving a lot of time and cost spent in mix proportion design and mechanical property testing.

[0031] Beneficial effects of the present invention: The design method provided by the present invention uses flow value and compressive strength as target parameters, saving manpower and material resources consumed in the process of adjusting the mix ratio. At the same time, when wet density is used as the target value, using the material proportion per unit volume as the factor of the equation regression can better ensure the accuracy of the regression result. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0033] Figure 1 The present invention is designed as a method flow chart.

[0034] Figure 2 It is the particle size distribution curve of granulated blast furnace slag.

[0035] Figure 3 is the particle size distribution curve of carbide slag. DETAILED DESCRIPTION

[0036] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0037] The purpose of the present invention can be achieved by the following technical solutions:

[0038] (1) First, it is necessary to identify the factors in the mixture, define the boundary constraints of the factors, and determine the key characteristics and target response of the product:

[0039] The solid cementitious materials used in the design method of pure solid waste foam lightweight soil mix ratio based on mixture design only include precursor mineral powder and carbide slag; in addition, the system also includes two substances, water and foam, for a total of four factors;

[0040] To ensure the rationality of the experiment, the carbide slag content is limited to 5-30% of the solid mass, and the water-cement mass ratio is 0.5-0.8; before entering the model, the parameters of each component should be converted into the percentage of the component in the total volume according to its actual density;

[0041] The purpose of creating this method is to control the flow value of the fresh slurry to meet the flow value control range of 160-190mm recommended by the "Technical Code for Bubble Mixed Lightweight Soil Filling Engineering" (TJG F10-01-2011), and the 7d and 28d compressive strengths meet the engineering strength requirements;

[0042] At the same time, it is necessary to select appropriate statistical algorithms: Sheffe quadratic regression model, I-optimal design method, and Design Expert 13.0 for model design, testing, and residual analysis;

[0043]

[0044] (2) Design and execution: The total number of experimental runs was 18 times, and the experiments were carried out in the order shown in Table 1: The foamed lightweight soil was prepared by the pre-foaming method. In order to prevent the foam structure from being damaged during the mixing process, a hand-held mixer equipped with a cross-shaped stirring rod was selected; first, the calcium carbide slag was mixed with water, and stirred at a low speed of 145±5rm for 30s, then the mineral powder was added, stirred at a low speed for 60s, and then stirred at a high speed of 285±10rm for 60s; the protein anion composite foaming agent was used in the experiment, which was produced by Shandong Chilong Building Energy Saving Technology Co., Ltd.; the foaming liquid was prepared with a mass ratio of foaming agent: water = 1:49, and compressed air was mixed with the foaming liquid in the foaming machine. The foam density produced was 40kg / m 3 ; After the preparation of the pure slurry is completed, add the weighed foam in batches, stir and mix at a low speed until there is no white foam on the surface and the slurry is uniform; before casting the specimens, test the wet density and flow value of the slurry. Prepare 100mm×100mm×100mm specimens, form 12 specimens for each run, place them at 20±1℃, and relative humidity greater than 90% for curing until demolding. The group mixed with carbide slag is demolded after curing for 48h, and the group containing only mineral powder is demolded after curing until the specimen hardens; the demolded specimens are placed in plastic sealed bags and cured at 20±1℃ until the age; the compressive strength test follows GB / T 11969-2008. For the molded specimens, three standard specimens are taken from each group at each age to test the 7d and 28d compressive strength; the mix proportions and experimental measurement values ​​of each group are shown in Table 1;

[0045] Table 1 Test run times and response values

[0046]

[0047]

[0048] (3) Analyze data and evaluate models: The regression models of flow value, 7d and 28d compressive strength are shown in Equations 1-3. The models are tested by variance analysis, goodness of fit and residual test to ensure that the models are accurate within the 95% prediction interval.

