A stable and efficient antibacterial composition and preparation method thereof
By adding graphene and metal hydrate to the antibacterial materials and combining white oil, the problems of easy agglomeration and poor stability of antibacterial components are solved, and efficient and stable antibacterial effects and excellent lubricating and anti-wear properties are achieved.
Patent Information
- Application Number
- CN202110592472.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-28
AI Technical Summary
The antibacterial components added to existing antibacterial materials are not effective. Graphene is difficult to fully disperse in the alkane oil system due to the problems of easy agglomeration and wettability, resulting in poor antibacterial and stability.
Add 2-3% graphene and 1-5% metal hydrate (such as basic zinc carbonate) to the antibacterial composition, and generate zinc oxide supported on the graphene layer structure through high temperature decomposition, and combine white oil as solvent to form Stable graphene oxide-metal hydrate composite material improves antibacterial effect and enhances stability.
The antibacterial effect and stability of the antibacterial composition are significantly improved, and can maintain uniform dispersion after long-term placement, and have fast, broad-spectrum antibacterial and excellent lubricating and anti-wear properties.
Smart Images

Figure BDA0003090086580000071 
Figure BDA0003090086580000072 
Figure BDA0003090086580000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of antibacterial technology, and specifically relates to a stable and efficient antibacterial composition and a preparation method thereof. Background Art
[0002] With the development of economy and the improvement of living standards, people have higher and higher requirements for living environment. Microbial pollution affects people's healthy life, so the antibacterial property of antibacterial materials has received more and more attention, and the market demand has become larger and larger. It has become particularly important for many materials used by people in daily life to have antibacterial properties, which often become an important indicator for people to choose and buy. Nowadays, the antibacterial property of materials is often achieved by adding antibacterial ingredients to ordinary materials, but the actual application effect of the ingredients used to improve the antibacterial property of materials on the market is not ideal, and there are problems such as low antibacterial effect and poor stability.
[0003] Graphene is a two-dimensional ultra-thin nanomaterial with many excellent properties. However, due to its large specific surface area, graphene is prone to agglomeration, which not only reduces its own adsorption capacity, but also affects the excellent performance of graphene itself. And graphene agglomeration is irreversible unless external force is applied to make it evenly dispersed. At the same time, the wettability of graphene in the organic phase will affect its sedimentation volume, further affecting its dispersibility. Therefore, graphene often encounters obstacles in the actual application process and cannot fully exert its performance effect. Summary of the invention
[0004] In order to solve the above problems, the first aspect of the present invention provides a stable and efficient antibacterial composition, which comprises 2-3% of a two-dimensional material, 0-0.5% of an organic dispersant, and the balance made up of solvent oil, by weight percentage.
[0005] Preferably, the two-dimensional material is graphene.
[0006] Further preferably, the graphene is graphene oxide.
[0007] Graphene has a unique two-dimensional carbon structure, in which the carbon atoms are arranged in sp 2The graphene is hybridized in a layered structure and exhibits excellent optical and electrical properties. With the development of bio-nanotechnology, the application of graphene in the field of life sciences has received more and more attention. The present invention finds that adding 2-3% graphene to the antibacterial composition can enhance the antibacterial effect of the antibacterial composition. It is speculated that the graphene has a high activity of interacting with the skeleton molecules of the microbial cell membrane. When it contacts the microorganism, it can "extract" the bacterial cell membrane support structure and destroy the integrity of the cell membrane, thereby effectively eliminating the bacteria. Although graphene has many advantages, its high specific surface area and high adsorption make it easy to self-aggregate and difficult to fully disperse in the alkane oil system. The present invention has found through a large number of experimental investigations that when metal hydrates, especially basic zinc carbonate, are added to the antibacterial composition, the antibacterial effect of the antibacterial composition can be significantly improved. The reason may be that basic zinc carbonate can be decomposed into an antibacterial agent precursor at high temperature, and the generated zinc oxide is in situ loaded in the graphene layer structure to form an antibacterial component with a stronger surface effect, so that the adsorption capacity of the antibacterial composition on microorganisms is improved. On the one hand, the external skeleton structure of the bacteria is destroyed. On the other hand, the dissolution of metal oxides may destroy the metabolic balance of regulatory substances in the microorganism. Different mechanisms act simultaneously, which significantly enhances the antibacterial effect of the antibacterial composition.
