A high-light electroplating process for air intake grille
By adopting pretreatment, roughening and activation treatment steps in the plastic electroplating process, a dense conductive film layer is formed, which solves the problems of high preparation cost and large loss of palladium liquid, and achieves a more stable and efficient activation rate and excellent Surface performance.
Patent Information
- Application Number
- CN202210445804.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-04-26
AI Technical Summary
In the existing plastic electroplating process, the palladium active liquid is prepared with high cost and large losses, making it difficult to ensure a stable and efficient activation rate, affecting the conductivity and surface performance.
Pretreatment, roughening and activation treatment steps, including stamping micropore opening, water-based oil removal, roughening neutralization, activated colloid coating and ultrasonic homogenization, to form a dense conductive film layer, reduce the use of palladium active liquid, and reduce the use of Loss and production costs.
A more stable and efficient activation rate is achieved, the surface performance and gloss of the air intake grille are improved, and the use and production cost of palladium active liquid is significantly reduced.
Smart Images

Figure GHA0000008018430000081 
Figure GHA0000008018430000091 
Figure GHA0000008018430000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of plastic surface electroplating, and more specifically, to a high-light electroplating process for an air intake grille. Background Art
[0002] Electroplating is a process that uses electrolysis to attach a metal film to the surface of metal or other materials, thereby preventing metal oxidation (such as rust), improving wear resistance, conductivity, reflectivity, corrosion resistance (copper sulfate, etc.) and enhancing aesthetics. Moreover, with the renewal of the industry and the comprehensive accounting of the corresponding cost performance of enterprises, plastic electroplating, which has the advantages of light weight, easy processing and good surface smoothness, has also ushered in unprecedented development.
[0003] The specific steps of the plastic electroplating method in the related art are as follows: the surface of the air intake grille to be electroplated (plastic material) is roughened with chromic acid and sulfuric acid solutions, first activated in a solution containing a precious metal (palladium salt), and then debonded and rinsed, and then a conductive layer is formed on the plastic surface by chemical copper plating or chemical nickel plating, and finally electroplating is performed to complete the plastic electroplating operation.
[0004] In addition, the core step of the above-mentioned plastic electroplating method that is most important for the final performance is the activation treatment. However, the activation treatment in the related technology is simply to immerse the roughened air intake grille to be electroplated in a colloidal palladium activation solution. The palladium content in the colloidal palladium activation solution is above 200-300 mg / L. Therefore, the preparation cost is high and the loss rate is large. It is difficult to ensure a stable and efficient activation rate, and the palladium activation solution needs to be replenished regularly. Summary of the invention
[0005] In order to obtain a stable and efficient activation rate through a specific activation treatment, thereby reducing the negative impact of excessive activation rate differences on the conductivity and surface properties of electroplated plastic parts, the present application provides a high-light plating process for air intake grilles. The air intake grilles to be electroplated after the activation treatment have excellent surface properties and do not require regular replenishment of palladium activation solution, thereby significantly reducing production costs.
[0006] The present application provides a high-gloss electroplating process for an air intake grille, which adopts the following technical solutions:
[0007] A high-light electroplating process for an air intake grille comprises the following steps:
[0008] S1. Pretreatment: firstly, the side wall of the air intake grille to be electroplated is punched to open micropores, and then the side wall is washed and degreased to obtain the pretreated air intake grille to be electroplated;
[0009] S2, roughening treatment: then immerse the pre-treated air intake grille to be electroplated in a roughening liquid for roughening treatment, and neutralize it until there is no residual roughening liquid on the surface and the hole wall;
[0010] S3, activation treatment: coating the activated colloid on the surface of the air intake grille to be electroplated, and after ultrasonic homogenization, reacting at 24-72°C for 2-18 minutes until the surface of the product is completely dark brown, thus obtaining the activated air intake grille to be electroplated;
[0011] The activated colloid is composed of a divalent target salt, divalent tin, carbon black, starch, hydrochloric acid, tetrabutylammonium chloride, a dispersant and deionized water;
[0012] S4, debonding treatment: immerse the activated air intake grille to be electroplated in a debonding agent and extract and rinse repeatedly until the surface of the product turns light brown, thereby obtaining the debonded air intake grille to be electroplated;
[0013] S5. Electroplating film formation: immerse the air intake grille to be electroplated after debonding into the electroplating solution, and plate pre-plated nickel, bright acid copper, semi-bright nickel, bright nickel, microporous nickel and chromium on the air intake grille to be electroplated in sequence to obtain a high-gloss air intake grille.
