Curable adhesive composition and polarizing plate

By using a curable adhesive composition of maleic anhydride modified compound, (meth)acrylate compound and photopolymerization initiator in the polarizing plate, the problem of insufficient durability of the polarizing plate adhesive is solved, and moisture permeability is improved and closeness, suitable for image display devices.

CN114761839BActive Publication Date: 2024-11-15SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080080297.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2020-11-17
Publication Date
2024-11-15
Estimated Expiration
2040-11-17

AI Technical Summary

Technical Problem

In the bonding of the polarizing plate with the thermoplastic resin film, the adhesive is insufficient, resulting in high moisture permeability and poor adhesion, which affects the stability of the image display device.

Method used

The curable adhesive composition containing maleic anhydride modified compound, (meth)acrylate compound and photopolymerization initiator is used to form an adhesive layer to ensure good bond between the polarizer and the thermoplastic resin film and reduce moisture permeability. And improve the adhesion.

Benefits of technology

It has achieved improved durability, reduced moisture permeability and enhanced adhesion of the polarizing plate, and is suitable for image display devices such as liquid crystal display devices and organic EL display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114761839B_ABST
    Figure CN114761839B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a polarizing plate having good durability and comprising a polarizer, an adhesive layer and a thermoplastic resin film in sequence. The present invention provides a polarizing plate, which comprises a polarizer, an adhesive layer and a thermoplastic resin film in sequence, wherein the adhesive layer is a cured layer of a curable adhesive composition comprising a maleic anhydride modified compound (A), a (meth)acrylate compound (B) and a photopolymerization initiator (C). The curable adhesive composition may further comprise a petroleum resin (D).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable adhesive composition and a polarizing plate. Background Art

[0002] Polarizing plates widely used in image display devices represented by liquid crystal display devices and organic EL display devices usually have a structure in which a thermoplastic resin film such as a protective film is laminated on one or both sides of a polarizer. When laminating the polarizer and the thermoplastic resin film, an adhesive is usually used. As the adhesive, active energy ray curable adhesives and water-based adhesives are known (for example, Japanese Patent Publication No. 2009-008860 (Patent Document 1)).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-008860 Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of the present invention is to provide a polarizing plate having excellent durability, which includes a polarizer, an adhesive layer, and a thermoplastic resin film in this order.

[0008] Means for solving problems

[0009] The present invention provides the polarizing plate and curable adhesive composition shown below.

[0010] [1] A polarizing plate comprising, in order, a polarizer, an adhesive layer and a thermoplastic resin film,

[0011] The adhesive layer is a cured product layer of a curable adhesive composition containing a maleic anhydride-modified compound (A), a (meth)acrylate compound (B), and a photopolymerization initiator (C).

[0012] [2] The polarizing plate according to [1], wherein the (meth)acrylate compound (B) contains a monofunctional (meth)acrylate compound (B-1).

[0013] [3] The polarizing plate according to [2], wherein in the curable adhesive composition, the content of the monofunctional (meth)acrylate compound (B-1) is 60% by mass or more in 100% by mass of the (meth)acrylate compound (B).

[0014] [4] The polarizing plate according to [3], wherein in the curable adhesive composition, the content of the monofunctional (meth)acrylate compound (B-1) is 99% by mass or less in 100% by mass of the (meth)acrylate compound (B).

[0015] [5] The polarizing plate according to any one of [2] to [4], wherein the monofunctional (meth)acrylate compound (B-1) contains at least one compound selected from alicyclic alkyl (meth)acrylate compounds and aromatic (meth)acrylate compounds.

[0016] [6] The polarizing plate according to any one of [1] to [5], wherein the curable adhesive composition further contains a petroleum resin (D).

[0017] [7] The polarizing plate according to any one of [1] to [6], wherein the maleic anhydride-modified compound (A) comprises a maleic anhydride-modified polymer (A-1).

[0018] [8] A polarizing plate according to any one of [1] to [7], wherein a cured film of the curable adhesive composition having a thickness of 10 μm has a relative humidity of 90% and a relative humidity of 400 g / (m 2 · 24hr) or less.

[0019] [9] A polarizing plate according to any one of [1] to [8], wherein the laminate of a (meth)acrylic resin film having a thickness of 60 μm and a cured film having a thickness of 10 μm comprising the curable adhesive composition has a relative humidity of 55 g / (m 2 · 24hr) or less.

[0020]

[10] The polarizing plate according to any one of [1] to [9], wherein the thermoplastic resin film is a (meth)acrylic resin film.

[0021]

[11] The polarizing plate according to any one of [1] to

[10] , wherein the adhesive layer has a thickness of 2 μm to 50 μm.

[0022]

[12] A curable adhesive composition comprising a maleic anhydride-modified compound (A), a (meth)acrylate compound (B), a photopolymerization initiator (C) and a petroleum resin (D),

[0023] The (meth)acrylate compound (B) includes a monofunctional (meth)acrylate compound (B-1).

[0024]

[13] The curable adhesive composition according to

[12] , wherein a cured film having a thickness of 10 μm comprising the curable adhesive composition has a hardness of 400 g / (m 2 · 24hr) or less.

[0025]

[14] A polarizing plate comprising, in order, a polarizer, an adhesive layer and a thermoplastic resin film,

[0026] The adhesive layer is a cured product layer of the curable adhesive composition described in

[12] or

[13] .

[0027] Effects of the Invention

[0028] A polarizing plate having excellent durability and including a polarizer, an adhesive layer, and a thermoplastic resin film in this order can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic cross-sectional view showing an example of the layer structure of the polarizing plate of the present invention.

[0030] Figure 2 This is a schematic cross-sectional view showing another example of the layer structure of the polarizing plate of the present invention. DETAILED DESCRIPTION

[0031] <Curable Adhesive Composition>

[0032] The curable adhesive composition of the present invention (hereinafter also referred to as "adhesive composition") is suitable for bonding thermoplastic resin films, for example, it can be used for bonding a thermoplastic resin film to another thermoplastic resin film (or layer). One example of the application of the adhesive composition of the present invention is for polarizing plates, that is, it can be used to make polarizing plates. More specifically, the adhesive composition of the present invention is useful as an adhesive composition used in bonding a polarizer to a thermoplastic resin film.

[0033] The so-called polarizing plate in this specification refers to a laminated optical film comprising a polarizer and a thermoplastic resin film laminated on one or both sides thereof. In the polarizing plate, the polarizer and the thermoplastic resin film are laminated via an adhesive layer. The adhesive layer is a layer formed by an adhesive composition, more specifically, a cured layer of the adhesive composition.

[0034] The polarizing plate may include a film or layer other than the polarizer and the above-mentioned thermoplastic resin film.

[0035] The adhesive composition is a curable adhesive composition comprising a maleic anhydride-modified compound (A), a (meth)acrylate compound (B) and a photopolymerization initiator (C). The adhesive composition may also contain components other than the maleic anhydride-modified compound (A), the (meth)acrylate compound (B) and the photopolymerization initiator (C).

[0036] In addition, the compounds exemplified as the components contained or capable of being contained in the adhesive composition in the present specification may be used alone or in combination of two or more unless otherwise specified.

[0037] [1] Maleic anhydride modified compound (A)

[0038] The maleic anhydride-modified compound (A) is a compound containing a maleic anhydride structure in the molecule. The adhesive composition may contain one maleic anhydride-modified compound (A) or two or more maleic anhydride-modified compounds (A).

[0039] Examples of the maleic anhydride-modified compound (A) include maleic anhydride-modified polymers (A-1).

[0040] The maleic anhydride-modified polymer (A-1) is a polymer modified by introducing a maleic anhydride structure as a side chain of the polymer. The adhesive composition may contain one maleic anhydride-modified polymer (A-1) or two or more maleic anhydride-modified polymers (A-1).

[0041] The maleic anhydride structure mentioned above refers to the following structure.

[0042] [Chemistry 1]

[0043]

[0044] (* indicates the end bonded to the main chain.)

[0045] Among the maleic anhydride-modified polymers (A-1), examples of polymers modified with maleic anhydride include diene polymers, polyolefin polymers, (meth)acrylic polymers, polyester polymers, polystyrene polymers, polyether polymers, etc. These polymers may be homopolymers formed from one monomer or copolymers formed from two or more monomers.

[0046] The term "(meth)acrylic" as used herein means at least one selected from acrylic and methacrylic groups. The same applies to expressions such as "(meth)acryloyl" and "(meth)acrylate".

[0047] The maleic anhydride-modified polymer (A-1) is preferably in a liquid state because a solvent-free adhesive composition having good adhesiveness can be prepared. The liquid state means that the polymer exhibits fluidity at a temperature of 25°C.

[0048] The viscosity of the liquid maleic anhydride-modified polymer (A-1) at 25°C is preferably 10 Pa·sec or more and 10,000 Pa·sec or less, more preferably 15 Pa·sec or more and 7,000 Pa·sec or less, further preferably 15 Pa·sec or more and 300 Pa·sec or less, and particularly preferably 15 Pa·sec or more and 100 Pa·sec or less, from the viewpoint of obtaining an adhesive composition having good coating properties.

[0049] A preferred example of the liquid maleic anhydride-modified polymer (A-1) is maleic anhydride-modified polybutadiene. These polymers may be homopolymers or copolymers, and are preferably homopolymers.

[0050] The number average molecular weight of the maleic anhydride-modified polymer (A-1) is usually 500 to 15,000, preferably 600 to 12,000, more preferably 700 to 10,000, further preferably 2,000 to 10,000, particularly preferably 3,500 to 10,000, from the viewpoint of viscosity and coating properties.

[0051] The number average molecular weight of the maleic anhydride-modified polymer (A-1) can be measured as a standard polystyrene conversion value based on gel permeation chromatography (GPC).

[0052] The acid value of the maleic anhydride modified polymer (A-1) is usually 10KOHmg / g or more and 200KOHmg / g or less. From the viewpoint of the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer), it is preferably 15KOHmg / g or more and 150KOHmg / g or less, more preferably 20KOHmg / g or more and 100KOHmg / g or less, further preferably 30KOHmg / g or more and 100KOHmg / g or less, and particularly preferably 45KOHmg / g or more and 100KOHmg / g or less. If a maleic anhydride modified polymer (A-1) having an acid value in this range is used, it is advantageous in improving the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer), and is particularly advantageous in providing an adhesive composition having high adhesion between the polyvinyl alcohol-based polarizer and the thermoplastic resin film when a polyvinyl alcohol-based polarizer is used as the polarizer.

[0053] The acid value of the maleic anhydride-modified polymer (A-1) was measured by a neutralization titration method using phenolphthalein as an indicator in accordance with JIS K 0070:1992.

[0054] When the total amount of the adhesive composition is set to 100 mass %, the content of the maleic anhydride modified compound (A) is usually 3 mass % or more and 40 mass % or less. From the viewpoint of improving the adhesion of the adhesive composition to the thermoplastic resin film (or layer), especially when a polyvinyl alcohol-based polarizer is used as the polarizer, from the viewpoint of improving the adhesion between the polyvinyl alcohol-based polarizer and the thermoplastic resin film, it is preferably 5 mass % or more and 35 mass % or less, and more preferably 10 mass % or more and 30 mass % or less.