[0008] Preferably, the antibacterial composition also includes metal hydrate.
[0009] Further preferably, the weight ratio of the graphene oxide to the metal hydrate is (1-5):1.
[0010] Preferably, the metal hydrate is basic zinc carbonate, FeSO 4 7H 2 O、NiSO 4 7H 2 O、ZnSO 4 7H 2 O or CuSO 4 ·5H 2 At least one of O.
[0011] Preferably, the mass ratio of the metal hydrate to the antibacterial composition is 1-2%.
[0012] Graphene and metal hydrates both have high surface activity, and the effective combination process of the two is difficult to control. The present invention explores and finds that when the graphene is specifically graphene oxide, the active functional groups in its π-π structure increase, and the presence of oxygen atoms makes it easier for graphene to form resonant induction with free electrons. The ability of graphene to load metal hydrates is greatly improved, and the metal hydrates are evenly filled in the two-dimensional carbon layer structure, which solves the problem that graphene is easy to agglomerate and difficult to fully and effectively load metal hydrates. The obtained graphene oxide-metal hydrate composite material can quickly adsorb pathogens in the air, destroy its cell structure and life activity balance, and the antibacterial effect is further improved.
[0013] Graphene oxide and metal hydrate have obvious synergistic effect on the antibacterial effect of the product, but their compatibility in alkane oil is poor, and they are prone to stratification, agglomeration and discoloration defects after being placed for a long time. The present invention has found through a large number of experimental studies that when the weight ratio of graphene oxide and metal hydrate is (1-5): 1, the stability of the antibacterial composition is significantly improved. It may be that under this condition, nano-scale basic zinc carbonate and organic dispersant are co-intercalated in the graphene sheet structure to form a stable space barrier, which inhibits the agglomeration of graphene to form sedimentation particles, and improves the compatibility of the non-structured phase and the structured phase in the antibacterial composition, so that the antibacterial composition can still maintain a uniform and dispersed storage state after being placed for a long time, and it is not easy to produce precipitation to affect the antibacterial effect of the antibacterial composition. The surface properties of the antibacterial agent and the antibacterial agent precursor in the system are optimized under the "anchoring effect" of the organic dispersant, and can fully act on the internal and external structures of microorganisms to achieve a rapid and broad-spectrum antibacterial effect.
[0014] Preferably, the organic dispersant is selected from one or more of alkylbenzene sulfonates, quaternary ammonium salts, amine salts, sulfate ester salts, and phosphate ester salts.
[0015] Preferably, the solvent oil is alkane oil and / or aromatic hydrocarbon oil.
[0016] Preferably, the alkane oil is white oil.
[0017] Preferably, the kinematic viscosity of the white oil is 2-10 mm 2 / s, the test temperature is 40℃.
[0018] Further preferably, the white oil is a mixture of No. 3 white oil, No. 5 white oil and No. 7 white oil.
[0019] Further preferably, the weight ratio of No. 3 white oil, No. 5 white oil and No. 7 white oil is 1:(2-4):(1.4-3).
