Molecular polar substance adsorption carbon
The activated carbon prepared by the alkali activation method solves the problem of insufficient adsorption performance of activated carbon in the liquid phase and gas phase in the existing technology, achieves efficient adsorption and regeneration, and significantly improves the adsorption performance and removal efficiency of molecular polar substances.
Patent Information
- Application Number
- CN202080080875.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-30
AI Technical Summary
After the existing activated carbon has been modified for adsorption performance, it is difficult to show excellent performance in both the liquid phase and the gas phase. Moreover, washing after adsorption causes the agent to be lost and cannot be reused.
Prepare activated carbon through alkali activation method to increase its specific surface area and acidic functional group amount, ensure that the acidic functional group amount is above 2.1meq/g and the basic functional group amount is below 0.6meq/g, and form a high active surface area in the pores to avoid impregnation Agent to achieve excellent adsorption performance and regeneration of molecular polar substances.
It achieves efficient adsorption performance for molecular polar substances in the gas phase and liquid phase, and retains acidic functional groups after washing to ensure the regeneration ability of activated carbon, significantly improving the adsorption performance and removal efficiency.
Smart Images

Figure CN114746175B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to molecular polar substance adsorption carbon, in particular to activated carbon with excellent adsorption performance for molecular polar substances. Background Art
[0002] Activated carbon with a high specific surface area is widely used as an adsorbent material. For example, activated carbon is used to remove odor-causing substances such as ammonia or chloramine from liquids or gases. In recent years, technologies for modifying activated carbon have been proposed to improve the adsorption performance of specific adsorbates.
[0003] For example, Patent Document 1 proposes activated carbon having phosphoric acid impregnated in its pores as activated carbon having improved adsorption performance for ammonia in a gas phase. This activated carbon can chemically adsorb ammonia on phosphoric acid, and therefore exhibits excellent adsorption performance for ammonia.
[0004] In addition, Patent Document 2 proposes an activated carbon having a specific surface area of 500 to 900 m 2 The activated carbon has a total acidic functional group content of about 1.0 to 2.4 milliequivalents / g and an acidic functional group content derived from carboxylic acid of about 0.2 to 0.9 milliequivalents / g. The activated carbon has excellent adsorption performance for trace metals in the liquid phase due to the increased acidic functional group content.
[0005] In addition, Patent Document 3 proposes controlling the amount of surface oxides (0.35 meq / g or more) and the BET specific surface area (900 to 2020 m 2 / g) of activated carbon. The activated carbon has the ability to chemically adsorb polar substances and the adsorption capacity derived from the pores of the activated carbon.
[0006] Prior art documents
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Publication No. 2002-159852
[0009] Patent Document 2: Japanese Patent Publication No. 2004-315243
[0010] Patent Document 3: Japanese Patent Publication No. 2019-098324 Summary of the invention
[0011] Activated carbon itself can be used in either liquid or gas phases, but when the adsorption performance is modified, it is modified according to the use environment. For example, as in Patent Document 1, activated carbon impregnated with agents such as phosphoric acid is suitable for removing ammonia and the like in the gas phase, but since the impregnated agent will be lost, it cannot be used in the liquid phase. Generally, if the activated carbon carrying the agent is washed after adsorption of the adsorbate, the agent will be lost, so it cannot be reused. In addition, as in Patent Document 2, activated carbon that suppresses the specific surface area to a low level and increases the amount of acidic functional groups is suitable for metal adsorption in the liquid phase, but the adsorption amount is low and does not have sufficient adsorption performance. The activated carbon of Patent Document 3 does not have a sufficient adsorption rate for chloramine, for example.
[0012] The present invention has been made in view of the above-mentioned situation, and an object of the present invention is to provide a molecular adsorption activated carbon which has excellent adsorption performance for molecular polar substances and can be regenerated.
[0013] The present invention that solves the above-mentioned problems has the following constitution: [1] A molecular polar substance adsorption carbon obtained by an alkali activation method, wherein the amount of acidic functional groups is 2.1 meq / g or more, the amount of basic functional groups is greater than 0 and is less than 0.6 meq / g, and the specific surface area is 1000 to 4000 m 2 / g.
[0014] [2] The molecular polar substance adsorbing carbon according to [1], wherein the total amount of hydroxyl groups and carboxyl groups contained in the acidic functional groups is 0.6 meq / g or more, which is also a preferred embodiment.
[0015] [3] The molecular polar substance adsorbing carbon according to [1] or [2], wherein the ratio of the amount of the acidic functional groups to the total amount of the acidic functional groups and the amount of the basic functional groups is 70% or more, which is also a preferred embodiment.
[0016] [4] The molecular polar substance adsorbing carbon according to any one of [1] to [3], wherein the amount of acidic functional groups per unit specific surface area of the polar substance adsorbing carbon is 0.7 μeq / m 2 The above are also preferred embodiments.
[0017] [5] The molecular polar substance adsorbing carbon according to any one of [1] to [4], wherein the polar substance adsorbing carbon has no chemical impregnated in its pores, which is also a preferred embodiment.
[0018] [6] The molecular polar substance adsorbing carbon according to any one of [1] to [5], wherein the active surface area of the polar substance adsorbing carbon is 180 m 2 / g or more is also a preferred embodiment.
[0019] The molecular polar substance adsorbing carbon of the present invention has a high specific surface area and a large amount of acidic functional groups, so it has excellent adsorption performance for molecular polar substances. In addition, the molecular polar substance adsorbing carbon of the present invention allows the acidic functional groups to adsorb molecular polar substances, and even if it is subjected to regeneration treatment such as washing, the acidic functional groups remain, so it can be reused as an adsorbent material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The ammonia adsorption amount of the activated carbon in the examples is shown.
[0021] Figure 2 The relationship between the amount of acidic functional groups and the amount of ammonia adsorption of the activated carbon of the examples is shown.
[0022] Figure 3 The relationship between the amount of OH groups and the amount of ammonia adsorption of the activated carbon of the Examples is shown.
[0023] Figure 4 The relationship between the COOH group content and the ammonia adsorption amount of the activated carbon of the examples is shown.
[0024] Figure 5 The relationship between the acidic functional group ratio and the ammonia adsorption amount of the activated carbon of the examples is shown.
[0025] Figure 6 The relationship between the amount of acidic functional groups per unit specific surface area and the amount of ammonia adsorption of the activated carbon of the examples is shown.