[0055] [2] (Meth)acrylate compound (B)

[0056] The (meth)acrylate compound (B) is a radical polymerizable compound having one or more (meth)acryloyloxy groups in the molecule.

[0057] The adhesive composition may contain one or two or more (meth)acrylate compounds (B).

[0058] Examples of the (meth)acrylate compound (B) include a monofunctional (meth)acrylate compound (B-1) having one (meth)acryloyloxy group in the molecule, a bifunctional (meth)acrylate compound (B-2) having two (meth)acryloyloxy groups in the molecule, and a polyfunctional (meth)acrylate compound (B-3) having three or more (meth)acryloyloxy groups in the molecule.

[0059] The (meth)acrylate compound (B) may contain one or more of the monofunctional (meth)acrylate compound (B-1), the bifunctional (meth)acrylate compound (B-2), and the polyfunctional (meth)acrylate compound (B-3).

[0060] An example of the monofunctional (meth)acrylate compound (B-1) is an alkyl (meth)acrylate. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0061] Other examples of the monofunctional (meth)acrylate compound (B-1) include compounds other than the above compounds, which are the following compounds:

[0062] Aryl (meth)acrylate esters such as benzyl (meth)acrylate, and phenoxy (meth)acrylate esters such as 2-phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and ethoxylated-o-phenylphenol (meth)acrylate, aromatic (meth)acrylate compounds containing an aromatic ring in the group bonded to the -O- of the ester bond (-C(=O)-O-);

[0063] Alicyclic alkyl (meth)acrylate compounds containing an alicyclic ring in the group bonded to the -O- of the ester bond (-C(=O)-O-), such as cyclohexyl (meth)acrylate, cyclohexylmethyl (meth)acrylate, dicyclopentyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, and isobornyl (meth)acrylate;

[0064] (Meth)acrylic acid aminoalkyl ester compounds such as N,N-dimethylaminoethyl acrylate;

[0065] (meth)acrylate compounds including an ether bond in the -O- bonded group of the ester bond (-C(=O)-O-) such as dicyclopentadienyloxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.

[0066] Other examples of the monofunctional (meth)acrylate compound (B-1) include:

[0067] (meth)acrylate compounds containing a hydroxyl group in the group bonded to —O— of the ester bond (—C(═O)—O—), such as 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, and pentaerythritol mono(meth)acrylate;

[0068] (Meth)acrylate 2-carboxyethyl, ω-carboxy-polycaprolactone (n≈2) mono(meth)acrylate, 1-[2-(meth)acryloyloxyethyl]phthalate, 1-[2-(meth)acryloyloxyethyl]hexahydrophthalate, 1-[2-(meth)acryloyloxyethyl]succinate, 4-[2-(meth)acryloyloxyethyl]trimellitate, N-(meth)acryloyloxy-N',N'-dicarboxymethyl-p-phenylenediamine, and the like, wherein the group bonded to -O- of the ester bond (-C(=O)-O-) contains a carboxyl group, and the like.

[0069] Examples of the bifunctional (meth)acrylate compound (B-2) include alkylene glycol di(meth)acrylates, polyoxyalkylene glycol di(meth)acrylates, halogen-substituted alkylene glycol di(meth)acrylates, di(meth)acrylates of aliphatic polyols, di(meth)acrylates of hydrogenated dicyclopentadiene or tricyclodecanediol, di(meth)acrylates of dioxanediol or dioxanediol, di(meth)acrylates of alkylene oxide adducts of bisphenol A or bisphenol F, and epoxy di(meth)acrylates of bisphenol A or bisphenol F.

[0070] More specific examples of the bifunctional (meth)acrylate compound (B-2) include ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol di(meth)acrylate, ester, di(trimethylolpropane) di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly-1,4-butylene glycol di(meth)acrylate, silicone di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol ester, 2,2-bis[4-(meth)acryloyloxyethoxyethoxyphenyl]propane, 2,2-bis[4-(meth)acryloyloxyethoxyethoxycyclohexyl]propane, hydrogenated biscyclopentadienyl di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-dioxane-2,5-diyl di(meth)acrylate [alias: dioxanediol di(meth)acrylate], hydroxypivalaldehyde and trimethylolpropane Acetal compound [chemical name: 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane] di(meth)acrylate, tris(hydroxyethyl)isocyanurate di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, propoxylated bisphenol F di(meth)acrylate, etc.

[0071] The bifunctional (meth)acrylate (B-2) preferably has at least one alicyclic skeleton or at least one aromatic ring in the molecule, and more preferably has at least one aromatic ring.

[0072] From the viewpoints of moisture permeability of the cured product, compatibility with the maleic anhydride-modified compound (A), and adhesion to a resin film (particularly a (meth)acrylic resin film), the bifunctional (meth)acrylate (B-2) preferably contains a compound represented by the following formula, and more preferably a compound represented by the following formula.

[0073] [Chemistry 21

[0074]

[0075] (In the formula, R1 and R2 each independently represent a hydrogen atom or a methyl group, X represents an ethyleneoxy group (-C2H4O-) or a propyleneoxy group (-C3H6O-), n represents an integer of 1 to 20, and m represents an integer of 1 to 20.)

[0076] X is preferably an ethyleneoxy group. The average of the total of m and n is preferably 2-20, more preferably 3-15, and particularly preferably 4-13.

[0077] Examples of the polyfunctional (meth)acrylate compound (B-3) having three or more (meth)acryloyloxy groups in the molecule include poly(meth)acrylates of trifunctional or higher aliphatic polyols such as glycerol tri(meth)acrylate, alkoxylated glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate.

[0078] Poly(meth)acrylates of halogen-substituted polyols having three or more functional groups;

[0079] Tri(meth)acrylates of alkylene oxide adducts of glycerol;

[0080] Tri(meth)acrylate of alkylene oxide adduct of trimethylolpropane;

[0081] 1,1,1-Tris[(meth)acryloyloxyethoxyethoxy]propane;

[0082] Tris(hydroxyethyl)isocyanurate tri(meth)acrylate, etc.

[0083] From the viewpoint of reducing the viscosity of the adhesive composition and the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer), the (meth)acrylate compound (B) preferably contains a monofunctional (meth)acrylate compound (B-1).

[0084] From the viewpoint of reducing the viscosity of the adhesive composition and the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer), the monofunctional (meth)acrylate compound (B-1) preferably contains at least one compound selected from alicyclic alkyl (meth)acrylate compounds and aromatic (meth)acrylate compounds. Among them, from the viewpoint of reducing the moisture permeability (hereinafter sometimes referred to as low moisture permeability) of the cured film formed from the adhesive composition, alicyclic alkyl (meth)acrylate compounds are more preferred.

[0085] When the total amount of the adhesive composition is 100 mass %, the content of the (meth)acrylate compound (B) is usually 15 mass % to 75 mass %, and from the viewpoint of the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer), it is preferably 15 mass % to 70 mass %, more preferably 20 mass % to 60 mass %, and further preferably 30 mass % to 55 mass %.

[0086] When the total amount of the (meth)acrylate compound (B) is 100% by mass, the content of the monofunctional (meth)acrylate compound (B-1) is usually 60% by mass or more, and is preferably 70% by mass or more, and more preferably 80% by mass or more, from the viewpoint of the adhesive ability of the adhesive composition to the thermoplastic resin film (or layer).

[0087] When the total amount of the (meth)acrylate compound (B) is set to 100 mass %, the content of the monofunctional (meth)acrylate compound (B-1) can be 100 mass %, but from the viewpoint of the mechanical strength of the cured product of the adhesive composition and further from the viewpoint of the mechanical strength of the polarizing plate produced using the adhesive composition, it is preferably 99 mass % or less, more preferably 98 mass % or less, and can also be 90 mass % or less.

[0088] When the content of the monofunctional (meth)acrylate compound (B-1) is less than 100% by mass, the remainder of the (meth)acrylate compound (B) is a bifunctional (meth)acrylate compound (B-2) and / or a polyfunctional (meth)acrylate compound (B-3), preferably containing a bifunctional (meth)acrylate compound (B-2).

[0089] When the total amount of the (meth)acrylate compound (B) is 100 mass %, the content of the bifunctional (meth)acrylate compound (B-2) is preferably 0.5 mass % or more, more preferably 1 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less.

[0090] 〔3〕Photopolymerization initiator (C)

[0091] The photopolymerization initiator (C) is not particularly limited as long as it is a compound that generates active radicals, an acid, etc. by the action of light and initiates polymerization of the (meth)acrylate compound (B).

[0092] The adhesive composition may contain only one type of photopolymerization initiator (C), or may contain two or more types.

[0093] The photopolymerization initiator (C) is not particularly limited, and examples thereof include oxime compounds such as O-acyl oxime compounds, alkyl phenyl ketone compounds, and acyl phosphine oxide compounds.

[0094] The O-acyl oxime compound is a compound having a structure represented by the following formula (d): Hereinafter, * represents a bonding end.

[0095] [Chemistry 3]

[0096]

[0097] Examples of the O-acyl oxime compound include N-benzoyloxy-1-(4-phenylsulfanylphenyl)butane-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octane-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine, N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxolanylmethoxy)benzoyl}-9H-carbazole-3 -yl]ethane-1-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-3-cyclopentylpropane-1-imine, N-benzoyloxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[4-(2-hydroxyethoxy)phenylsulfanylphenyl]propane-1-one-2-imine, N-acetoxy-1-[4-(1-methyl-2-methoxyethoxy)-2-methylphenyl]-1-(9-ethyl-6-nitro-9H-carbazole-3-yl)methane-1-imine, and the like.

[0098] Commercially available products such as Irgacure (trade name) OXE01, Irgacure OXE02, Irgacure OXE03 (all manufactured by BASF), N-1919, NCI-930, and NCI-831 (all manufactured by ADEKA) can also be used.

[0099] The alkyl phenyl ketone compound is a compound having a partial structure represented by the following formula (d4) or a partial structure represented by the following formula (d5). In these partial structures, the benzene ring may have a substituent.

[0100] [Chemistry 4]

[0101]

[0102] Examples of the compound having a structure represented by formula (d4) include 2-methyl-2-morpholinyl-1-(4-methylsulfanylphenyl)propane-1-one, 2-dimethylamino-1-(4-morpholinylphenyl)-2-benzylbutane-1-one, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]butane-1-one.

[0103] Commercially available products such as Omnirad (trade name) 369, Omnirad 907, and Omnirad 379 (all manufactured by IGM Resins B.V.) may also be used.