[0020] Solvent oil is the main base material of the antibacterial composition, and the difference in its properties directly affects the performance of the antibacterial composition. The present invention found that when white oil is selected as the solvent oil, the compatibility of the inorganic phase and the organic phase in the system is good, and the antibacterial composition can still maintain a uniformly dispersed storage state after being placed in high and low temperature cycles; the present invention unexpectedly found that when white oil is selected as the solvent oil, the antibacterial composition exhibits excellent lubrication and anti-wear effects, especially when the white oil is No. 3 white oil, No. 5 white oil, and No. 7 white oil, the antibacterial composition and the steel ball are in contact and friction. The wear area of the steel ball after the wear test is small. The reason is that the shear strength of the inorganic layered structure in the antibacterial composition is low, and the carbon layer structure forms a stress protection film between the steel ball and the friction surface, which reduces the contact between the friction surfaces and effectively dilutes the wear pressure borne by the steel ball. It was further found that when the weight ratio of No. 3 white oil, No. 5 white oil, and No. 7 white oil was 1:(2-4):(1.4-3), the stability, antibacterial property and wear resistance of the antibacterial composition were optimized to the greatest extent. This may be because under this condition, the fluidity of graphene, metal hydrate and organic dispersant in the base material is optimal, and the effective components in the system can maintain good dispersion, which inhibits the components from agglomerating to form sludge and aggravating the wear of the steel balls, thereby giving the antibacterial composition excellent lubrication and anti-wear effects.
[0021] The second aspect of the present invention provides a method for preparing the stable and efficient antibacterial composition, which comprises mixing the two-dimensional material and the metal hydrate at a temperature above 200° C., and then mixing the mixture with solvent oil and an organic dispersant to obtain the antibacterial composition.
[0022] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0023] (1) The present invention provides a stable and efficient antibacterial composition, which has high antibacterial properties, stability and wear resistance. The antibacterial composition of the present invention can be widely used in antibacterial materials, which is of great significance for improving people's health and quality of life. The preparation method of the present invention is simple and convenient, has strong repeatability, and is conducive to large-scale production.
[0024] (2) The present invention improves the problem of graphene agglomeration by adding graphene and metal hydrate to the composition, forming an antibacterial component with a stronger surface effect, so that the adsorption capacity of the antibacterial composition on microorganisms is improved, on the one hand, the external skeleton structure of bacteria is destroyed, and on the other hand, the dissolution of metal oxides may destroy the metabolic balance of regulatory substances in the microorganism. Different mechanisms act simultaneously, significantly enhancing the antibacterial effect of the antibacterial composition. At the same time, the present invention preferably uses white oil as the main base material, and the compatibility of the inorganic phase and the organic phase in the system is good. The antibacterial composition can still maintain a uniformly dispersed storage state after being placed in cycles at different temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1is the original spectrum of the TGA test curve of the antibacterial composition of Example 1; DETAILED DESCRIPTION
[0026] The content of the present invention can be further understood by combining the following detailed description of the preferred implementation method of the present invention and the embodiments included. Unless otherwise stated, all technical and scientific terms used in this article have the same meaning as those of ordinary skill in the art to which the application belongs. If the definition of a specific term disclosed in the prior art is inconsistent with any definition provided in the application, the term definition provided in the application shall prevail.
[0027] The raw materials in the present invention are purchased from the following manufacturers:
[0028] Graphene oxide: Shanghai Maoguo Nanotechnology Co., Ltd.
[0029] Sodium dodecylbenzenesulfonate: Nanjing Milan Chemical Co., Ltd.
[0030] Fatty alcohol ammonium sulfate: Nantong Qianhe Chemical Co., Ltd.
[0031] Nano basic zinc carbonate: Sigma-Aldrich
[0032] No. 3 white oil: Haorui Petrochemical
[0033] No. 5 white oil: Haorui Petrochemical
[0034] No. 7 white oil: Haorui Petrochemical
[0035] Example 1
[0036] This embodiment provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7mm. 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0037] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition. Figure 1 Original spectrum of TGA test curve of antibacterial composition.
[0038] Example 2
[0039] This embodiment provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7mm. 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:2:3.
[0040] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.
[0041] Example 3
[0042] This embodiment provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7mm. 2 / s, and the test temperature is 40° C. The white oil is No. 3 white oil.
[0043] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.
[0044] Example 4
[0045] This embodiment provides a stable and efficient antibacterial composition, which includes 2% graphene oxide, 0.3% fatty alcohol ammonium sulfate, 1% nano basic zinc carbonate, and solvent oil as the balance. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7 mm 2 / s, and the test temperature is 40° C. The white oil is No. 5 white oil.