[0026] Figure 7 The relationship between the amount of basic functional groups and the amount of ammonia adsorption of the activated carbon of the Examples is shown.
[0027] Figure 8 The relationship between the specific surface area of the activated carbon and the amount of chloramine removed in the examples is shown.
[0028] Fig. 9 The relationship between the amount of acidic functional groups in the activated carbon of the examples and the amount of chloramine removed is shown.
[0029] Fig.10 The relationship between the amount of basic functional groups in the activated carbon of the examples and the amount of chloramine removed is shown.
[0030] Fig.11 The relationship between the active surface area of the activated carbon and the chloramine removal amount in the examples is shown.
[0031] Fig.12 The relationship between the specific surface area of the activated carbon and the chloramine removal rate in the examples is shown.
[0032] Fig.13 The relationship between the amount of acidic functional groups in the activated carbon of the examples and the chloramine removal rate is shown.
[0033] Fig.14 The relationship between the amount of basic functional groups in the activated carbon of the examples and the chloramine removal rate is shown.
[0034] Fig.15 The relationship between the active surface area of the activated carbon of the examples and the chloramine removal rate is shown.
[0035] Fig.16 The relationship between the chloramine removal rate and the chloramine removal amount in the examples is shown. DETAILED DESCRIPTION
[0036] The inventors of the present invention have repeatedly conducted in-depth research with the purpose of providing an activated carbon that not only improves the adsorption performance of molecular polar substances but also can be regenerated. First, the activated carbon with an increased specific surface area was brought into contact with an ammonia-containing gas, but the ammonia adsorption performance was low. In addition, even if the amount of acidic functional groups is increased as in Patent Document 2, if the specific surface area of the activated carbon is small, the ammonia adsorption performance is also low. In order to improve the adsorption performance of molecular polar substances, the inventors of the present invention believe that it is effective to increase the specific surface area to increase the adsorption amount and to increase the edge surface of the activated carbon to increase the amount of acidic functional groups. However, when the specific surface area is increased, the amount of acidic functional groups will decrease, and it is difficult to increase both at the same time. Therefore, the inventors of the present invention have once again studied the preparation conditions of activated carbon, and found that by optimizing the activation conditions by using different preparation conditions from the past, such as alkaline activation treatment at low temperature, it is possible to provide an activated carbon with both increased specific surface area and acidic functional group amount, which is most suitable for adsorbing molecular polar substances, thereby completing the present invention.
[0037] In the present invention, the adsorption performance of activated carbon refers to the adsorption amount and / or adsorption rate of molecular polar substances present in the gas phase and / or liquid phase.
[0038] In addition, various physical properties of activated carbon were measured according to the measurement methods described in Examples unless otherwise specified.
[0039] The molecular polar substance adsorption carbon of the present invention is an activated carbon obtained by an alkaline activation method, wherein the amount of acidic functional groups is 2.1 meq / g or more, the amount of basic functional groups is greater than 0 and is less than 0.6 meq / g, and the specific surface area is 1000 to 4000 m 2 / g.
[0040] (Molecular polar substance adsorption carbon)
[0041] In the present invention, molecular polar substance adsorption carbon refers to activated carbon having the adsorption capacity of molecular polar substances. Molecular polar substances refer to substances whose molecules have electrical polarity, including compounds having polar groups such as amino, halogen, hydroxyl, carboxyl, nitro, formyl, alkoxy, ester, and nitrile. Specifically, malodorous components such as trimethylamine, hydrogen sulfide, ammonia, and methyl mercaptan; volatile organic compounds (VOCs) such as formaldehyde, toluene, xylene, ethylbenzene, styrene, and acetaldehyde; and disinfectants for tap water such as chloramine and hypochlorous acid can be exemplified.
[0042] (Specific surface area)
[0043] The specific surface area of the molecular polar substance adsorbed carbon of the present invention is 1000 to 4000 m 2 / g. If the specific surface area is increased, the amount of adsorption of molecular polar substances can be increased, and the edge surface in the pores increases, which can improve the adsorption performance. On the other hand, if the specific surface area is too large, the amount of acidic functional groups decreases, and the adsorption force of molecular polar substances in the pores decreases. The specific surface area of carbon for molecular polar substance adsorption is preferably 1250m 2 / g or more, more preferably 1500m 2 / g or more, more preferably 1700m 2 / g or more, most preferably 1800m 2 / g or more, preferably 3800m 2 / g or less, more preferably 3500m 2 / g or less, more preferably 3000m 2 / g or less, and most preferably 2500m 2 / g or less.
[0044] (acidic functional group amount)
[0045] The amount of acidic functional groups of the molecular polar substance adsorption carbon of the present invention is 2.1 meq / g or more. In the above-mentioned specific surface area, if the acidic functional groups are increased, the adsorption performance of molecular polar substances can be improved. The amount of acidic functional groups is preferably 2.3 meq / g or more, more preferably 2.5 meq / g or more, and further preferably 2.7 meq / g or more. The upper limit is not particularly limited, preferably 10.0 meq / g or less, more preferably 7.0 meq / g or less, and further preferably 5.0 meq / g or less.
[0046] (Basic functional group amount)
[0047] The amount of basic functional groups of the molecular polar substance adsorption carbon of the present invention is greater than 0 and is less than 0.6 meq / g. If the basic functional groups are too many, the acidic functional groups are reduced, and the adsorption performance for molecular polar substances is reduced. On the other hand, since it is difficult to completely remove the basic functional groups, it is set to be greater than 0. The amount of basic functional groups is preferably less than 0.5 meq / g, more preferably less than 0.4 meq / g, further preferably less than 0.3 meq / g, preferably more than 0.001 meq / g, and more preferably more than 0.003 meq / g.
[0048] (Ratio of acidic functional groups)
[0049] From the viewpoint of improving the adsorption performance for molecular polar substances, the ratio of the amount of acidic functional groups to the total amount of acidic functional groups and basic functional groups (amount of acidic functional groups / (amount of acidic functional groups+amount of basic functional groups)×100) is preferably 70% or more, more preferably 80% or more, further preferably 90% or more, and most preferably 95% or more.
[0050] (Alkali activation method)
[0051] The molecular polar substance adsorption carbon of the present invention is an alkali-activated carbon obtained by an alkali activation method. By alkali-activating the activation raw material, a pore structure different from other activation methods such as steam activation can be obtained, and a high specific surface area and a high acidic functional group content can be achieved. In addition, compared with the pore structure of steam-activated carbon, the alkali-activated carbon of the present invention has a pore structure that helps to improve adsorption performance. As an alkali activation method, the alkali activation treatment step described later is exemplified. In addition, as described later, alkali metals such as potassium sometimes remain in the activated carbon accompanying the alkali activation treatment.