[0104] Examples of the compound having a structure represented by formula (d5) include 2-hydroxy-2-methyl-1-phenylpropane-1-one, 2-hydroxy-2-methyl-1-〔4-(2-hydroxyethoxy)phenyl〕propane-1-one, 1-hydroxycyclohexyl phenyl ketone, oligomers of 2-hydroxy-2-methyl-1-(4-isopropenylphenyl)propane-1-one, α,α-diethoxyacetophenone, and benzyl dimethyl ketal.

[0105] Commercially available products such as Omnirad (trade name) 184 (manufactured by IGM Resins BV) may also be used.

[0106] Examples of the acylphosphine oxide compound include phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (for example, trade name "Omnirad 819" (manufactured by IGM Resins BV)) and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0107] Further examples of the photopolymerization initiator (C) include:

[0108] Benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether and benzoin isobutyl ether;

[0109] Benzophenone compounds such as benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetrakis(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, and 4,4'-bis(N,N'-dimethylamino)-benzophenone;

[0110] Xanthenone compounds such as 2-isopropylthioxanthone and 2,4-diethylthioxanthone;

[0111] Anthracene compounds such as 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, and 2-ethyl-9,10-diethoxyanthracene;

[0112] Quinone compounds such as 9,10-phenanthrenequinone, 2-ethylanthraquinone, and camphorquinone;

[0113] Diphenylmethane, methyl phenylglyoxylate, titanocene compounds, etc.

[0114] When the total amount of the adhesive composition is set to 100 mass %, the content of the photopolymerization initiator (C) is usually 0.1 mass % to 20 mass %, and is preferably 0.5 mass % to 15 mass %, and more preferably 1 mass % to 10 mass % (for example, 8 mass % or less) from the viewpoint of the curability of the adhesive composition and the adhesion ability of the adhesive composition to the thermoplastic resin film (or layer).

[0115] When the total amount of the (meth)acrylate compound (B) is 100 parts by mass, the content of the photopolymerization initiator (C) is usually 0.1 parts by mass or more and 30 parts by mass or less, and is preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less, from the viewpoint of the curability of the adhesive composition and the adhesion ability of the adhesive composition to the thermoplastic resin film (or layer).

[0116] 〔4〕Petroleum resin (D)

[0117] The adhesive composition may further contain a petroleum resin (D). When the adhesive composition further contains a petroleum resin (D), the moisture permeability of a cured film formed from the adhesive composition can be reduced.

[0118] The adhesive composition that can form a cured film with low moisture permeability is suitable for applications that require the suppression of the entry and exit of water through the cured film. For example, in a polarizing plate or an image display panel including the polarizing plate in which at least one surface of the polarizer is laminated with a thermoplastic resin film via an adhesive layer, if the adhesive layer has low moisture permeability, the curling (warping) of the polarizing plate or the image display panel caused by the entry and exit of water can be suppressed.

[0119] When the adhesive composition further contains a petroleum resin (D), it can be advantageous in improving the adhesion between the polarizer and the thermoplastic resin film.

[0120] Examples of the petroleum resin (D) include aromatic petroleum resins, aliphatic petroleum resins, cycloaliphatic petroleum resins, aliphatic-aromatic petroleum resins, coumarone-based resins, etc. In addition, examples include resins obtained by hydrogenating these resins.

[0121] The aromatic petroleum resin is a resin containing one or more constituent units derived from aromatic hydrocarbons, and may be a resin obtained by hydrogenating the resin or a resin obtained by modifying the resin.

[0122] The aromatic petroleum resin is preferably a C9 petroleum resin. The C9 petroleum resin is a resin obtained by copolymerizing a C9 fraction, and may be a resin obtained by hydrogenating the resin or a resin obtained by modifying the resin.

[0123] The C9 petroleum resin may be a resin obtained by copolymerizing a C9 fraction with other monomer components, a resin obtained by hydrogenating the resin, or a resin obtained by modifying the resin. As other monomer components, a C5 fraction may be mentioned.

[0124] Examples of the C9 fraction include petroleum fractions having about 8 to 10 carbon atoms, such as styrene, alkylstyrene, vinyltoluene, 1-methyl-1-phenylethylene, indene, and methylindene.

[0125] Examples of the C5 fraction include petroleum fractions having about 4 to 5 carbon atoms, such as cyclopentadiene, pentene, pentadiene, and piperylene.

[0126] In addition, the petroleum resin (D) may be a C5-based petroleum resin obtained by copolymerizing the above-mentioned C5 fraction, a resin obtained by hydrogenating the C5-based petroleum resin, or a resin obtained by modifying the resin. In addition, it may be an alicyclic hydrocarbon resin obtained by polymerizing the C5 fraction after cyclodimerization. Examples of the alicyclic hydrocarbon resin include polymers containing constituent units derived from dicyclopentadiene.

[0127] The weight average molecular weight of the petroleum resin (D) is usually 500 to 10,000, preferably 500 to 7,000, more preferably 600 to 5,000, further preferably 600 to 3,000, and particularly preferably 600 to 1,500, from the viewpoint of reducing the moisture permeability of the cured film formed from the adhesive composition and the adhesion of the adhesive composition to the thermoplastic resin film (or layer).

[0128] The weight average molecular weight of the petroleum resin (D) can be measured as a standard polystyrene conversion value based on gel permeation chromatography (GPC).

[0129] When the adhesive composition contains a petroleum resin (D), when the total amount of the adhesive composition is set to 100 mass %, the content of the petroleum resin (D) is preferably 20 mass % or more and 70 mass % or less, and more preferably 30 mass % or more and 65 mass % or less, from the viewpoint of reducing the moisture permeability of a cured film formed from the adhesive composition and from the viewpoint of the adhesion ability of the adhesive composition to a thermoplastic resin film (or layer), and particularly when a polyvinyl alcohol-based polarizer is used as a polarizer, from the viewpoint of improving the adhesion between the polyvinyl alcohol-based polarizer and the thermoplastic resin film.

[0130] When the adhesive composition contains a monofunctional (meth)acrylate compound (B-1) and a petroleum resin (D), the mass ratio thereof (monofunctional (meth)acrylate compound (B-1) / petroleum resin (D)) is preferably 0.5 to 3.0, more preferably 0.7 to 2.0, further preferably 0.9 to 1.5, and even more preferably 1.0 to 1.3, from the viewpoint of reducing the moisture permeability of a cured film formed from the adhesive composition and from the viewpoint of the adhesion ability of the adhesive composition to a thermoplastic resin film (or layer), and particularly when a polyvinyl alcohol-based polarizer is used as a polarizer, from the viewpoint of improving the adhesion between the polyvinyl alcohol-based polarizer and the thermoplastic resin film.

[0131] The moisture permeability of the cured film formed from the adhesive composition is preferably low. For a cured film having a thickness of 10 μm including the adhesive composition, the moisture permeability measured by the cup method specified in JIS Z 0208 at a temperature of 40° C. and a relative humidity of 90% is preferably 400 g / (m 2 ·24hr) or less, more preferably 300g / (m 2 ·24hr) or less, more preferably 200g / (m 2 ·24hr) or less. The moisture permeability is usually 1g / (m 2 ·24hr) or more, for example, 5g / (m 2 ·24hr) or more.

[0132] Specifically, the moisture permeability J of a cured film composed of an adhesive composition can be determined by preparing a laminate having the cured film formed on a substrate film having a known moisture permeability, measuring the moisture permeability of the laminate by the above method, and using the measurement results based on the following formula.

[0133] 1 / Jt=(1 / J)+(1 / Jsub)

[0134] In the above formula, Jt is the moisture permeability of the above-mentioned laminate, and Jsub is the moisture permeability of the above-mentioned base film. As the base film, the same base film as the thermoplastic resin film described later can be used. When the moisture permeability of the laminate is measured in accordance with JIS Z 0208, the laminate is installed in a cup with the above-mentioned cured film facing outward.

[0135] In the case where a (meth)acrylic resin film having a thickness of 60 μm is used as the substrate film, for example, the laminate of the (meth)acrylic resin film and a cured film having a thickness of 10 μm containing the adhesive composition preferably has a moisture permeability of 55 g / (m 2 ·24hr) or less, more preferably 50g / (m 2 ·24hr) or less. The moisture permeability is usually 1g / (m 2 ·24hr) or more, for example, 5g / (m 2 ·24hr) or more.

[0136] 〔5〕Other ingredients

[0137] The adhesive composition may contain other components besides the above.

[0138] Examples of other components include curable components other than the (meth)acrylate compound (B), crosslinking agents, coupling agents, tackifiers, antioxidants, ultraviolet absorbers, thermal stabilizers and other additives.

[0139] [6] Viscosity of adhesive composition

[0140] The viscosity of the adhesive composition at 25°C is preferably 10000 mPa·sec or less, more preferably 2 mPa·sec or more and 7000 mPa·sec or less, and further preferably 4 mPa·sec or more and 5000 mPa·sec or less. In one embodiment, it is preferably 100 mPa·sec or more and 5000 mPa·sec or less, more preferably 100 mPa·sec or more and 4000 mPa·sec or less, and further preferably 100 mPa·sec or more and 3000 mPa·sec or less.

[0141] The viscosity of the adhesive composition at 25° C. can be measured using an E-type viscometer.

[0142] The adhesive composition preferably contains substantially no solvent (solvent-free adhesive composition). The term "substantially contains no solvent" means that the amount of solvent in the adhesive composition is 3% by mass or less, preferably 1% by mass or less, and more preferably 0.5% by mass or less. By making the adhesive composition substantially free of solvent, for example, when bonding two films, a solvent drying process is not required, productivity is improved, and degradation of the substrate caused by the solvent can also be suppressed.

[0143] When the adhesive composition contains substantially no solvent, the viscosity of the adhesive composition at 25°C is generally greater than 100 mPa·sec and less than 7000 mPa·sec, preferably greater than 500 mPa·sec and less than 5000 mPa·sec, more preferably greater than 1000 mPa·sec and less than 4000 mPa·sec, and further preferably greater than 1500 mPa·sec and less than 3500 mPa·sec.

[0144] <Polarizing Plate>

[0145] The adhesive composition of the present invention is suitable for bonding thermoplastic resin films, for example, it can be used for bonding a thermoplastic resin film to another thermoplastic resin film (or layer). One example of the application of the adhesive composition of the present invention is for polarizing plates, that is, it can be used to make polarizing plates. More specifically, the adhesive composition of the present invention is useful as an adhesive composition used in bonding a polarizer to a thermoplastic resin film such as a protective film laminated thereon.

[0146] The polarizing plate of the present invention comprises a polarizer and a thermoplastic resin film laminated on at least one surface of the polarizer via an adhesive layer formed from the adhesive composition. The adhesive layer is a cured product layer of the adhesive composition.

[0147] In the polarizing plate of the present invention, since the polarizer and the thermoplastic resin film are bonded together using the adhesive composition, the adhesion between the polarizer and the thermoplastic resin film can be improved, thereby improving the durability of the polarizing plate.

[0148] The polarizing plate of the present invention can be suitably used in image display devices such as liquid crystal display devices and organic EL devices.