[0049] Spreadability (mm)=-5.47(V%GBS)+75.72(V%CS)+7.35(V%Water)+1.46(V%Foam)-2.72(V%GBS)(V%CS)-0.97(V%CS)(V%Foam)

[0050] ln(Y7+0.002315)(MPa)=-0.1263(V%GBS)-28.0017(V%CS)-0.018605(V%Water)-0.06 10(V%Foam)+0.4366(V%GBS)(V%CS)+0.2853(V%CS)(V%Water)+0.2929(V%CS)(V%Foam)

[0051]

[0052] Wherein, (V%GBS) represents the volume of granulated blast furnace slag;

[0053] (V%CS) represents the volume of carbide slag;

[0054] (V% Water) represents the volume of water;

[0055] (V% Foam) represents the volume of foam;

[0056] Recommendations for the values ​​of various parameters are given according to different wet densities, as shown in Table 2:

[0057] Table 2 Recommended parameter values ​​at different wet densities

[0058]

[0059] (4) According to the parameter value suggestions given in step (3), the initial mix ratio parameters (expressed as volume ratio, the sum of all parameters is always 100%) are proposed; each parameter is substituted into the regression model in step (3) to obtain the flow value and 7d and 28d compressive strength values ​​under the mix ratio; when the flow value and 7d and 28d compressive strength values ​​meet the requirements, the preliminary mix ratio is obtained; if not, the mix ratio parameters are modified until they meet the requirements; whether the flow value meets the recommended range of 160-190 mm in the Technical Code for Bubble Mixed Lightweight Soil Filling Engineering (TJGF10-01-2011) and whether the compressive strength meets the engineering strength requirements;

[0060] (5) The preliminary mix ratio obtained by the above steps is tested for flow value. If it meets the requirements, the benchmark mix ratio can be obtained. If it does not meet the requirements, the preliminary mix ratio is corrected by the water-cement ratio ± 0.05. When the flow value is low, the water-cement ratio is increased by 0.05, and when the flow value is high, the water-cement ratio is reduced by 0.05 until the flow value meets the requirements of the specification and the benchmark mix ratio is obtained.

[0061] (6) Perform strength test adjustment based on the benchmark mix ratio. Three different mix ratios are used, one of which is the benchmark mix ratio, and the other two groups keep the same water-cement ratio. The carbide slag content (mass fraction) based on the benchmark mix ratio is increased and decreased by 5% respectively. Three standard samples in each group are subjected to compressive strength test after curing for 28 days to check whether they meet the engineering requirements. If they meet the requirements, the laboratory mix ratio is determined. If not, the carbide slag content is adjusted again and the above steps are repeated.

[0062] (7) After determining the laboratory mix ratio, convert it according to the moisture content of the materials on the construction site to obtain the construction mix ratio. The weighing amount of each material should be

[0063] m' GBS =m GBS

[0064] m' CS =m CS

[0065] m' w =m w -(m GBS a+m CS b)

[0066] m' f =m f

[0067] Among them, m` GBS is the mass of granulated blast furnace slag at the construction site; m` CS is the mass of tourmaline slag at the construction site; m` w is the quality of water in the construction site; m` f is the mass of foam at the construction site; m GBS is the mass of laboratory granulated blast furnace slag; m CS is the mass of tourmaline slag in the laboratory; m w is the quality of laboratory water; m f is the mass of the foam in the test room; m GBS a is the moisture content of granulated blast furnace slag at the construction site, m CS b is the moisture content of carbide slag at the construction site.

[0068] Example 1

[0069] The granulated blast furnace slag and carbide slag used in the examples are conventional materials and can be purchased commercially.

[0070] The granulated blast furnace slag used in the examples has an activity of S85, a density of 2900 kg / m3, and a particle size distribution of Figure 1 As shown; the carbide slag used was vacuum dried, ground, and passed through a 300μm sieve, with a density of 2185kg / m3 and a particle size distribution as shown Figure 2 As shown in the figure, the protein anion composite foaming agent used is produced by Shandong Chilong Building Energy Saving Technology Co., Ltd. The dilution ratio is 1:49, and the output foam density is 40-50kg / m 3 .