[0052] (Total amount of hydroxyl and carboxyl groups)
[0053] In the molecular polar substance adsorption carbon of the present invention, as the functional groups constituting the above-mentioned acidic functional groups, hydroxyl groups and carboxyl groups are contained. If the content of hydroxyl groups and carboxyl groups is large, the adsorption performance of molecular polar substances is further improved, so it is preferred. The total amount of hydroxyl groups and carboxyl groups is preferably 0.6 meq / g or more, more preferably 0.8 meq / g or more, more preferably 1.0 meq / g or more, and most preferably 1.5 meq / g or more. The upper limit is not particularly limited, preferably 10.0 meq / g or less, more preferably 7.0 meq / g or less, and more preferably 5.0 meq / g or less.
[0054] In addition, considering the adsorption performance for molecular polar substances, the contents of hydroxyl groups and carboxyl groups are each preferably 0.3 meq / g or more, more preferably 0.5 meq / g or more, further preferably 0.9 meq / g or more, and most preferably 1.0 meq / g or more.
[0055] (Acidic functional group amount per unit surface area)
[0056] In order to improve the adsorption performance of molecular polar substances, it is effective to increase both the specific surface area and the amount of acidic functional groups. The amount of acidic functional groups per unit specific surface area of molecular polar substance adsorption carbon is preferably 0.7 μeq / m 2 More preferably, 1.0 μeq / m 2 More preferably, 1.2 μeq / m 2 above.
[0057] (Active Surface Area)
[0058] When the active surface area (edge surface) is above a certain level, the adsorption performance of polar substances is significantly improved. The active surface area is preferably 180 m 2 / g or more, more preferably 185m 2 / g or more, more preferably 190m 2 / g or above.
[0059] Since the higher the active surface area, the higher the adsorption performance, there is no upper limit. 2 / g or less, more preferably 350m 2 / g or less, more preferably 250m 2 / g or less, and also exhibits excellent adsorption performance.
[0060] (Pore volume)
[0061] If the pore volume of the molecular polar substance adsorbing carbon is too small, the adsorption amount may not be sufficiently ensured. On the other hand, if the pore volume is too large, the volume becomes large and the filling amount during use is reduced. The pore volume of the molecular polar substance adsorbing carbon of the present invention is preferably 0.3 cm 3 / g or more, more preferably 0.6cm 3 / g or more, more preferably 0.8cm 3 / g or more, preferably 3.0cm 3 / g or less, more preferably 2.5cm 3 / g or less, more preferably 2.0cm 3 / g or less.
[0062] (Average pore diameter)
[0063] If the average pore diameter of the molecular polar substance adsorption carbon is too small, the diffusivity of the molecular polar substance is poor and the adsorption performance is reduced. On the other hand, if the average pore diameter is too large, the volume becomes larger and the filling amount during use is reduced. The average pore diameter of the molecular polar substance adsorption carbon of the present invention is preferably 0.5 nm or more, more preferably 1.0 nm or more, further preferably 1.5 nm or more, most preferably 1.8 nm or more, preferably 5.0 nm or less, more preferably 4.5 nm or less, and further preferably 4.0 nm or less.
[0064] The molecular polar substance adsorbing carbon of the present invention has excellent adsorption performance due to its high specific surface area and large amount of acidic functional groups suitable for adsorbing molecular polar substances. Therefore, the molecular polar substance adsorbing carbon of the present invention does not need to be impregnated with an agent such as phosphoric acid that helps adsorption in the pores.
[0065] In addition, the molecular polar substance adsorbing carbon of the present invention has acidic functional groups formed on the edge surface of the activated carbon. Therefore, even if the adsorbed molecular polar substances are removed by regeneration treatment such as washing, the acidic functional groups remain in the activated carbon and can be reused as an adsorbent. The molecular polar substance adsorbing carbon of the present invention also shows an adsorption rate of 90% or more after the regeneration treatment compared with that before the treatment.
[0066] The shape of the molecular polar substance adsorbing carbon of the present invention is not particularly limited as long as it is a shape suitable for the intended use, and examples thereof include powdery, granular, fibrous, and pelletized shapes.
[0067] The various physical property values such as specific surface area and pore volume of the molecular polar substance adsorbing carbon of the present invention and the surface functional group amounts such as acidic functional group amount and basic functional group amount are all values based on the measurement methods described in the Examples.
[0068] The molecular polar substance adsorption carbon of the present invention has excellent diffusivity, adsorption rate and adsorption amount of molecular polar substances. In addition, the acidic functional groups imparted to the activated carbon have excellent adsorption of molecular polar substances, so it can be used for any purpose in the gas phase and liquid phase.
[0069] As an embodiment, the molecular polar substance adsorption carbon of the present invention is effective in gas phase applications, for example, it has excellent adsorption performance for molecular polar substances in the gas phase such as gases containing molecular polar substances, gases containing odorous components, gases containing volatile organic compounds (VOCs), etc.
[0070] In addition, as another embodiment, the molecular polar substance adsorption carbon of the present invention is effective in liquid phase applications, for example, it has excellent adsorption performance for molecular polar substances in liquid phases such as liquids containing molecular polar substances, liquids containing odorous components, liquids containing volatile organic compounds, etc.
[0071] As a specific example of gas phase use, it is exemplified as an adsorbent for ammonia emitted from concrete or painting materials in exhibition facilities such as art galleries. When activated carbon impregnated with phosphoric acid is used in art galleries, it cannot be used because the phosphoric acid emitted in trace amounts from the activated carbon will corrode the frame of the painting. The molecular polar substance adsorbing carbon of the present invention is useful because it has the same ammonia adsorption performance as activated carbon impregnated with phosphoric acid.
[0072] As a specific example of liquid phase application, an adsorbent for chloramine contained in liquids such as tap water is exemplified. The molecular polar substance adsorbing carbon of the present invention has an excellent adsorption rate for polar substances in the liquid layer, and thus can achieve a removal effect in a short time.
[0073] The molecular polar substance adsorbing carbon of the present invention can also be used in combination with other materials. For example, by impregnating finely pulverized molecular polar substance adsorbing carbon on natural fibers or synthetic fibers, the fibers can be given a deodorizing function. Clothes, insoles, underarm pads, etc. using fibers impregnated with such molecular polar substance adsorbing carbon are effective in removing malodorous components, and since the adsorption function can be regenerated by washing, the deodorizing function can be sustained.