[0149] [1] Structure of polarizing plate

[0150] Examples of the layer constitution of the polarizing plate of the present invention are shown in Figure 1 and Figure 2 middle.

[0151] like Figure 1As shown, the polarizing plate of the present invention may include a polarizer 30, a first adhesive layer 15, and a first thermoplastic resin film 10 in this order, that is, may include a polarizer 30 and the first thermoplastic resin film 10 laminated and bonded on one surface thereof via the first adhesive layer 15.

[0152] It is preferred that the first adhesive layer 15 and the first thermoplastic resin film 10 are in direct contact with each other.

[0153] The polarizing plate 30 and the first adhesive layer 15 are preferably in direct contact with each other.

[0154] In addition, you can also Figure 2 As shown, the polarizing plate of the present invention includes a polarizer 30 , a first thermoplastic resin film 10 laminated on one surface thereof via a first adhesive layer 15 , and a second thermoplastic resin film 20 laminated on the other surface of the polarizer 30 via a second adhesive layer 25 .

[0155] It is preferred that the first adhesive layer 15 and the first thermoplastic resin film 10 are in direct contact with each other.

[0156] The polarizing plate 30 and the first adhesive layer 15 are preferably in direct contact with each other.

[0157] It is preferred that the second adhesive layer 25 and the second thermoplastic resin film 20 are in direct contact with each other.

[0158] The polarizing plate 30 and the second adhesive layer 25 are preferably in direct contact with each other.

[0159] When the polarizing plate has the first adhesive layer 15 and the second adhesive layer 25, either one of them may be formed by the adhesive composition of the present invention, or both adhesive layers may be formed by the adhesive composition of the present invention. The adhesive layer formed by the adhesive composition of the present invention is preferably the adhesive layer on the visible side (the adhesive layer away from the adhesive layer described later).

[0160] When both adhesive layers are formed from the adhesive composition of the present invention, the adhesive compositions may have the same composition or different compositions.

[0161] Not limited to Figure 1 and Figure 2For example, the polarizing plate of the present invention may include other layers (or films) other than those mentioned above. As other layers, for example, there can be cited an adhesive layer laminated on the outer surface of the first thermoplastic resin film 10, the second thermoplastic resin film 20 and / or the polarizer 30; a separator (also called a "peeling film") laminated on the outer surface of the adhesive layer; a protective film (also called a "surface protection film") laminated on the outer surface of the first thermoplastic resin film 10, the second thermoplastic resin film 20 and / or the polarizer 30; an optically functional film (or layer) laminated on the outer surface of the first thermoplastic resin film 10, the second thermoplastic resin film 20 and / or the polarizer 30 via an adhesive layer and an adhesive layer, etc.

[0162] 〔2〕Polarizing film

[0163] The polarizer 30 is a film having the function of selectively transmitting linear polarized light in a certain direction from natural light. Examples of the polarizer 30 include an iodine-based polarizer obtained by adsorbing iodine as a dichroic pigment to a polyvinyl alcohol resin film and orienting it, a dye-based polarizer obtained by adsorbing a dichroic dye as a dichroic pigment to a polyvinyl alcohol resin film and orienting it, and a coating-type polarizer obtained by coating a dichroic dye in a lyotropic liquid crystal state and orienting and fixing it. These polarizers are called absorption-type polarizers because they selectively transmit linear polarized light in a certain direction from natural light and absorb linear polarized light in another direction.

[0164] The polarizer 30 is not limited to an absorption-type polarizer, but may also be a reflection-type polarizer that selectively transmits linear polarized light in a certain direction from natural light and reflects linear polarized light in another direction, or a scattering-type polarizer that scatters linear polarized light in another direction. However, from the perspective of excellent visibility when the polarizing plate is applied to an image display device, etc., an absorption-type polarizer is preferred.

[0165] Among them, the polarizer 30 is more preferably a polyvinyl alcohol polarizer formed by a polyvinyl alcohol resin, further preferably a polyvinyl alcohol polarizer obtained by allowing a polyvinyl alcohol resin film to adsorb dichroic pigments such as iodine and dichroic dyes and orient them, and particularly preferably a polyvinyl alcohol polarizer obtained by allowing a polyvinyl alcohol resin film to adsorb iodine and orient them.

[0166] The polyvinyl alcohol-based polarizing plate can be produced by a conventionally known method using a polyvinyl alcohol-based resin film (or layer).

[0167] The thickness of the polarizer 30 can be set to 30 μm or less, preferably 25 μm or less (for example, preferably 20 μm or less, more preferably 15 μm or less, more preferably 10 μm or less, and more preferably 8 μm or less). The thickness of the polarizer 30 is usually 2 μm or more. Reducing the thickness of the polarizer 30 is conducive to the thinning of the polarizing plate, and then the image display device using the polarizing plate.

[0168] 〔3〕Thermoplastic resin film

[0169] The first thermoplastic resin film 10 and the second thermoplastic resin film 20 can be light-transmitting (preferably optically transparent) films containing thermoplastic resins, for example, films containing polyolefin resins such as chain polyolefin resins (polyethylene resins, polypropylene resins, etc.), cyclic polyolefin resins (norbornene resins, etc.); cellulose ester resins such as triacetyl cellulose and diacetyl cellulose; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resins; (meth) acrylic resins; or mixtures, copolymers, etc. thereof.

[0170] The first thermoplastic resin film 10 and the second thermoplastic resin film 20 may be either unstretched films or uniaxially or biaxially stretched films. The biaxial stretching may be simultaneous biaxial stretching in which the film is stretched in two stretching directions at the same time, or sequential biaxial stretching in which the film is stretched in a first direction and then in a second direction different from the first direction.

[0171] The first thermoplastic resin film 10 and / or the second thermoplastic resin film 20 may be a protective film that plays a role in protecting the polarizing plate 30 , or may be a protective film having an optical function such as a retardation film.

[0172] For example, a retardation film having an arbitrary retardation value can be produced by stretching a film made of the above-mentioned thermoplastic resin (uniaxial stretching or biaxial stretching, etc.) or forming a liquid crystal layer on the thermoplastic resin film.

[0173] The (meth)acrylic resin may be, for example, a polymer containing methacrylate as a main monomer (containing 50% by mass or more), and is preferably a copolymer of methacrylate and other copolymerization components.

[0174] In one embodiment, the (meth)acrylic resin contains methyl methacrylate as a copolymerization component, or contains methyl methacrylate and methyl acrylate as copolymerization components.

[0175] Examples of other copolymer components other than methyl acrylate include methacrylate esters other than methyl methacrylate such as ethyl methacrylate, n-, iso- or tert-butyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, benzyl methacrylate, 2-ethylhexyl methacrylate and 2-hydroxyethyl methacrylate;

[0176] Acrylates such as ethyl acrylate, n-butyl acrylate, iso-butyl acrylate or tert-butyl acrylate, cyclohexyl acrylate, phenyl acrylate, benzyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, etc.;

[0177] Hydroxyalkyl acrylates such as methyl 2-(hydroxymethyl)acrylate, methyl 2-(1-hydroxyethyl)acrylate, ethyl 2-(hydroxymethyl)acrylate, n-, iso- or tert-butyl 2-(hydroxymethyl)acrylate;

[0178] Unsaturated acids such as methacrylic acid and acrylic acid;

[0179] Halogenated styrenes such as chlorostyrene and bromostyrene;

[0180] Substituted styrenes such as vinyltoluene and α-methylstyrene;

[0181] Unsaturated nitriles such as acrylonitrile and methacrylonitrile;

[0182] Unsaturated anhydrides such as maleic anhydride and citraconic anhydride;

[0183] Unsaturated imides such as phenylmaleimide and cyclohexylmaleimide; and other monofunctional monomers.

[0184] The above other monofunctional monomers may be used alone or in combination of two or more.

[0185] As the other copolymerization components, a polyfunctional monomer may also be used.

[0186] Examples of the polyfunctional monomer include compounds obtained by esterifying two terminal hydroxyl groups of ethylene glycol or its oligomers with (meth)acrylic acid, such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, nonaethylene glycol di(meth)acrylate, and tetradecaethylene glycol di(meth)acrylate;

[0187] A compound in which two terminal hydroxyl groups of propylene glycol or its oligomer are esterified with (meth)acrylic acid;

[0188] Compounds obtained by esterifying the hydroxyl group of a diol with (meth)acrylic acid, such as neopentyl glycol di(meth)acrylate, hexanediol di(meth)acrylate, and butanediol di(meth)acrylate;

[0189] Compounds in which both terminal hydroxyl groups of bisphenol A, alkylene oxide adducts of bisphenol A, or halogen-substituted products thereof are esterified with (meth) acrylic acid;

[0190] Compounds obtained by esterifying a polyol such as trimethylolpropane or pentaerythritol with (meth)acrylic acid, and compounds obtained by ring-opening addition of epoxy groups of glycidyl (meth)acrylate to terminal hydroxyl groups thereof;

[0191] Compounds obtained by ring-opening addition of epoxy groups of glycidyl (meth)acrylate to dibasic acids such as succinic acid, adipic acid, terephthalic acid, phthalic acid, halogen-substituted dibasic acids thereof, or alkylene oxide adducts thereof;

[0192] Aryl (meth)acrylates; aromatic divinyl compounds such as divinylbenzene; etc.

[0193] Among them, ethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and neopentyl glycol dimethacrylate are preferably used.

[0194] The (meth)acrylic resin may be a resin modified by a reaction between functional groups of the copolymer. Examples of such reactions include a polymer chain decarbinolation condensation reaction between a methyl group of methyl (meth)acrylate and a hydroxyl group of methyl 2-(hydroxymethyl)acrylate, and a polymer chain dehydration condensation reaction between a carboxyl group of (meth)acrylic acid and a hydroxyl group of methyl 2-(hydroxymethyl)acrylate.

[0195] The glass transition temperature of the (meth)acrylic resin is preferably 80° C. to 160° C. The glass transition temperature can be controlled by adjusting the polymerization ratio of the methacrylate monomer to the acrylate monomer, the carbon chain length of each ester group and the type of functional group they have, and the polymerization ratio of the multifunctional monomer to all monomers.

[0196] As a method for increasing the glass transition temperature of (meth) acrylic resin, it is also effective to introduce a ring structure into the main chain of the polymer. The ring structure is preferably a heterocyclic structure such as a cyclic anhydride structure, a cyclic imide structure and a lactone structure. Specifically, cyclic anhydride structures such as glutaric anhydride structure and succinic anhydride structure; cyclic imide structures such as glutarimide structure and succinimide structure; lactone ring structures such as butyrolactone and valerolactone can be cited.

[0197] There is a tendency that the glass transition temperature of the (meth)acrylic resin can be increased as the content of the ring structure in the main chain increases.

[0198] The cyclic anhydride structure and the cyclic imide structure can be introduced by the following methods, i.e., a method of introducing by copolymerizing a monomer having a cyclic structure such as maleic anhydride or maleimide; a method of introducing a cyclic anhydride structure by a dehydration / demethanolation condensation reaction after polymerization; a method of introducing a cyclic imide structure by reacting an amino compound.