[0071] (1) According to the parameter recommendations given above, the initial mix ratio parameters are determined, using a water-cement ratio of 0.65 and a carbide slag mass content of 15% (converted to volume parameters: granulated blast furnace slag content 12.02%, carbide slag content 2.82%, water content 26.65%, and foam content 58.51%);

[0072] (2) Substituting the parameters in (1) into the regression model, the flow value under this ratio is calculated to be 177 mm, the 7d compressive strength value is 1.0 MPa, and the 28d compressive strength value is 3.7 MPa;

[0073] (3) According to the flow value range of 160-200 mm specified in the Technical Specification for Bubble Mixed Lightweight Soil Filling Engineering (TJG F10-01-2011), the flow value of 177 mm calculated in step (2) meets the requirements of the specification, and the compressive strength value meets the engineering requirements of 7d>0.4MPa and 28d>0.8MPa;

[0074] (4) As verified by (3), the flow value, 7d and 28d compressive strength under this mix ratio all meet the requirements of the Technical Specification for Bubble Mixed Lightweight Soil Filling Engineering (TJG F10-01-2011). The granulated blast furnace slag content is 12.7%, the calcium carbide slag content is 1.9%, the water content is 26.7%, and the foam content is 58.7%, which is the initial mix ratio of this example (expressed in volume ratio).

[0075] (5) The preliminary mix ratio obtained in the above steps is 12.7% of mineral powder, 1.9% of calcium carbide slag, 26.7% of water, and 58.7% of foam, and the flow value is tested by trial mixing. With reference to the flow value test method in the Technical Specification for Bubble Mixed Lightweight Soil Filling Engineering (TJG F10-01-2011), the flow value under this mix ratio is 166 mm, which meets the requirements of the specification, and the benchmark mix ratio of this example is obtained;

[0076] (6) Perform strength test adjustment on the basis of the benchmark mix ratio. Use the experimental procedure of step (5) and adopt three groups of different mix ratios, one of which is the benchmark mix ratio, and the other two groups keep the same water-cement ratio. The carbide slag content (mass fraction) based on the benchmark mix ratio is increased and decreased by 5% respectively, that is, the carbide slag content is 5%, 10%, and 15% respectively. The specific mix ratio parameters are shown in Table 3; each group of three standard samples is subjected to compressive strength test after curing for 28 days. The test results are shown in Table 4. After inspection, the compressive strength at 28 days is higher than 0.8 MPa. Based on cost considerations, the 20% content group is selected to determine the laboratory mix ratio;

[0077] Table 3 Mix ratio under different carbide slag dosage

[0078]

[0079] Table 4 28d compressive strength test results

[0080] Carbide slag content (%) 28d compressive strength (MPa) 10 3.1 15 2.3 20 2.2

[0081] (7) After determining the laboratory mix ratio, convert it into the construction mix ratio based on the moisture content of the materials at the construction site.

[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A design method for all-solid waste foam lightweight filler, characterized in that: The steps include: (1) Identify the factors in the mixture, define the factor boundary constraints, and determine the key characteristics and target response of the product: and select appropriate statistical algorithms; The factors in the mixture are determined by volume ratio of carbide slag, water, granulated blast furnace slag and foam; (2) Design and implementation: First, carbide slag, water, granulated blast furnace slag and foam are mixed according to different volume ratios to obtain a pure slurry; a foaming agent and water are used to prepare foam; foam is added to the pure slurry to obtain a slurry; before casting the specimen, the wet density and flow value of the slurry are tested; after casting, the 7d compressive strength and 28d compressive strength of the slurry are tested; through the test, the flow value, 7d compressive strength and 28d compressive strength of the slurry under different volume ratios of carbide slag, water, granulated blast furnace slag and foam are obtained; (3) Analyze data and evaluate model: By analyzing the data, the regression model of flow value, 7d and 28d compressive strength is obtained; and the value recommendations of each parameter are given according to different wet densities; (4) According to the parameter value recommendations given in step (3), the mix parameters are initially proposed; the laboratory mix ratio is obtained through flow value test and strength test; (5) After determining the laboratory mix ratio, convert it into the construction mix ratio based on the moisture content of the materials at the construction site.

2. The design method according to claim 1, characterized in that: To ensure the rationality of the experiment, the mass of carbide slag is limited to 0-30% of the solid mass, and the water-cement mass ratio is 0.5-0.8; before entering the model, the parameters of each component should be converted into the percentage of the component in the total volume according to its actual density.

3. The design method according to claim 1, characterized in that: The key characteristics and target response quantities of the product are determined as follows: the flow value of the fresh slurry is controlled to meet the flow value control range of 160-190mm recommended by the "Technical Code for Bubble Mixed Lightweight Soil Filling Engineering" (TJG F10-01-2011), and the 7d and 28d compressive strengths meet the engineering strength requirements.