[0074] The molecular polar substance adsorbing carbon of the present invention is also useful as a filter material for removing polar substances from liquids such as tap water, and as a filter material for filtering and preparing purified water for artificial dialysis. In addition, for example, by filling the molecular polar substance adsorbing carbon of the present invention in a container such as a filter cartridge, it can also be used as a water purifier.
[0075] The following is an explanation of the preparation method of the molecular polar substance adsorbing carbon of the present invention, but the preparation method of the present invention is not limited to the following preparation method as long as the above-mentioned desired physical properties can be obtained, and can also be appropriately changed. In addition, the following preparation conditions represent the preferred range, but it is necessary to appropriately adjust each preparation condition to obtain the desired physical properties.
[0076] (Activated raw materials)
[0077] The activated raw material is a carbonized product of a carbonaceous material. Well-known carbonaceous materials are used in the present invention. For example, difficult-graphitizing carbons such as wood, sawdust, charcoal, coconut shells, cellulose fibers, and synthetic resins (such as phenolic resins), graphitizable carbons such as mesophase asphalt, asphalt coke, petroleum coke, coal coke, needle coke, polyvinyl chloride, polyimide, and polyacrylonitrile, and mixtures thereof. These carbonaceous materials can be used alone or in combination of two or more. Preferred carbonaceous materials are combinations of synthetic resins such as phenolic resins and other carbonaceous materials (such as paper-phenolic resin laminates), polyacrylonitrile resins, and asphalt-based carbon fibers. In particular, nitrogen-containing carbonaceous materials such as polyacrylonitrile resins are preferred because they can increase the amount of acidic functional groups.
[0078] (Carbonization process)
[0079] The activation raw material is obtained by carbonizing the carbonaceous material before the activation treatment. The carbonization treatment may be heat-treating the carbonaceous material in an inert gas such as nitrogen, for example, at 400° C. to 1000° C. for 1 to 3 hours.
[0080] (Alkali Activation Treatment Process)
[0081] The activation treatment process of the present invention is to mix an activating agent containing an alkali metal compound with an activation raw material, and heat them in an inert gas to obtain an alkali activation treatment of activated carbon. In the present invention, since the alkali activation treatment is carried out at a lower temperature than before, both the specific surface area and the amount of acidic functional groups can be increased.
[0082] In the alkali activation treatment step of the present invention, an alkali metal compound is used as an alkali activator. Examples of the alkali metal compound include alkali metal hydroxides such as potassium hydroxide and sodium hydroxide; alkali metal carbonates such as potassium carbonate and sodium carbonate; and alkali metal sulfates such as potassium sulfate and sodium sulfate. Preferably, the alkali metal hydroxide is used, and more preferably, potassium hydroxide is used.
[0083] The amount of the activator used shows that the higher the mixing ratio of the activator to the activated raw material, the greater the specific surface area of the activated carbon. On the other hand, if the mixing ratio of the activator is too high, the density of the activated carbon shows a tendency to decrease. In the present invention, as long as the mixing ratio of the activator is adjusted to achieve the above-mentioned specific surface area, the mass ratio of the activator to the activated raw material (mass of the activator / mass of the activated raw material) is preferably 0.5 or more, more preferably 1.0 or more, more preferably 2.0 or more, preferably 10.0 or less, more preferably 5.0 or less, and more preferably 4.0 or less.
[0084] The alkali activation treatment of the present invention is performed under any inert atmosphere such as argon, helium, nitrogen, etc.
[0085] When the alkali activation treatment temperature of the present invention is too low, sufficient specific surface area and acidic functional group amount cannot be ensured. On the other hand, if it reaches 800°C or more, the amount of acidic functional groups decreases. Therefore, the heating temperature during the alkali activation treatment is 450°C or more, preferably 500°C or more, more preferably 550°C or more, and less than 800°C, more preferably 780°C or less, and further preferably 760°C or less. The activation treatment time is preferably 1 hour or more, more preferably 2 hours or more, preferably 10 hours or less, and more preferably 5 hours or less. In order to achieve the increase of the specific surface area and the amount of acidic functional groups of the present invention, the heating rate is preferably 1°C / minute or more, more preferably 5°C / minute or more, preferably 20°C / minute or less, and more preferably 15°C / minute or less.
[0086] (Washing process)
[0087] The washing process is a process of washing the activated carbon after the alkali activation process with water or an inorganic acid to remove the alkali metals remaining in the activated carbon. By repeating the washing process multiple times, the alkali metal removal rate can be increased.
[0088] (Water washing)
[0089] The temperature of water used in the water washing treatment is preferably 20° C. or higher, more preferably 30° C. or higher, and preferably 100° C. or lower, more preferably 95° C. or lower. The water washing treatment is preferably performed by repeating water washing and filtration several times until the pH of the filtrate reaches 7.0 or lower.
[0090] (Inorganic acid washing)
[0091] In the inorganic acid washing, as the inorganic acid, hydrochloric acid, hydrofluoric acid and the like, oxoacids such as sulfuric acid, nitric acid, phosphoric acid, and perchloric acid can be used, preferably hydrochloric acid. From the viewpoint of maintaining the physical properties of the activated carbon and improving the alkali metal removal rate, it is preferred to adjust the inorganic acid concentration in such a way that the inorganic acid is 10 to 100 parts by mass relative to 100 parts by mass of the activated carbon. The liquid temperature of the inorganic acid aqueous solution is preferably set to a temperature range that can suppress the volatilization of the inorganic acid and improve the alkali metal removal efficiency in the activated carbon, preferably 20°C or more, more preferably 30°C or more, preferably 100°C or less, and more preferably 95°C or less. The inorganic acid washing treatment is preferably repeated for washing and filtering, preferably until the potassium residual amount in the activated carbon reaches 5000 mg / kg or less (more than 0 mg / kg), more preferably the alkali metal residual amount in the activated carbon reaches 2500 mg / kg or less (more than 0 mg / kg), and further preferably reaches 1000 mg / kg or less (more than 0 mg / kg). The residual alkali metal content can be measured using an ICP emission spectrometer.