[0199] A resin (polymer) having a lactone ring structure can be obtained by the following method, namely, after preparing a polymer having a hydroxyl group and an ester group in the polymer chain, heating and, if necessary, in the presence of a catalyst such as an organic phosphorus compound, cyclizing and condensing the hydroxyl group and the ester group in the obtained polymer to form a lactone ring structure.

[0200] The first thermoplastic resin film 10 and the second thermoplastic resin film 20 may contain additives as necessary. Examples of the additives include lubricants, anti-blocking agents, heat stabilizers, antioxidants, ultraviolet absorbers, antistatic agents, impact resistance improvers, and surfactants.

[0201] From the viewpoint of film forming properties and impact resistance of the film, the (meth)acrylic resin may contain acrylic rubber particles as an impact modifier. The acrylic rubber particles are particles having an elastic polymer as an essential component, wherein the elastic polymer is mainly composed of acrylic ester, and the acrylic rubber particles may be particles having a single-layer structure substantially formed of the elastic polymer alone, or particles having a multi-layer structure having the elastic polymer as one layer.

[0202] Examples of the elastic polymer include cross-linked elastic copolymers obtained by copolymerizing an alkyl acrylate as a main component with other vinyl monomers and cross-linking monomers copolymerizable with the alkyl acrylate.

[0203] Examples of the alkyl acrylate serving as the main component of the elastic polymer include alkyl acrylates having an alkyl group with 1 to 8 carbon atoms, such as methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. Alkyl acrylates having an alkyl group with 4 or more carbon atoms are preferably used.

[0204] Examples of other vinyl monomers copolymerizable with the above-mentioned alkyl acrylate include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylates such as methyl methacrylate; aromatic vinyl compounds such as styrene; vinyl cyanide compounds such as acrylonitrile, and the like.

[0205] Examples of the crosslinkable monomer include crosslinkable compounds having at least two polymerizable carbon-carbon double bonds in the molecule, and more specifically, (meth)acrylate esters of polyols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate; alkenyl (meth)acrylate esters such as allyl (meth)acrylate; and divinylbenzene.

[0206] At least one of the first thermoplastic resin film 10 and the second thermoplastic resin film 20 is preferably a film containing a (meth)acrylic resin (a (meth)acrylic resin film), and the (meth)acrylic resin film is preferably laminated and bonded to the polarizer 30 via an adhesive layer formed from the adhesive composition of the present invention.

[0207] The adhesive composition of the present invention can show good adhesion particularly when the thermoplastic resin film is a (meth)acrylic resin film. Therefore, the adhesive composition of the present invention can be suitably used for bonding a polarizer and a (meth)acrylic resin film.

[0208] The (meth)acrylic resin film preferably has a resin component containing a (meth)acrylic resin. The first thermoplastic resin film 10 and the second thermoplastic resin film 20 may be films formed of the same thermoplastic resin or films formed of different thermoplastic resins. The first thermoplastic resin film 10 and the second thermoplastic resin film 20 may be the same or different in thickness, presence or absence of additives, type of additives, phase difference characteristics, etc.

[0209] In one embodiment, the first thermoplastic resin film 10 is a (meth)acrylic resin film, and the second thermoplastic resin film 20 is a polyolefin resin film (preferably a cyclic polyolefin resin film), a cellulose ester resin, or a polyester resin film.

[0210] In another embodiment, the first thermoplastic resin film 10 and the second thermoplastic resin film 20 are (meth)acrylic resin films.

[0211] The first thermoplastic resin film 10 and / or the second thermoplastic resin film 20 may have a surface treatment layer (coating layer) such as a hard coat layer, an anti-glare layer, an anti-reflection layer, a light diffusion layer, an antistatic layer, an antifouling layer, or a conductive layer on its outer surface (the surface on the side opposite to the polarizer 30).

[0212] The thickness of the first thermoplastic resin film 10 and the second thermoplastic resin film 20 is usually 5 μm or more and 200 μm or less, preferably 10 μm or more and 120 μm or less, more preferably 10 μm or more and 85 μm or less, and further preferably 15 μm or more and 65 μm or less. The thickness of the first thermoplastic resin film 10 and the second thermoplastic resin film 20 may be 50 μm or less, or 40 μm or less. Reducing the thickness of the first thermoplastic resin film 10 and the second thermoplastic resin film 20 is advantageous for reducing the thickness of the polarizing plate, and further, the image display device using the polarizing plate.

[0213] The surfaces of the first thermoplastic resin film 10 and the second thermoplastic resin film 20 on which the adhesive composition is applied may be subjected to surface modification treatment such as saponification treatment, plasma treatment, corona treatment, primer treatment, etc., from the viewpoint of improving adhesion.

[0214] [4] Production of polarizing plate and adhesive layer

[0215] By laminating and bonding the first thermoplastic resin film 10 on one surface of the polarizing plate 30 via the first adhesive layer 15, a Figure 1 The polarizing plate of the structure shown in the figure can be obtained by laminating and bonding the second thermoplastic resin film 20 on the other surface of the polarizer 30 via the second adhesive layer 25. Figure 2 A polarizing plate having the structure shown.

[0216] When manufacturing a polarizing plate having both the first thermoplastic resin film 10 and the second thermoplastic resin film 20 (hereinafter, they are also simply collectively referred to as "thermoplastic resin films"), these thermoplastic resin films may be laminated and bonded one by one in stages, or the thermoplastic resin films on both sides may be laminated and bonded simultaneously.

[0217] exist Figure 1 In the polarizing plate having the structure shown, the first adhesive layer 15 is formed of the adhesive composition of the present invention. The first adhesive layer 15 is a cured product layer of the adhesive composition of the present invention.

[0218] More specifically, Figure 1 The polarizing plate having the structure shown above can be produced by a production method including the following steps (a) to (c).

[0219] (a) forming a coating layer of the adhesive composition of the present invention on at least one of the first thermoplastic resin film 10 and the polarizer 30;

[0220] (b) a step of obtaining a laminated film by laminating the first thermoplastic resin film 10 or the polarizing plate 30 via a coating layer;

[0221] (c) A step of irradiating the laminated film with active energy rays to cure the coating layer.

[0222] In the step (a), the coating layer may be formed on at least one of the first thermoplastic resin film 10 and the polarizer 30 , but it is preferred that a coating layer of the adhesive composition of the present invention is formed on the first thermoplastic resin film 10 .

[0223] The coating layer can be formed by various coating methods such as a doctor blade, a wire bar, a die coater, a comma-type knife coater, and a gravure coater.

[0224] It should be noted that before forming the coating layer in step (a), there may be a step of subjecting one or both of the bonding surfaces of the first thermoplastic resin film 10 and the polarizer 30 to a bonding-facilitating treatment (surface activation treatment) such as saponification treatment, corona discharge treatment, plasma treatment, flame treatment, primer treatment, anchor coating treatment, etc.

[0225] Step (b) is a step of laminating the first thermoplastic resin film 10 or the polarizing plate 30 to obtain a laminated film, and the lamination can be performed by pressing from above and below using a laminating roll or the like, for example.

[0226] Step (c) is a step of irradiating the laminated film obtained in step (b) with active energy rays to cure the coating layer. Irradiation with active energy rays may be performed from either the first thermoplastic resin film 10 or the polarizer 30, or from both.

[0227] The light source for irradiating the active energy ray can be any light source capable of generating ultraviolet rays, electron beams, X-rays, etc. In particular, light sources having a light emission distribution at a wavelength of 400 nm or less can be suitably used, such as low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, metal halide lamps, etc.

[0228] exist Figure 2 In the polarizing plate of the structure shown, at least one of the first adhesive layer 15 and the second adhesive layer 25 is formed from the adhesive composition of the present invention. The first adhesive layer 15 and / or the second adhesive layer 25 is a cured layer of the adhesive composition of the present invention.

[0229] exist Figure 2 In the polarizing plate having the structure shown, at least one of the first adhesive layer 15 and the second adhesive layer 25 may be formed of the adhesive composition of the present invention, and the other may be formed of an adhesive composition different from the adhesive composition of the present invention.

[0230] As other adhesive compositions, there can be mentioned conventionally known water-based adhesives and active energy ray-curable adhesives.

[0231] Examples of the water-based adhesive include conventionally known adhesive compositions using a polyvinyl alcohol-based resin or a urethane resin as a main component.

[0232] The active energy ray-curable adhesive is an adhesive that cures by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. When an active energy ray-curable adhesive is used, the adhesive layer of the polarizing plate is a cured layer of the adhesive.

[0233] The active energy ray-curable adhesive may be an adhesive containing an epoxy compound cured by cationic polymerization as a curable component, and is preferably an ultraviolet curable adhesive containing the epoxy compound as a curable component. The so-called epoxy compound refers to a compound having an average of one or more, preferably two or more epoxy groups in the molecule. Only one epoxy compound may be used, or two or more epoxy compounds may be used in combination.

[0234] Examples of epoxy compounds include hydrogenated epoxy compounds (glycidyl ethers of polyols having alicyclic rings) obtained by reacting epichlorohydrin with alicyclic polyols obtained by hydrogenating aromatic rings of aromatic polyols; aliphatic epoxy compounds such as polyglycidyl ethers of aliphatic polyols or alkylene oxide adducts thereof; and alicyclic epoxy compounds which are epoxy compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule.

[0235] The active energy ray-curable adhesive may contain a radically polymerizable (meth)acrylic compound as a curable component instead of or together with the epoxy compound. Examples of the (meth)acrylic compound include (meth)acrylic acid ester monomers having one or more (meth)acrylic acid groups in the molecule; (meth)acrylic acid ester oligomers having at least two (meth)acrylic acid groups in the molecule obtained by reacting two or more functional group-containing compounds; and other compounds containing (meth)acrylic acid groups.

[0236] When the active energy ray-curable adhesive contains an epoxy compound that cures by cationic polymerization as a curable component, it is preferred to contain a photocationic polymerization initiator. Examples of the photocationic polymerization initiator include aromatic diazonium salts; aromatic iodonium salts, aromatic sulfonium salts and other onium salts; and iron-arene complexes.

[0237] When the active energy ray-curable adhesive contains a radical polymerizable component such as a (meth) acrylic acid compound, it preferably contains a photo radical polymerization initiator. Examples of the photo radical polymerization initiator include acetophenone initiators, benzophenone initiators, benzoin ether initiators, thioxanthone initiators, xanthone, fluorenone, camphorquinone, benzaldehyde, anthraquinone, and the like.

[0238] Figure 2 The polarizing plate having the structure shown above can be produced by a production method including the following steps (A) to (D).