[0014] By adopting the above technical solution, the surface of the air intake grille to be electroplated after the above water-based oil removal and roughening treatment is rough and the bonding force is greatly improved. In the subsequent activation treatment, the activated colloid can be stably adhered to the surface of the air intake grille to be electroplated. Compared with the immersion activation method, the activation rate is high, the loss is effectively reduced, and the preparation cost is saved;
[0015] In addition, after ultrasonic homogenization, the activated colloid can be evenly combined on the surface and hole wall of the air intake grille to be electroplated, which is beneficial to the full implementation of surface replacement, sensitization reduction and other reactions of the air intake grille to be electroplated, and can form a dense conductive film layer structure. After the above conductive film layer structure is exposed to palladium through degumming treatment, the electroplating film formation operation can be stably carried out through electrolysis.
[0016] Preferably, the activated colloid in S3 is composed of the following components in weight percentage: target salt 0.002-0.003%, divalent tin 0.2-0.4%, carbon black 4-6%, starch 20-28%, hydrochloric acid 25-30%, tetrabutylammonium chloride 1-3%, dispersant 0.5-1%, and the balance is deionized water.
[0017] By adopting the above technical solution, the activated colloid composed of the above components can not only provide the ions required for replacement through palladium salt, divalent tin, hydrochloric acid and tetrabutylammonium chloride, and allow the ions with reducing effect to maintain their reducing ability for a long time under certain conditions, but also cause certain micro-corrosion under the action of hydrochloric acid and tetrabutylammonium chloride, thereby facilitating the formation of a conductive film layer;
[0018] Among them, starch, carbon black and dispersant give the activated colloid a certain viscosity, so that it can adhere to the surface of the air intake grille to be electroplated in the form of paint for reaction. Compared with immersion activation, the reaction is more complete and the loss and preparation cost are significantly reduced. The palladium content in the colloidal palladium active solution is only 0.002-0.003%, and under the above operating temperature and conditions, the starch will gradually peel off due to gelatinization and other reasons, thereby ensuring the conductivity and surface quality of the conductive film layer.
[0019] Preferably, the target salt is one or more of palladium chloride, palladium sulfate, sodium tetrachloropalladate and diammonium palladium tetrachloride.
[0020] By adopting the above technical scheme, the palladium salt composed of the above composition, in addition to providing the palladium ions required for the replacement reaction, can also be compounded with other components to allow the reducing ions to maintain their reducing ability for a long time under certain conditions, and to allow a large number of crystal nuclei for the growth of metal crystals to form on the non-metal surface. In addition, the multi-component palladium salt has a certain compounding effect, among which the compounding effect of divalent palladium salt and tetravalent palladium chloride complex is the most significant.
[0021] Preferably, the specific steps of S1 are as follows:
[0022] S1a, firstly punch and open micro-pores on the side wall of the grille to be electroplated, wherein the density of opening micro-pores is 2-4 / cm 2 , pore diameter is 0.3-0.5mm;
[0023] S1b, then wash and degrease it at 54-60℃ for 1.5-4min to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is a 50-80g / L JF-CL188 aqueous solution.
[0024] By adopting the above technical scheme, after the air intake grille to be electroplated is degreased by water, it can effectively remove harmful substances such as grease, dust and sweat stains on the surface of the air intake grille to be electroplated to ensure the effect of subsequent process, and it can also provide binding sites for subsequent electroplating and activation through the micropores opened on the air intake grille to be electroplated.