4. The design method according to claim 1, characterized in that: The Sheffe quadratic regression model and I-optimal design method were used, and Design Expert 13.0 was used for model design, testing, and residual analysis.

5. The design method according to claim 1, characterized in that: The foaming agent is a protein anion composite foaming agent; the foaming liquid is prepared with a mass ratio of foaming agent: water = 1:

49.

6. The design method according to claim 1, characterized in that: The specific steps for preparing the slurry are: first, mix carbide slag with water, stir at a low speed of 145±5rm for 30s, then add mineral powder, stir at a low speed for 60s and then stir at a high speed of 285±10rm for 60s; prepare the foaming liquid, and mix the compressed air with the foaming liquid in a foaming machine; after preparing the net slurry, add the weighed foam in batches, and stir at a low speed until there is no white foam on the surface and the slurry is uniform.

7. The design method according to claim 6, characterized in that: To prevent the foam structure from being destroyed during the stirring process, choose a handheld mixer equipped with a cross-shaped stirring rod.

8. The design method according to claim 1, characterized in that: In step (2), the conditions for testing the 7d and 28d compressive strength are as follows: prepare a 100mm×100mm×100mm sample, form 12 test pieces for each operation, place them at 20±1°C and a relative humidity greater than 90% for curing until demolding, wherein the group mixed with carbide slag is demolded after curing for 48h, and the group containing only mineral powder is demolded after curing until the test piece hardens; the demolded test pieces are placed in a plastic sealed bag and cured at 20±1°C until the age; the compressive strength test follows GB / T 11969-2008, and for the formed samples, three standard samples are taken from each group at each age to test the 7d and 28d compressive strength.

9. The design method according to claim 1, characterized in that: In step (4), according to the parameter value suggestions given in step (3), the mix ratio parameters are initially proposed; each parameter is substituted into the regression model in step (3) to obtain the flow value and the 7d and 28d compressive strength values ​​under the mix ratio; when the flow value and the 7d and 28d compressive strength values ​​meet the requirements, the preliminary mix ratio is obtained; if not, the mix ratio parameters are adjusted until they meet the requirements; The preliminary mix ratio obtained by the above steps is tested for flow value. If it meets the requirements, the benchmark mix ratio can be obtained. If it does not meet the requirements, the preliminary mix ratio is adjusted until the flow value meets the specification requirements and the benchmark mix ratio is obtained. The strength test is adjusted on the basis of the benchmark mix ratio. If it meets the requirements, the laboratory mix ratio is determined. If it does not meet the requirements, the amount of calcium carbide slag is adjusted and the above steps are repeated until the strength requirements are met. The requirements are whether the flow value meets the recommended range of 160-190mm in the "Technical Code for Bubble Mixed Light Soil Filling Engineering" (TJG F10-01-2011), and whether the compressive strength meets the engineering strength requirements.

10. The design method according to claim 1, characterized in that: In step (5), the amount of each material should be: m' GBS =m GBS m' CS =m CS m' w =m w -(m GBS a+m CS b) m' f =m f Among them, m` GBS is the mass of granulated blast furnace slag at the construction site; m` CS is the mass of tourmaline slag at the construction site; m` w is the quality of water in the construction site; m` f is the mass of foam at the construction site; m GBS is the mass of laboratory granulated blast furnace slag; m CS is the mass of tourmaline slag in the laboratory; m w is the quality of laboratory water; m f is the mass of the foam in the test room; m GBS a is the moisture content of granulated blast furnace slag at the construction site, m CS b is the moisture content of carbide slag at the construction site.

Citation Information

Patent Citations

  • A Method For Preparing The Fast-Hardening Early-Strength High-Performance All-Solid Waste Concrete

    AU2020101143A4

  • Novel energy-saving environmentally-friendly foam light soil used for subgrade and road beds and preparation method of foam light soil

    CN110002897A

  • All-solid-waste underground filling cementing material for high-sulfur tailings and preparation method of all-solid-waste underground filling cementing material

    CN112429986A

  • All-solid-waste foam concrete and preparation method thereof

    CN112811858A

  • Granulated Blast-furnace Slag Activator, Its Manufacturing Method Thereof, and Manufacturing Method of Cement

    US20200299194A1