[0092] (Water washing process)
[0093] After the inorganic acid washing treatment, water washing treatment is performed to remove the inorganic acid remaining in the activated carbon. From the viewpoint of improving the removal efficiency of the inorganic acid, the temperature of the water used in the water washing treatment is preferably 20°C or more, more preferably 30°C or more, further preferably 50°C or more, preferably 100°C or less, and more preferably 95°C or less. The water washing treatment is preferably repeated several times to wash with water and filter until the pH of the filtrate reaches 6.5 or more.
[0094] (Drying process)
[0095] After the washing treatment, the activated carbon may be dried by drying. The drying may be carried out under any conditions that can remove the remaining moisture in the activated carbon, and for example, it is preferred to dry the activated carbon by heating in an air atmosphere for 0.5 to 24 hours.
[0096] The alkali-activated carbon obtained by appropriately adjusting the various preparation conditions has the above-mentioned structure as the molecular polar substance-adsorbing carbon of the present invention.
[0097] This application claims the benefit of priority based on Japanese Patent Application No. 2009-212411 filed on November 25, 2019. The entire contents of Japanese Patent Application No. 2009-212411 filed on November 25, 2019 are incorporated herein by reference in their entirety.
[0098] Example
[0099] The following embodiments are given to illustrate the present invention in more detail, but the present invention is not limited to the following embodiments and can of course be implemented by adding changes within the scope that is suitable for the above and below purposes, all of which are included in the technical scope of the present invention.
[0100] Example 1
[0101] (Activated raw materials)
[0102] As the carbonaceous material, a paper phenol resin laminate was treated in a nitrogen atmosphere at 700° C. for 2 hours to be carbonized, and the obtained paper phenol resin carbonized product was used as an activation material.
[0103] (Activation treatment process)
[0104] To 1.0 parts by weight of the obtained paper phenolic resin carbonized product, a commercially available alkali activator (aqueous potassium hydroxide solution with a concentration of 48.5%) was added so that the mass ratio of the activator ([mass of the alkali component of the activator] / [mass of the activated raw material]: hereinafter referred to as the KOH / C ratio) was 4.0, and the temperature was raised to 600°C under a nitrogen atmosphere and maintained at this temperature for 2 hours to obtain alkali-activated carbon.
[0105] (Water washing process)
[0106] The obtained alkali-activated carbon was washed with warm water at 60° C. until the pH of the filtrate became 7.0 or less.
[0107] (Inorganic acid washing process)
[0108] The activated carbon after the water washing treatment was subjected to an acid washing treatment in a 5.25 wt % hydrochloric acid aqueous solution adjusted to a liquid temperature of 60° C. for 1 hour, and then suction filtration was performed.
[0109] (Post-treatment process (water washing process))
[0110] The activated carbon after filtration was repeatedly washed and dehydrated with warm water at 60° C. until the pH reached 6.5 or higher.
[0111] (Drying process)
[0112] The obtained activated carbon was dried in a dryer set at 115° C. for 24 hours to obtain activated carbon No. 1.
[0113] Example 2
[0114] Activated carbon No. 2 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminated board to coke.
[0115] Example 3
[0116] Polyacrylonitrile (PAN) resin as a carbonaceous material was placed in a muffle furnace (manufactured by Koyo Heat Treatment Co., Ltd.), and the temperature in the furnace was raised to 650°C (heating rate: 10°C / min) under a nitrogen atmosphere and maintained at this temperature for 2 hours. The obtained PAN resin carbonized product was used as an activation raw material.
[0117] (Activation treatment process)
[0118] Alkali-activated carbon was obtained in the same manner as in Example 1 except that the obtained PAN resin carbonized product was used and the KOH / C ratio was changed to 3.0. The alkali-activated carbon was subjected to the same washing treatment and drying treatment as in Example 1 to prepare activated carbon No. 3.
[0119] Example 4
[0120] Activated carbon No. 4 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminate to pitch-based carbon fibers (average fiber diameter 15 μm, average fiber length 200 μm).
[0121] Example 5
[0122] Activated carbon No. 5 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminate to coke and KOH / C was adjusted to 2.0.
[0123] Example 6
[0124] Activated carbon No. 6 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminated board to coke.
[0125] Example 7
[0126] Activated carbon No. 7 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminate to coke and KOH / C was adjusted to 5.0.
[0127] Example 8
[0128] Activated carbon No. 8 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminate to pitch-based carbon fibers (average fiber diameter 15 μm, average fiber length 200 μm) and KOH / C was set to 3.0.
[0129] Example 9
[0130] Activated carbon No. 9 was prepared in the same manner as in Example 1 except that the carbonaceous material was changed from the paper phenol resin laminate to pitch-based carbon fibers (average fiber diameter 15 μm, average fiber length 200 μm) and KOH / C was set to 5.0.
[0131] Comparative Example 1
[0132] Alkali-activated carbon was obtained in the same manner as in Example 1 except that the PAN resin carbonized product obtained in Example 3 was used as the activation raw material and the activation treatment conditions were set to a KOH / C ratio of 0.8 and an activation temperature of 800° C. The alkali-activated carbon was subjected to the same washing and drying treatments as in Example 1 to produce activated carbon No. 10.
[0133] Comparative Example 2
[0134] Commercially available coconut shell steam-activated activated carbon (W10-30 manufactured by MC Inbiotech Co., Ltd.) was used as activated carbon No. 11.
[0135] Comparative Example 3
[0136] Commercially available acid-impregnated activated carbon (MAXSORB XCA-AS manufactured by MC Inbiotech) was used as activated carbon No. 12.
[0137] Comparative Example 4
[0138] 100 g of the activated carbon of Example 6 was placed in a muffle furnace (manufactured by Koyo Heat Treatment Co., Ltd.), and the temperature was raised to 600° C. in a nitrogen atmosphere and maintained at the temperature for 2 hours to produce activated carbon No. 13.
[0139] Comparative Example 5
[0140] Coke was used as an activation raw material, a commercially available alkali activator was added in a ratio of KOH / C = 1.6, the temperature was raised to 800°C in a nitrogen atmosphere, and the temperature was maintained for 2 hours to obtain alkali-activated carbon. The alkali-activated carbon was subjected to the same washing and drying treatment as in Example 1 to produce activated carbon No. 14.
[0141] Comparative Example 6
[0142] Activated carbon No. 15 was prepared in the same manner as in Comparative Example 5 except that the carbonaceous material was changed from coke to pitch-based carbon fibers (average fiber diameter 15 μm, average fiber length 200 μm) and KOH / C was set to 1.7.