[0239] (A) a coating layer forming step of forming a coating layer of an adhesive composition on at least one of the first thermoplastic resin film 10 and the polarizer 30;

[0240] (B) a coating layer forming step of forming a coating layer of an adhesive composition on at least one of the second thermoplastic resin film 20 and the polarizer 30;

[0241] (C) a step of obtaining a laminated film by laminating a thermoplastic resin film or a polarizing plate 30 via a coating layer;

[0242] (D) A step of irradiating the laminated film with active energy rays to cure the coating layer.

[0243] The step (A) is the same as the above-mentioned step (a).

[0244] In the step (B), the coating layer may be formed on at least one of the second thermoplastic resin film 20 and the polarizer 30 , but it is preferred that the coating layer of the adhesive composition of the present invention is formed on the second thermoplastic resin film 10 .

[0245] Before forming the coating layer in step (B), one or both of the bonding surfaces of the second thermoplastic resin film 20 and the polarizer 30 may be subjected to an adhesion-facilitating treatment (surface activation treatment) such as saponification treatment, corona discharge treatment, plasma treatment, flame treatment, primer treatment, anchor coating treatment, etc.

[0246] Step (C) is a step of obtaining a laminated film by laminating the thermoplastic resin film or the polarizing plate 30 via the coating layer formed in step (A) and step (B). For example, lamination can be performed by pressing from above and below using a laminating roll or the like.

[0247] Step (D) is a step of irradiating the laminated film obtained in step (C) with active energy rays to cure the coating layer. The irradiation with active energy rays may be performed from either the first thermoplastic resin film 10 or the second thermoplastic resin film 20, or from both. The light source for irradiating the active energy rays may be the same as the light source used in the above-mentioned step (c).

[0248] in addition, Figure 2 The polarizing plate shown can also be obtained by injecting an adhesive composition between a polarizer and a thermoplastic resin film, laminating the films via a layer of the adhesive composition, and then irradiating the films with active energy rays.

[0249] The thickness of the adhesive layer formed by the adhesive composition of the present invention is, for example, 0.1 μm or more and 100 μm or less, preferably 0.5 μm or more and 80 μm or less, more preferably 1 μm or more and 60 μm or less, and further preferably 2 μm or more and 50 μm or less in the polarizing plate. From the viewpoint of thinning the polarizing plate, it is also preferred that the thickness of the adhesive layer be 30 μm or less, and further preferably 20 μm or less.

[0250] The thickness of the first adhesive layer 15 and the second adhesive layer 25 may be the same or different.

[0251] 〔5〕Other components of polarizing plate

[0252] 〔5-1〕Optical functional film

[0253] The polarizing plate may include other optically functional films other than the polarizing plate 30 for imparting a desired optical function, and a suitable example thereof is a retardation film.

[0254] As described above, the first thermoplastic resin film 10 and / or the second thermoplastic resin film 20 may also serve as a phase difference film, but a phase difference film may be laminated separately from the thermoplastic resin film. In the latter case, the phase difference film may be laminated on the outer surface of the first thermoplastic resin film 10 and / or the second thermoplastic resin film 20 via an adhesive layer or a bonding agent layer. In addition, a phase difference film may be laminated instead of the first thermoplastic resin film 10 or the second thermoplastic resin film 20. If a specific example is given, for example, the following structure is used, that is, Figure 1 The single-sided protective polarizing plate shown has a first thermoplastic resin film 10 bonded to one surface of the polarizer 30 and a retardation film bonded to the other surface of the polarizer 30. In this case, the retardation film may be laminated on the surface of the polarizer 30 via a pressure-sensitive adhesive layer or an adhesive layer.

[0255] Examples of the retardation film include a birefringent film formed of a stretched film of a light-transmitting thermoplastic resin; a film in which discotic liquid crystal or nematic liquid crystal is fixedly oriented; and a film in which the above-mentioned liquid crystal layer is formed on a base film.

[0256] The base film is usually a film made of a thermoplastic resin, and an example of the thermoplastic resin is a cellulose ester resin such as triacetyl cellulose.

[0257] As the thermoplastic resin forming the birefringent film, the thermoplastic resins described with respect to the first and second thermoplastic resin films 10 and 20 can be used.

[0258] Examples of other optically functional films (optical members) that can be contained in the polarizing plate include a light-collecting plate, a brightness enhancement film, a reflective layer (reflective film), a semi-transmissive reflective layer (semi-transmissive reflective film), a light diffusion layer (light diffusion film), etc. These are generally provided when the polarizing plate is a polarizing plate disposed on the back side (backlight side) of the liquid crystal cell.

[0259] 〔5-2〕Adhesive layer

[0260] The polarizing plate of the present invention may include an adhesive layer for bonding it to an image display element such as a liquid crystal cell, an organic EL element, or other optical member. Figure 1 The polarizing plate of the structure shown can be laminated on the outer surface of the polarizer 30. Figure 2 In the polarizing plate having the structure shown, the first thermoplastic resin film 10 or the second thermoplastic resin film 20 may be laminated on the outer surface.

[0261] As the adhesive used in the adhesive layer, an adhesive having a base polymer of (meth) acrylic resin, silicone resin, polyester resin, polyurethane resin, polyether resin, etc. can be used. Among them, (meth) acrylic adhesives are preferred from the viewpoints of transparency, adhesion, reliability, weather resistance, heat resistance, reprocessability, etc.

[0262] The thickness of the pressure-sensitive adhesive layer is determined based on its adhesive strength and the like, and is preferably in the range of 1 μm to 50 μm, and preferably 2 μm to 40 μm.

[0263] The polarizing plate may include a separator laminated on the outer surface of the adhesive layer. The separator may be a film including polyethylene resins such as polyethylene, polypropylene resins such as polypropylene, polyester resins such as polyethylene terephthalate, etc. Among them, a stretched film of polyethylene terephthalate is preferred.

[0264] The adhesive layer may contain glass fibers, glass beads, resin beads, fillers consisting of metal powders and other inorganic powders, pigments, colorants, antioxidants, ultraviolet absorbers, antistatic agents, and the like as necessary.

[0265] 〔5-3〕Protective film

[0266] The polarizing plate of the present invention may include a protective film for protecting its surface (thermoplastic resin film surface, polarizer surface, etc.) The protective film is peeled off together with the adhesive layer after the polarizing plate is bonded to, for example, an image display device or other optical member.

[0267] The protective film is formed of, for example, a base film and an adhesive layer laminated thereon. The above description is applicable to the adhesive layer.

[0268] The resin constituting the base film may be, for example, a thermoplastic resin such as polyethylene resin such as polyethylene, a polypropylene resin such as polypropylene, a polyester resin such as polyethylene terephthalate and polyethylene naphthalate, or a polycarbonate resin, and preferably a polyester resin such as polyethylene terephthalate.

[0269] Example

[0270] The present invention is further described in detail below by giving examples, but the present invention is not limited to these examples. In the examples, % and parts indicating the content or usage amount are by mass unless otherwise specified. The thickness of the film and adhesive layer (cured film) was measured using a digital altimeter "MH-15M" manufactured by Nikon Corporation.

[0271] <Example 1>

[0272] (1) Preparation of curable adhesive composition

[0273] The components shown in Table 1 were mixed in the blending amounts shown in Table 1 to prepare a curable adhesive composition A. The unit of the blending amount of each component shown in Table 1 is part by mass.

[0274] The details of each component shown in Table 1 are as follows.

[0275] (A): maleic anhydride-modified liquid polybutadiene (trade name "Lithene ultraN4-B-10MA" manufactured by Synthomer), number average molecular weight: 8200, viscosity at 25°C: 60 to 90 Pa·sec, acid value: 54 KOHmg / g)

[0276] (B-1): dicyclopentyl acrylate (trade name "FA-513AS" manufactured by Hitachi Chemical Co., Ltd.)

[0277] (B-2a): ethoxylated bisphenol A diacrylate (trade name "ABE-300" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In the following formula, X represents an ethyleneoxy group, and the sum of m and n is an average of 3.

[0278] [Chemistry 5]

[0279]

[0280] (B-2b): Propoxylated bisphenol A diacrylate (trade name "A-BPP-3" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In the following formula, X represents a propyleneoxy group, and the sum of m and n is an average of 3.

[0281] [Chemistry 6]

[0282]

[0283] (C): Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (trade name "Omnirad 819" manufactured by IGM Resins BV)

[0284] (Da): C9-based petroleum resin (trade name "ARKON P-100" manufactured by Arakawa Chemical Industries, Ltd., fully hydrogenated resin (alicyclic saturated hydrocarbon resin), softening point: 100.5° C., weight average molecular weight: 1600)

[0285] The weight average molecular weight of the (Da) component of the C9 petroleum resin is measured in accordance with the following procedure.

[0286] Pretreatment method: After dissolving the sample in cyclohexane, the sample was diluted by adding an eluent and filtered through a 0.45 μm membrane filter. The resulting solution was used as a measurement solution.

[0287] ·Measurement conditions

[0288] Chromatographic column: TSKgel SuperHM-H×2+SuperH2500×1(6.0mm ID×150mm×3 pieces)

[0289] Eluent: Toluene

[0290] Flow rate: 0.6mL / min.

[0291] Detector: RI detector

[0292] Column temperature: 40°C

[0293] Injection volume: 40μL

[0294] Molecular weight standard: Standard polystyrene

[0295] (2) Preparation of polarizing plate

[0296] A polymethyl methacrylate (PMMA) film having a thickness of 60 μm and a retardation film made of a cyclic polyolefin resin having a thickness of 50 μm (product name “ZEONOR” manufactured by ZEON Corporation of Japan) were prepared.

[0297] A corona treatment was applied to one side of the PMMA film, and the curable adhesive composition A prepared in (1) was applied to the corona treated surface using an adhesive coating device. A corona treatment was applied to one side of the phase difference film, and a curable adhesive composition B containing an epoxy compound as a curable component was applied to the corona treated surface using an adhesive coating device. The obtained coating layer and a polyvinyl alcohol-iodine polarizer having a thickness of 23 μm were laminated using a clamping roller to obtain a laminate. From the phase difference film side of the laminate, the total cumulative amount of irradiation (the cumulative amount of light irradiation intensity in the wavelength range of 320 to 400 nm) was about 200 mJ / cm 2 The layer of curable adhesive composition B and the layer of curable adhesive composition A were cured by ultraviolet light (UVB) (measured value obtained by measuring device: UV Power Puck II manufactured by FusionUV), thereby preparing a polarizing plate having a structure of PMMA film / curable adhesive composition A cured layer / polarizer / curable adhesive composition B cured layer / retardation film. It should be noted that the thickness of the cured layer of curable adhesive composition A is about 10 μm, and the thickness of the cured layer of curable adhesive composition B is 2.5 μm.

[0298] <Examples 2 to 5, Comparative Example 1>

[0299] A curable adhesive composition A was prepared in the same manner as in Example 1 except that the amounts of the components were changed as shown in Table 1. A polarizing plate was produced in the same manner as in Example 1 except that the curable adhesive composition A was used.