[0046] The preparation method of the stable and efficient antibacterial composition comprises: mixing graphene oxide and nano basic zinc carbonate at 260° C. to obtain a mixture, and mixing the mixture, solvent oil and fatty alcohol ammonium sulfate to obtain a stable and efficient antibacterial composition.
[0047] Comparative Example 1
[0048] This comparative example provides a stable and efficient antibacterial composition, which includes 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance of solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7mm.2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0049] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing nano basic zinc carbonate, solvent oil and sodium dodecylbenzene sulfonate to obtain the stable and efficient antibacterial composition.
[0050] Comparative Example 2
[0051] This comparative example provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, and the balance of solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7 mm 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0052] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide, solvent oil and sodium dodecylbenzene sulfonate to obtain the stable and efficient antibacterial composition.
[0053] Comparative Example 3
[0054] This comparative example provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7 mm 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0055] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.
[0056] Comparative Example 4
[0057] This comparative example provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 15 mm 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0058] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.
[0059] Comparative Example 5
[0060] This comparative example provides a stable and efficient antibacterial composition, which includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil. The solvent oil is white oil, and the kinematic viscosity of the white oil is 7 mm 2 / s, and the test temperature is 40° C. The white oil is a mixture of No. 3 white oil, No. 5 white oil, and No. 7 white oil, and the weight ratio of the No. 3 white oil, No. 5 white oil, and No. 7 white oil is 1:3:2.
[0061] The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 150° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.
[0062] Performance Testing
[0063] The antibacterial compositions obtained in Examples 1 to 4 and Comparative Examples 1 to 5 were subjected to performance tests.
[0064] 1. Antibacterial activity: The antibacterial composition was incubated with Escherichia coli and Staphylococcus aureus at 37°C (the number of bacteria was 1×10 4 cfc / mL), and the number of bacteria was measured after 8h and 24h. The results are shown in Table 1.
[0065] Table 1 Antibacterial test results
[0066]
[0067] 2. Stability: The antibacterial composition was poured into a centrifuge tube and placed continuously in a transparent water bath at different temperatures, i.e., 15°C for 5 days, 40°C for 40 days, and 15°C for 75 days, and the time when obvious precipitation began to appear in the centrifuge tube was recorded. Examples 1 to 4 of the present invention did not precipitate at all, while the comparative examples precipitated at different times. The results are shown in Table 2.
[0068] Table 2 Stability test results
[0069]
[0070]
[0071] 3. Wear resistance: Wear test was conducted according to the industry standard SH / T0189-92. The experimental conditions were: speed 1200r / min, load 392N, test time 60min. The results are shown in Table 3.
[0072] Table 3 Wear resistance test results
[0073] project Wear spot diameter (mm) Example 1 0.569 Example 2 0.577 Example 3 0.588 Example 4 0.586 Comparative Example 1 0.648 Comparative Example 2 0.649 Comparative Example 3 0.695 Comparative Example 4 0.689 Comparative Example 5 0.671
[0074] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A stable and efficient antibacterial composition, characterized in that: Calculated by weight percentage, it includes 2.5% graphene oxide, 0.3% sodium dodecylbenzene sulfonate, 1.5% nano basic zinc carbonate, and the balance is supplemented by solvent oil; the solvent oil is white oil, and the kinematic viscosity of the white oil is 7mm 2 / s, the test temperature is 40°C; the white oil is a mixture of No. 3 white oil, No. 5 white oil and No. 7 white oil; the weight ratio of No. 3 white oil, No. 5 white oil and No. 7 white oil is 1:3:
2.
2. A method for preparing a stable and efficient antibacterial composition according to claim 1, characterized in that: The preparation method of the stable and efficient antibacterial composition comprises the following steps: mixing graphene oxide and nano basic zinc carbonate at 300° C. to obtain a mixture; and mixing the mixture, solvent oil and sodium dodecylbenzene sulfonate to obtain a stable and efficient antibacterial composition.