[0143] Comparative Example 7
[0144] 100 g of the activated carbon of Comparative Example 2 was placed in a rotary kiln (produced by Tanaka Tech), and the temperature in the kiln was raised to 500° C. while air was circulated in the kiln at a flow rate of 5 L / min. The temperature was maintained for 3 hours to perform oxidation treatment, thereby producing activated carbon No. 16.
[0145] Comparative Example 8
[0146] 100 g of the activated carbon of Comparative Example 2 was charged into a rotary kiln (manufactured by Tanaka tec), and the temperature in the furnace was raised to 500°C while air was circulated in the furnace at a flow rate of 0.5 L / min. Then, air was circulated in the furnace at a flow rate of 0.5 L / min and pure water was circulated in the furnace at a flow rate of 3.62 g / min so that the relative humidity reached 90%, and the temperature was maintained for 3 hours to carry out oxidation treatment, thereby producing activated carbon No. 17.
[0147] Comparative Example 9
[0148] 100 g of the activated carbon of Comparative Example 2 was placed in a beaker and oxidized for 3 hours in a 20% nitric acid aqueous solution at 60°C while stirring at 300 rpm. After the oxidation treatment, the nitric acid aqueous solution was removed by rinsing with warm water at 60°C while suction filtration was performed, and the filtered activated carbon was boiled in warm water for 1 hour. The boiled activated carbon was repeatedly washed and dehydrated with warm water at 60°C until the pH reached 6.5 or above. The obtained activated carbon was dried in a dryer set at 115°C for 24 hours to produce activated carbon No. 18.
[0149] Comparative Example 10
[0150] Coconut shell steam-activated activated carbon with a high specific surface area (Z10-30HS, a primary pulverized product manufactured by MC Inbiotech Co., Ltd.) was used as activated carbon No. 19.
[0151] Each of the above samples was evaluated under the following conditions.
[0152] (Specific surface area)
[0153] The sample (0.2 g) was vacuum dried at 250°C and the amount of nitrogen adsorbed in a liquid nitrogen atmosphere (-196°C) was measured using a nitrogen adsorption apparatus (ASAP-2420 manufactured by Micromeritics) to obtain a nitrogen adsorption isotherm. The specific surface area (m 2 / g).
[0154] (Total pore volume)
[0155] The total pore volume (mL / g) was calculated from the amount of nitrogen adsorbed at a relative pressure (P / P0) = 0.93 in the nitrogen adsorption isotherm.
[0156] (Average pore diameter)
[0157] The average pore diameter was calculated based on the following formula, assuming that the pores of activated carbon were cylindrical.
[0158] Average pore diameter (nm) = 4 × total pore volume (mL / g) / specific surface area (m 2 / g)×1000
[0159] (Total acidic functional groups)
[0160] The amount of acidic functional groups is determined according to the Boehm method (document "HP Boehm, Adzan. Catal, 16, 179 (1966)"). Specifically, 50 mL of an aqueous sodium ethoxide solution (0.1 mol / L) is added to 1 g (Examples 1 to 9) or 2 g (Comparative Examples 1, 2, 4 to 10) of activated carbon, stirred at 500 rpm for 2 hours, and then allowed to stand for 24 hours. After 24 hours, the mixture is stirred for another 30 minutes and filtered for separation. 0.1 mol / L of hydrochloric acid is added dropwise to 25 mL of the obtained filtrate, and the hydrochloric acid titration at a pH of 4.0 is measured. In addition, as a blank test, 0.1 mol / L of hydrochloric acid is added dropwise to 25 mL of the sodium ethoxide aqueous solution (0.1 mol / L), and the hydrochloric acid titration at a pH of 4.0 is measured. Then, the amount of acidic functional groups (meq / g) is calculated by the following formula (1).
[0161] [Mathematical formula 1]
[0162]
[0163] Where, a: Hydrochloric acid titration in blank test
[0164] b: Hydrochloric acid titration when the sample is reacted
[0165] S: Sample mass (g)
[0166] (Single acidic functional group)
[0167] 0.1 mol / 1000 mL of NaOH, 0.05 mol / 1000 mL of Na2CO3, or 0.1 mol / 1000 mL of NaHCO3 was used instead of 0.1 mol / 1000 mL of NaOEt, and the same evaluation as the total acidic functional group amount was performed. In addition, the calculation of each acidic functional group was obtained by the following formula.
[0168] [Table 1]
[0169]
[0170] The method for quantifying the amount of functional groups in activated carbon is based on the method of [Surface, 34[2](1996) Otowa p.62] or [Catal., 1966
[16] (US) p.179]. 1 g (Examples 1 to 9) or 2 g (Comparative Examples 1, 2, 4 to 10) of activated carbon is placed in a 100 mL conical flask, and 50 mL of N / 10 alkaline reagent ((a) sodium bicarbonate, (b) sodium carbonate, (c) caustic soda, (d) sodium ethoxide) is added respectively. After shaking for 24 hours, the mixture is filtered and the unreacted alkaline reagent is titrated with N / 10 hydrochloric acid. Since the carboxyl group reacts with all reagents (a) to (d), the lactone group reacts with reagents (b) to (d), the hydroxyl group reacts with reagents (c) to (d), and the quinone group reacts with reagent (d), the amount of functional groups is quantified by subtracting the respective titration amounts.
[0171] (Basic functional group)
[0172] The amount of basic functional groups is obtained by back titration during the determination of the amount of acidic functional groups. Specifically, 50 mL of hydrochloric acid (0.1 mol / L) is added to 1 g (Examples 1 to 9) or 2 g (Comparative Examples 1, 2, 4 to 10) of activated carbon, stirred at 500 rpm for 2 hours, and then allowed to stand for 24 hours. After 24 hours, the mixture is stirred for another 30 minutes and filtered for separation. 0.1 mol / L of sodium hydroxide is added dropwise to 25 mL of the obtained filtrate, and the amount of sodium hydroxide titrated when the pH reaches 8.0 is measured. In addition, as a blank test, 0.1 mol / L of sodium hydroxide is added dropwise to 25 mL of the hydrochloric acid (0.1 mol / L), and the amount of sodium hydroxide titrated when the pH reaches 8.0 is measured. Then, the amount of basic functional groups (meq / g) is calculated by the following formula (2).
[0173] [Mathematical formula 2]
[0174]
[0175] Where, a: the titration amount of sodium hydroxide in the blank test
[0176] b: The amount of sodium hydroxide titrated when the sample is reacted
[0177] S: Sample mass (g)
[0178] (ratio of acidic functional groups)
[0179] The ratio of the acidic functional group amount was calculated from the above-mentioned acidic functional group amount (meq / g) and basic functional group amount (meq / g).