[0300] <Measurement and Evaluation>

[0301] (1) Moisture Permeability of Cured Film Formed from Curable Adhesive Composition A

[0302] The curable adhesive composition A was applied to a PMMA film having a thickness of 60 μm and subjected to a corona treatment using an adhesive coating device.

[0303] An untreated polyethylene terephthalate (PET) film was laminated on the coating layer of the curable adhesive composition A and laminated using a nip roller. Then, the total cumulative light intensity (the cumulative intensity of light irradiation in the wavelength range of 320 to 400 nm) was about 200 mJ / cm 2 The adhesive layer was cured by ultraviolet light (UVB) of 0.1% (measured value obtained by measuring device: UV Power Puck II manufactured by FusionUV) to obtain a laminate having a layer structure of PMMA film / cured adhesive layer / PET film. Thereafter, the PET film was peeled off to obtain a laminate having a layer structure of PMMA film / cured adhesive layer (cured film) (water vapor permeability measurement sample).

[0304] The obtained laminate (water vapor permeability measurement sample) was measured by the cup method specified in JIS Z 0208 at a temperature of 40°C and a relative humidity of 90% to obtain a water vapor permeability of 100 g / (m 2 · 24 hr)]. It should be noted that, during the measurement, the cured adhesive layer (cured film) in the above-mentioned laminate was placed in an environment of a temperature of 40° C. and a relative humidity of 90%. In addition, the laminate was installed in a cup with the cured film facing outward.

[0305] The results are shown in the column "Moisture permeability of laminated body" in Table 1. The numerical values ​​in parentheses represent the thickness of the cured film of the laminated body (unit: μm).

[0306] Furthermore, using the moisture permeability (Jt) of the obtained laminate, the moisture permeability (J) of the cured film itself under the conditions of a temperature of 40° C. and a relative humidity of 90% was determined based on the following formula.

[0307] 1 / Jt=(1 / J)+(1 / Jsub)

[0308] The moisture permeability (Jsub) of a 60 μm-thick PMMA film as a substrate film measured by the cup method specified in IS Z 0208 at a temperature of 40° C. and a relative humidity of 90% was 70 g / (m 2 ·24hr).

[0309] The results are shown in the column "Moisture permeability of cured film" in Table 1. The numerical values ​​in parentheses represent the thickness of the cured film (unit: μm).

[0310] (2) Evaluation of Adhesion Between PMMA Films (Initial)

[0311] (2-1) Preparation of measurement samples

[0312] One surface of a 60 μm-thick PMMA film was subjected to a corona treatment, and the curable adhesive composition A was applied to the corona-treated surface using an adhesive coating device.

[0313] The coating layer of the curable adhesive composition A was laminated with the corona-treated surface of a 60 μm thick PMMA film on one side of which a corona treatment was applied using a nip roller. Then, the total cumulative light intensity (the cumulative amount of light irradiation intensity in the wavelength range of 320 to 400 nm) was about 200 mJ / cm 2The adhesive layer was cured by ultraviolet light (UVB) (measured value obtained by measuring device: UV Power Puck II manufactured by FusionUV), thereby obtaining a measurement sample having a layer structure of PMMA film / cured adhesive layer (cured film) / PMMA film. It should be noted that the thickness of the cured film of the curable adhesive composition A was 10 μm.

[0314] (2-2) Peel test

[0315] The prepared test sample was cut into a size of 200 mm in length and 25 mm in width as a test piece for measuring the peel strength between PMMA films. The blade of a cutter was inserted between the PMMA films, and 30 mm was peeled off from the end in the length direction. The peeled portion was clamped by the clamping part of the test machine. The test piece in this state was subjected to a peeling test in an atmosphere of 23°C and 55% relative humidity in accordance with JIS K 6854-3:1999 "Adhesives - Peel Adhesive Strength Test Method - Part 3: T-type Peeling" at a clamping moving speed of 300 mm / min. The average peeling force (unit: N / 25 mm) over a length of 170 mm excluding the 30 mm of the clamping part was determined and used as the peel strength between PMMA films. The results are shown in Table 1. After the test sample was prepared, the peel strength was measured after it was left to stand for 24 hours in an environment of 23°C and 50% relative humidity.

[0316] In Table 1, "material failure" means that the peel strength is extremely high and the film breaks before the film is peeled off during the test. The same applies to Tables 2 to 4.

[0317] In Comparative Example 1, the peel strength was too small and the peel strength could not be measured by the above test.

[0318] (3) Evaluation of Adhesion Between Polarizers (Initial)

[0319] (3-1) Preparation of measurement samples

[0320] A polarizing plate having a thickness of 23 μm and a cycloolefin-based film having a thickness of 50 μm were bonded together using an acrylic pressure-sensitive adhesive composition to produce a polarizing plate with a protective film on one side.

[0321] The curable adhesive composition A was applied to one surface of a polarizing plate having a thickness of 23 μm using an adhesive coating device.

[0322] The coating layer of the curable adhesive composition A was laminated on the polarizer surface of the same polarizer with a protective film on one side using a nip roller. Then, the total cumulative light intensity (the cumulative amount of light irradiation intensity in the wavelength range of 320 to 400 nm) was about 200 mJ / cm 2The adhesive layer was cured by ultraviolet light (UVB) (measured value obtained by measuring device: UV Power Puck II manufactured by FusionUV), thereby obtaining a measurement sample having a layer structure of cycloolefin film / adhesive layer / polarizer / cured adhesive layer (cured film) / polarizer / adhesive layer / cycloolefin film. It should be noted that the thickness of the cured film of the curable adhesive composition A was 10 μm.

[0323] (3-2) Peel test

[0324] The peeling test was performed in the same manner as in (2-2) above, except that the test sample prepared in (3-1) above was used and the blade of a cutter was inserted between the polarizers. The results are shown in Table 1. It should be noted that the peeling strength was measured after the test sample was prepared and left to stand for 24 hours in an environment of a temperature of 23°C and a relative humidity of 50%RH.

[0325] In Comparative Example 1, the peel strength was too small and the peel strength could not be measured by the above test.

[0326] (4) Evaluation of Adhesion Between Polarizer of Polarizing Plate and PMMA Film (Initial)

[0327] An adhesive layer is formed on the PMMA film side of the obtained polarizing plate. The obtained polarizing plate with an adhesive layer is cut into a size of 200 mm in length (parallel to the absorption axis direction of the polarizer) and 25 mm in width, and the adhesive layer is bonded to a glass plate to obtain a laminate. The obtained laminate is used as a test piece for measuring the peel strength between the polarizer and the PMMA film. The blade of a cutter is inserted between the polarizer and the PMMA film of the test piece, and 30 mm is peeled off from the end in the length direction. The peeled part is clamped by the upper clamp of the test machine, and the lower clamp is clamped by the glass plate. For the test piece in this state, a peel test is carried out at a clamping moving speed of 300 mm / min in an atmosphere of a temperature of 23°C and a relative humidity of 55% in accordance with JIS K 6854-2:1999 "Adhesive-Peel Adhesive Strength Test Method-Part 2: 180 Degree Peeling", and the average peeling force of a length of 170 mm excluding the 30 mm of the clamping part is calculated, and it is set as the peel strength between the polarizer and the PMMA film. The results are shown in Table 1. After the polarizing plate was produced, it was left to stand for 24 hours in an environment of a temperature of 23° C. and a relative humidity of 50% RH, and then the peel strength was measured.

[0328] In Comparative Example 1, the peel strength was too small and the peel strength could not be measured by the above test.

[0329] (5) Evaluation of durability of polarizing plate (high temperature environment)

[0330] (5-1) Preparation of samples for measurement

[0331] The phase difference film surface of the obtained polarizing plate containing a cyclic polyolefin resin was corona treated, and an acrylic adhesive layer (with a separator) was laminated to the corona treated surface using a laminator to obtain a polarizing plate with an adhesive layer having a layer structure of polarizing plate / adhesive layer / separator.

[0332] The obtained polarizing plate with adhesive layer was cut into a size of 30 mm × 30 mm, and after peeling off the separator, the adhesive layer side of the polarizing plate with adhesive layer was attached to alkali-free glass (trade name "EAGLEXG" manufactured by Corning). 2 After the autoclave treatment was carried out for 20 minutes at a temperature of 23° C. and a relative humidity of 55%, the sample was allowed to stand for 24 hours.

[0333] (5-2) Durability test

[0334] The measurement sample was left in a dry environment at 95° C. for 24 hours, and then left in an environment at 23° C. and 50% RH for 24 hours. The measurement sample was visually observed, and the durability of the polarizing plate was evaluated according to the following evaluation criteria. The results are shown in Table 1.

[0335] A: No peeling was observed between the polarizing plate and the PMMA film.

[0336] B: Peeling was partially observed between the polarizing plate and the PMMA film.

[0337] C: Peeling was observed entirely between the polarizing plate and the PMMA film.

[0338] (6) Evaluation of durability of polarizing plate (high temperature and high humidity environment)

[0339] (6-1) Preparation of samples for measurement

[0340] A sample for measurement was prepared in the same manner as in the above (5-1).

[0341] (6-2) Durability test

[0342] The above-mentioned measurement sample was placed in a high temperature and high humidity environment of 80°C and 90%RH for 24 hours, and then placed in an environment of 23°C and 50%RH for 24 hours. The measurement sample was visually observed and the durability of the polarizing plate was evaluated according to the same evaluation criteria as in (5-2). The results are shown in Table 1.

[0343] (7) Evaluation of adhesion between PMMA films (after exposure to high temperature and high humidity environment)

[0344] (7-1) Preparation of samples for measurement

[0345] A sample for measurement was prepared in the same manner as in the above (2-1).

[0346] (7-2) Peel test

[0347] The prepared measurement sample was cut into a size of 200 mm in length and 25 mm in width as a test piece for measuring the peel strength between PMMA films. The test piece was placed in a high temperature and high humidity environment of 80°C and 90% RH for 24 hours, and then placed in an environment of 23°C and 50% RH for 24 hours. Thereafter, the peel strength between PMMA films was measured in the same manner as in (2-2) above. The results are shown in Table 1.

[0348] In Comparative Example 1, the peel strength was too small and the peel strength could not be measured by the above test.

[0349] (8) Evaluation of Adhesion Between Polarizers (After Exposure to High Temperature and High Humidity Environment)

[0350] (8-1) Preparation of samples for measurement

[0351] A sample for measurement was prepared in the same manner as in the above (3-1).

[0352] (8-2) Peel test

[0353] The peel test was performed in the same manner as in the above (7-2) except that the measurement sample prepared in the above (8-1) was used.

[0354] In Comparative Example 1, the peel strength was too small and the peel strength could not be measured by the above test.

[0355] (9) Evaluation of Adhesion Between Polarizer and PMMA Film of Polarizing Plate (After Exposure to High Temperature and High Humidity Environment)

[0356] An adhesive layer is formed on the PMMA film side of the obtained polarizing plate. The obtained polarizing plate with an adhesive layer is cut into a size of 200 mm in length (parallel to the absorption axis direction of the polarizer) and 25 mm in width, and the adhesive layer is bonded to a glass plate to obtain a laminate. The obtained laminate is used as a test piece for measuring the peel strength between the polarizer and the PMMA film. After the test piece is placed in a high temperature and high humidity environment of 80°C and a relative humidity of 90% RH for 24 hours, it is placed in an environment of 23°C and a relative humidity of 50% RH for 24 hours. Thereafter, the peel strength between the polarizer and the PMMA film is measured in the same manner as in (4) above. The results are shown in Table 1.

[0357] In Comparative Example 1, the peel strength was too small to be measured by the above test.

[0358] [Table 1]

[0359]

[0360] <Example 6>

[0361] (1) Preparation of curable adhesive composition

[0362] The components shown in Table 2 were mixed in the amounts shown in Table 2 to prepare curable adhesive compositions A. The unit of the amount of each component shown in Table 2 is parts by mass.

[0363] The details of each component shown in Table 2 are as follows.

[0364] (A): Maleic anhydride-modified liquid polybutadiene (trade name "Lithene ultraN4-B-10MA" manufactured by Synthomer, number average molecular weight: 8200, viscosity at 25°C: 60 to 90 Pa·sec, acid value: 54 KOHmg / g)

[0365] (B-1): dicyclopentyl acrylate (trade name "FA-513AS" manufactured by Hitachi Chemical Co., Ltd.)

[0366] (B-2c): ethoxylated bisphenol A diacrylate (trade name "A-BPE-10" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In the following formula, X represents an ethyleneoxy group, and the sum of m and n is an average of 10.

[0367] [Chemistry 7]

[0368]

[0369] (C): Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (trade name "Omnirad 819" manufactured by IGM Resins BV)

[0370] (Db): Petroleum resin (trade name "T-REZ HA105" manufactured by JXTG Energy Corporation, hydrogenated resin (alicyclic saturated hydrocarbon resin containing dicyclopentadiene as a monomer component), softening point (nominal value): 104.5°C, weight average molecular weight (nominal value): 610)

[0371] (2) Preparation of polarizing plate

[0372] A polarizing plate was produced in the same manner as in Example 1 except that the curable adhesive composition A prepared in the above (1) of Example 6 was used as the curable adhesive composition A.

[0373] <Examples 7 to 9>

[0374] A curable adhesive composition A was prepared in the same manner as in Example 6 except that the amounts of the components were changed as shown in Table 2. A polarizing plate was produced in the same manner as in Example 6 except that the curable adhesive composition A was used.

[0375] <Measurement and Evaluation>

[0376] In Examples 6 to 9, the same items as in Example 1 were measured and evaluated. The results are shown in Table 2.

[0377] [Table 2]

[0378]

[0379] <Example 10>

[0380] (1) Preparation of curable adhesive composition

[0381] The components shown in Table 3 were mixed in the blending amounts shown in Table 3 to prepare a curable adhesive composition A. The unit of the blending amount of each component shown in Table 3 is part by mass.

[0382] The details of each component shown in Table 3 are as follows.

[0383] (Aa): Maleic anhydride-modified liquid polybutadiene (trade name "Lithene ultraN4-B-10MA" manufactured by Synthomer, number average molecular weight: 8200, viscosity at 25°C: 60 to 90 Pa·sec, acid value: 54 KOHmg / g)

[0384] (Ab): Maleic anhydride-modified liquid polybutadiene (trade name "Lithene ultraPM4-7.5NA" manufactured by Synthomer, viscosity at 25°C: 2 to 6 Pa·sec, acid value: 40 KOHmg / g)

[0385] (B-1a): dicyclopentyl acrylate (trade name "FA-513AS" manufactured by Hitachi Chemical Co., Ltd.)

[0386] (B-1b): Benzyl acrylate (trade name "Viscoat #160, BZA" manufactured by Osaka Organic Chemical Industry Co., Ltd.)

[0387] (B-1c): 3,3,5-trimethylcyclohexyl acrylate (trade name "Viscoat #196, TMCHA" manufactured by Osaka Organic Chemical Industry Co., Ltd.)

[0388] (B-2c): ethoxylated bisphenol A diacrylate (trade name "A-BPE-10" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.). In the following formula, X represents an ethyleneoxy group, and the sum of m and n is an average of 10.

[0389] [Chemistry 8]

[0390]

[0391] (B-2d): Tricyclodecane dimethanol diacrylate (trade name "A-DCP" manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0392] (B-3): Trimethylolpropane triacrylate (trade name "A-TMPT" manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0393] (C): Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (trade name "Omnirad 819" manufactured by IGM Resins BV)

[0394] (Db): Petroleum resin (trade name "T-REZ HA105" manufactured by JXTG Energy Corporation, hydrogenated resin (alicyclic saturated hydrocarbon resin containing dicyclopentadiene as a monomer component), softening point (nominal value): 104.5°C, weight average molecular weight (nominal value): 610)

[0395] (2) Preparation of polarizing plate

[0396] A polarizing plate was produced in the same manner as in Example 1, except that the curable adhesive composition A prepared in the above (1) of Example 10 was used as the curable adhesive composition A.

[0397] <Examples 11 to 19>

[0398] A curable adhesive composition A was prepared in the same manner as in Example 10 except that the amounts of the components were changed as shown in Table 3 or Table 4. A polarizing plate was produced in the same manner as in Example 10 except that the curable adhesive composition A was used.

[0399] <Measurement and Evaluation>

[0400] About Examples 11 to 19, the same items as those of Example 1 and the like were measured and evaluated. The results are shown in Tables 3 and 4.

[0401] [Table 3]

[0402]

[0403] [Table 4]

[0404]

[0405] <Measurement of Viscosity>

[0406] The viscosity of the curable adhesive compositions A prepared in Examples 6 to 9, 11, 13 to 15 and 18 was measured at a temperature of 25° C. and a rotation speed of 5 rpm using an E-type viscometer [“TVE-25” manufactured by Toki Sangyo Co., Ltd.].

[0407] The viscosity of the curable adhesive composition A of Example 6 is 4478 mPa·sec, the viscosity of the curable adhesive composition A of Example 7 is 4069 mPa·sec, the viscosity of the curable adhesive composition A of Example 8 is 2314 mPa·sec, the viscosity of the curable adhesive composition A of Example 9 is 1488 mPa·sec, the viscosity of the curable adhesive composition A of Example 11 is 1823 mPa·sec, the viscosity of the curable adhesive composition A of Example 13 is 2920 mPa·sec, the viscosity of the curable adhesive composition A of Example 14 is 2611 mPa·sec, the viscosity of the curable adhesive composition A of Example 15 is 1811 mPa·sec, and the viscosity of the curable adhesive composition A of Example 18 is 2401 mPa·sec.

[0408] Description of Reference Numerals

[0409] 10: first thermoplastic resin film, 15: first adhesive layer, 20: second thermoplastic resin film, 25: second adhesive layer, 30: polarizing plate.

Claims

1. A polarizing plate comprising, in order, a polarizer, an adhesive layer and a thermoplastic resin film, The adhesive layer is a cured product layer of a curable adhesive composition containing a maleic anhydride-modified compound (A), a (meth)acrylate compound (B), and a photopolymerization initiator (C). When the total amount of the adhesive composition is 100 mass %, the content of the maleic anhydride-modified compound (A) is 3 mass % or more and 40 mass % or less, and the content of the (meth)acrylate compound (B) is 15 mass % or more and 75 mass % or less, The (meth)acrylate compound (B) comprises a bifunctional (meth)acrylate (B-2) represented by the following formula: In the formula, R1 and R2 each independently represent a hydrogen atom or a methyl group, X represents an ethyleneoxy group (-C2H4O-) or a propyleneoxy group (-C3H6O-), n represents an integer of 1 to 20, and m represents an integer of 1 to 20.

2. The polarizing plate according to claim 1, wherein The (meth)acrylate compound (B) includes a monofunctional (meth)acrylate compound (B-1).

3. The polarizing plate according to claim 2, wherein: In the curable adhesive composition, the content of the monofunctional (meth)acrylate compound (B-1) is 60% by mass or more in 100% by mass of the (meth)acrylate compound (B).

4. The polarizing plate according to claim 3, wherein In the curable adhesive composition, the content of the monofunctional (meth)acrylate compound (B-1) is 99% by mass or less in 100% by mass of the (meth)acrylate compound (B).

5. The polarizing plate according to any one of claims 2 to 4, wherein The monofunctional (meth)acrylate compound (B-1) includes at least one compound selected from alicyclic alkyl (meth)acrylate compounds and aromatic (meth)acrylate compounds.

6. The polarizing plate according to claim 1 or 2, wherein: The curable adhesive composition further includes a petroleum resin (D).

7. The polarizing plate according to claim 1 or 2, wherein: The maleic anhydride-modified compound (A) includes a maleic anhydride-modified polymer (A-1).

8. The polarizing plate according to claim 1 or 2, wherein: A cured film having a thickness of 10 μm and comprising the curable adhesive composition has a hardness of 400 g / (m 2 · 24hr) or less.

9. The polarizing plate according to claim 1 or 2, wherein: The laminated body of the (meth)acrylic resin film with a thickness of 60 μm and the cured film with a thickness of 10 μm comprising the curable adhesive composition had a viscosity of 55 g / (m 2 · 24hr) or less.

10. The polarizing plate according to claim 1 or 2, wherein: The thermoplastic resin film is a (meth)acrylic resin film.

11. The polarizing plate according to claim 1 or 2, wherein: The adhesive layer has a thickness of 2 μm or more and 50 μm or less.

12. A curable adhesive composition comprising a maleic anhydride-modified compound (A), a (meth)acrylate compound (B), a photopolymerization initiator (C) and a petroleum resin (D), The (meth)acrylate compound (B) comprises a monofunctional (meth)acrylate compound (B-1), When the total amount of the adhesive composition is 100 mass %, the content of the maleic anhydride-modified compound (A) is 3 mass % or more and 40 mass % or less, and the content of the (meth)acrylate compound (B) is 15 mass % or more and 75 mass % or less, When the total amount of the (meth)acrylate compound (B) is 100% by mass, the content of the monofunctional (meth)acrylate compound (B-1) is 60% by mass or more, The (meth)acrylate compound (B) further includes a bifunctional (meth)acrylate (B-2) represented by the following formula: In the formula, R1 and R2 each independently represent a hydrogen atom or a methyl group, X represents an ethyleneoxy group (-C2H4O-) or a propyleneoxy group (-C3H6O-), n represents an integer of 1 to 20, and m represents an integer of 1 to 20.

13. The curable adhesive composition according to claim 12, wherein A cured film having a thickness of 10 μm and comprising the curable adhesive composition has a hardness of 400 g / (m 2 · 24hr) or less.

14. A polarizing plate comprising, in order, a polarizer, an adhesive layer and a thermoplastic resin film, The adhesive layer is a cured product layer of the curable adhesive composition according to claim 12 or 13.