[0180] Acidic functional group amount / (acidic functional group amount+basic functional group amount)×100
[0181] (Acidic functional group amount per unit surface area)
[0182] According to the above specific surface area (m 2 / g), the amount of acidic functional groups (meq / g), and the amount of acidic functional groups per unit specific surface area (μeq / m 2 ).
[0183] Acidic functional group amount (meq / g) / specific surface area (m 2 / g)×1000(unit adjustment)
[0184] (Acidic functional group amount and active surface area after oxidation)
[0185] The un-crushed activated carbon fibers of Examples 4, 8 to 9 and Comparative Example 6, and the granular carbons of Examples 2, 3, 5 to 7 and Comparative Examples 1, 2, 4, 5, 7 to 10 were crushed to a size of less than 250 μm using a mortar, and oxidized at 300° C. for 24 hours in an air atmosphere. The amount of acidic surface functional groups (meq / g) after oxidation was calculated based on the following formula so that the area occupied by one molecule of the oxygen-containing compound was 0.083 nm: 2 , calculate the active surface area (m 2 / g).
[0186] [Mathematical formula 3]
[0187] Active surface area (m 2 / g)=a×10 -3 ×b×c×10 -18
[0188] a: Amount of acidic surface functional groups after oxidation (meq / g)
[0189] b: 6.02×10 23 (mol -1 ) Avogadro's constant
[0190] c: 0.083(nm 2 ) The area occupied by one molecule of oxygen-containing compound
[0191] (Ammonia adsorption evaluation)
[0192] Activated carbon crushed to 250 μm or less was added to a 5 L Tedlar sampling bag. The amount of activated carbon added was as follows.
[0193] Examples 1, 2, 4 and Comparative Example 3: 0.01 g, 0.02 g, 0.03 g
[0194] Example 3: 0.005g, 0.01g, 0.02g
[0195] Comparative Example 1: 0.03g, 0.06g, 0.09g
[0196] Comparative Example 2: 0.1g, 0.3g, 0.5g
[0197] After the activated carbon was added, the Tedlar sampling bag was degassed using a vacuum pump and then filled with 3L of dry air. Next, ammonia water (manufactured by Kishida Chemical Co., Ltd., purity 28%) was injected into the Tedlar sampling bag to make its initial concentration 100ppm, and it was left to stand in a constant temperature bath at 25°C for 24 hours. Then, the ammonia concentration in the Tedlar sampling bag was quantified using a detection tube (manufactured by Gastec Co., Ltd.) to prepare an adsorption isotherm. The adsorption amount at an equilibrium concentration of 10ppm was calculated using the Freundlich formula from the obtained adsorption isotherm.
[0198] [Table 2A]
[0199]
[0200] [Table 2B]
[0201]
[0202] Activated carbon No. 1 to 4 all have a specific surface area of 1500m 2 / g or more, and having a high specific surface area of 2.1meq / g or more, a high acidic functional group content of 2.1meq / g or more, and a low basic functional group content of 0.2meq / g or less, and a molecular polar substance adsorbing carbon that meets the requirements of the present invention. In addition, the acidic functional group content of these activated carbons after oxidation is 3.15meq / g or more, and the active surface area is 180m 2 The ammonia adsorption amounts of activated carbons No. 1 to 4 were all 10.0 mg / g or more, showing adsorption performance superior to that of activated carbons No. 10 and 11 as comparative examples.
[0203] Activated carbon No. 10 is a conventional high temperature activated alkali activated carbon. The specific surface area of this activated carbon is 2000m 2 / g or more, but the amount of ammonia adsorption is small due to the small amount of acidic functional groups.
[0204] In addition, activated carbon No. 11 is a coconut shell activated carbon activated by water vapor, but it hardly adsorbs ammonia due to its small amount of acidic functional groups. Activated carbon No. 12 is activated carbon impregnated with a chemical, and it has a high ammonia adsorption capacity due to the effect of the chemical, but it cannot be reused.
[0205] like Figure 1 As shown, the activated carbons No. 1 to 4 (Examples 1 to 4) satisfying the requirements of the present invention have an ammonia adsorption capacity more than twice that of the conventional activated carbon No. 10 (Comparative Example 1), showing excellent ammonia adsorption performance. In addition, activated carbons No. 2 to 4 show excellent adsorption performance equivalent to activated carbon No. 12 (Comparative Example 3) impregnated with a reagent.
[0206] like Figures 2 to 4 As shown in Figures 7 and 8, there is a correlation between the amount of acidic functional groups and the amount of basic functional groups. If the amount of acidic functional groups increases, the amount of basic functional groups tends to decrease. In addition, it can be seen that when the amount of acidic functional groups increases, the amount of ammonia adsorption also increases. Furthermore, as Figure 6 As shown, when the amount of acidic functional groups per unit specific surface area increases, the amount of ammonia adsorption also tends to increase, and the increase in not only the amount of acidic functional groups but also the specific surface area is effective in improving the adsorption performance.
[0207] (Chloramine adsorption evaluation)
[0208] In a 100 mL stoppered conical flask (brown), activated carbon of adjusted particle size was added. Examples 4, 8 to 9 and Comparative Example 6 were un-crushed activated carbon fibers, and Examples 2, 3, 5 to 7 and Comparative Examples 1, 2, 4, 5, 7 to 10 were granular activated carbon graded with a sieve of 53 to 125 μm. The amount of activated carbon added was as follows.
[0209] ·Examples 2 to 9: 0.01g, 0.03g, 0.05g, 0.1g, 0.2g
[0210] Comparative Examples 2, 8 to 10: 0.1 g, 0.3 g, 0.5 g, 1.0 g, 1.5 g
[0211] ·Comparative Examples 1, 4 to 7: 0.05 g, 0.1 g, 0.2 g, 0.3 g, 0.5 g
[0212] After the activated carbon was added, 100 mL of a chloramine (monochloramine) aqueous solution prepared to about 100 ppm was added, and the mixture was stirred at 200 rpm for 2 hours in a constant temperature bath at 25° C., and then the activated carbon was filtered with a syringe filter to obtain a filtrate.
[0213] 0.5 mL of phosphate buffer was taken in a 10 mL stoppered colorimetric tube, and the filtrate diluted to a predetermined concentration was added to the buffer to make a total of 10 mL. Then, 0.1 g of N,N-diethyl-p-phenylenediamine (DPD) reagent (manufactured by Kanto Chemical Co., Ltd.) was added, and after mixing, the free residual chlorine concentration of the color-developed test solution was measured using a residual chlorine meter (manufactured by HACH Co., Ltd.).
[0214] Then, 0.1 g of potassium iodide (manufactured by Kishida Chemical Co., Ltd.) was added to the test solution to be measured and dissolved. After standing for 2 minutes, the residual chlorine concentration was measured using a residual chlorine meter. The combined residual chlorine (chloramine) concentration (mg / L) was calculated from the difference between the above residual chlorine concentration and the free residual chlorine concentration, and an adsorption isotherm was prepared from the relationship between the residual chloramine concentration and the chloramine removal amount per unit weight of activated carbon (mg / g-activated carbon). The removal amount at a residual concentration of 3 ppm was calculated from the obtained adsorption isotherm using the Freundlich formula.
[0215] (Evaluation of chloramine removal rate)
[0216] 0.1 g of activated carbon with adjusted particle size was placed in a 100 mL stoppered conical flask (brown). As the activated carbon with adjusted particle size, un-crushed activated carbon fibers were used in Example 4 and Comparative Example 6, and granular activated carbon classified by a sieve of 53 to 125 μm was used in Examples 2, 3, 5 to 7 and Comparative Examples 1, 2, 4, 5, 7 to 10.
[0217] After adding activated carbon, add 100 mL of chloramine (monochloramine) aqueous solution adjusted to about 100 ppm, stir at 200 rpm in a constant temperature bath at 25°C for 5 minutes, 10 minutes, 20 minutes, 30 minutes, 60 minutes, 90 minutes and 120 minutes, and then calculate the combined residual chlorine (chloramine) concentration (mg / L) in the same way as the above method. From the obtained residual chloramine concentration (C) and the initial chloramine concentration (C0), and defining the stirring time (reaction time) as t, the chloramine removal rate per unit time is calculated by the following formula and defined as the chloramine removal rate (v, % / min).
[0218] v(% / min)={(C0-C) / C0×100} / t
[0219] [Table 3A]
[0220]
[0221] [Table 3B]
[0222]
[0223] Activated carbon No. 2 to 9 all have a specific surface area of 1500m 2 / g or more, and having a high specific surface area of 2.1meq / g or more, a high acidic functional group content of 2.1meq / g or more, and a low basic functional group content of 0.2meq / g or less, and a molecular polar substance adsorbing carbon that meets the requirements of the present invention. In addition, the acidic functional group content of these activated carbons after oxidation is 3.15meq / g or more, and the active surface area is 180m 2 / g or above.
[0224] Activated carbons No. 2 to 9 all had a chloramine removal amount of 30 mg / g or more and a chloramine removal rate of 6% / min or more, and showed superior adsorption performance compared to activated carbons No. 10, 11, and 13 to 19 as comparative examples.
[0225] Activated carbon No. 10, 11, 13 to 19 has a specific surface area of 1000m 2 / g or more, but the amount of acidic functional groups is small and the active surface area is also small. These activated carbons have insufficient chloramine removal capacity and slow chloramine removal rate.
[0226] Figures 8 to 11 This is a graph showing the relationship between various physical properties of activated carbon and the amount of chloramine removed. Figures 12 to 15 This is a graph showing the relationship between various physical properties of activated carbon and the chloramine removal rate.
[0227] like Figure 8 , 12 As shown, no correlation was found between specific surface area and chloramine removal amount and chloramine removal rate.
[0228] like Fig. 9 As shown in Figure 2, when the amount of acidic functional groups is large, the amount of chloramine removal also tends to increase. Fig.13 As shown, there is a correlation between the amount of acidic functional groups and the chloramine removal rate.
[0229] In addition, from Fig. 9 , 10 , 13, and 14, it can be seen that there is a correlation between the amount of acidic functional groups and the amount of basic functional groups, and when the amount of acidic functional groups increases, the amount of basic functional groups tends to decrease.
[0230] like Fig. 9 , 11 As shown in Figures 13 and 15, it can be seen that activated carbon Nos. 2 to 9 show excellent adsorption performance for chloramine.
[0231] Fig.16 It is a graph showing the relationship between the chloramine removal rate and the amount of chloramine removed.
[0232] like Fig.16 As shown, it can be seen that the activated carbons No. 2 to 7 have excellent catalytic performance.
Claims
1. A molecular polar substance adsorption carbon obtained by an alkali activation method, wherein the amount of acidic functional groups is 2.1 meq / g or more, the amount of basic functional groups is greater than 0 and less than 0.3 meq / g, and the specific surface area is 1000 to 4000 m 2 / g, The activation raw material of the molecular polar substance adsorbed carbon is a carbide of a carbonaceous substance. The carbonaceous material is selected from at least one of wood, sawdust, charcoal, coconut shell, cellulose fiber, phenolic resin, mesophase pitch, pitch coke, petroleum coke, needle coke, polyvinyl chloride and polyimide.
2. The molecular polar substance adsorbing carbon according to claim 1, wherein: The total amount of hydroxyl groups and carboxyl groups contained in the acidic functional groups is 0.6 meq / g or more.
3. The molecular polar substance adsorbing carbon according to claim 1 or 2, wherein: The ratio of the amount of the acidic functional groups to the total amount of the acidic functional groups and the basic functional groups is 70% or more.
4. The molecular polar substance adsorbing carbon according to claim 1 or 2, wherein: The amount of acidic functional groups per unit specific surface area of the polar substance adsorbed carbon is 0.7 μeq / m 2 above.
5. The molecular polar substance adsorbing carbon according to claim 1 or 2, wherein: The polar substance adsorption carbon has no medicine impregnated in the pores.
6. The molecular polar substance adsorbing carbon according to claim 1 or 2, wherein: The active surface area of the polar substance adsorbing carbon is 180m 2 / g or above.
7. The molecular polar substance adsorbing carbon according to claim 1 or 2, wherein: The molecular polar substance adsorption carbon is selected from powder, granular or particle form.
Citation Information
Patent Citations
Active carbon fiber for removing malodorous gas and air cleaning sheet
JP2002159852A
Activated carbon and method for manufacturing the same
JP2004315243A
Charge eraser and method for erasing charge
JP2009212411A
Polar substance adsorption active carbon
JP2019098324A
Active carbon fiber and method of producing the same
JP2017172099A