[0025] Preferably, the specific steps of S2 are as follows:
[0026] S2a, then immerse the pre-treated air intake grille to be electroplated in the roughening solution, and perform the roughening treatment at 66-70°C for 6-18 minutes until the surface gloss of the product is weakened and roughened:
[0027] The roughening solution is composed of the following components in weight percentage: CrO3 38-44%, H2SO4 38-42%, trivalent chromium salt 0-2%, and the balance is water;
[0028] S2b, then neutralize and reduce the product with reduced gloss and rough surface at 18-35°C for 0.5-2min until there is no residual roughening liquid on the product surface and pore wall;
[0029] The neutralization reduction solution is composed of the following components in weight percentage: 0.5-3% sodium sulfite, 2-3% HCl, and the balance is water.
[0030] By adopting the above technical solution, the surface gloss of the air intake grille to be electroplated after roughening by the above process is significantly weakened, and a large number of dense microscopic rough structures (dovetail holes) are formed on the surface, thereby significantly increasing the contact area and bonding force between the electroplating surface and the air intake grille to be electroplated, and the surface of the air intake grille to be electroplated is hydrophilic;
[0031] The above-mentioned neutralization reduction reaction utilizes the reducing property of the solution to reduce and remove the residual chromic acid on the surface of the parts, thereby ensuring the normal progress of the subsequent processes, thereby reducing the occurrence of the phenomenon that the subsequent electroplated air intake grille cannot be completely plated (plastic exposure) due to the residual chromic acid.
[0032] Preferably, the activated colloid is first coated on the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 50-150um. Then, it is ultrasonically treated at a power of 80-120W for 3-5min until homogenized, and then reacted at 24-72°C for 2-18min until the surface of the product is completely dark brown, thereby obtaining the activated air intake grille to be electroplated.
[0033] By adopting the above technical scheme, after the activated colloid is sprayed on the surface of the air intake grille to be electroplated, it can be evenly and stably adsorbed in the dovetail holes on the surface of the air intake grille to be electroplated under the homogenizing effect of ultrasound and the corrosion effect of hydrochloric acid and tetrabutylammonium chloride, thereby providing a catalytic center for the subsequent electroplating reaction, that is, a large number of crystal nuclei for the growth of metal crystals can be formed on the non-metallic surface, thereby ensuring the conductivity and surface quality of the conductive film layer.
[0034] Preferably, the specific steps of S4 are as follows:
[0035] The activated air intake grille to be electroplated is immersed in a debonding agent, treated at 45-55°C for 2-8 minutes, and repeated 2-3 times until the surface of the product is light brown, to obtain the debonded air intake grille to be electroplated, wherein the debonding agent is 75-125ml / L PL-6A aqueous solution.
[0036] By adopting the above technical scheme, the residual binder components on the surface of the air intake grille to be electroplated after the above debonding treatment can be effectively stripped off, and the divalent tin around the palladium can also be dissolved to expose the palladium, thereby effectively activating the catalytic activity of the palladium.
[0037] Preferably, the specific steps of S5 are as follows:
[0038] S5a, pre-nickel layer:
[0039] First, immerse the debonded air intake grille into the electroplating solution I and heat it at a temperature of 45-55°C and a current density of 1-1.5A / dm 2 Electroplating for 4-6 minutes under the conditions of , the pre-nickel-plated air intake grille to be electroplated is obtained, and the coating film thickness is 10-25um;
[0040] The electroplating solution I is composed of the following components in weight percentage: NiSO4 22-26%, NiCl2 4.0-5.5%, H3BO3 4.0-5.5%, and the balance is water;
[0041] S5b, bright acid copper layer:
[0042] Immerse the pre-nickel-plated air intake grille into the electroplating solution II at a temperature of 22-26°C and a current density of 2-4A / dm 2 Electroplating for 40-60 minutes under the conditions of , the air intake grille to be electroplated with a bright acid copper layer is obtained, and the coating film thickness is 25-40um;
[0043] The electroplating solution II is composed of the following components in weight percentage: CuSO4 18-22%, H2SO4 6.0-7.5%, and the balance is water;
[0044] S5c, semi-bright nickel layer:
[0045] Immerse the air intake grille to be electroplated with a bright acid copper layer into electroplating solution III at a temperature of 55-60°C and a current density of 2-4A / dm 2 , electroplating for 20-23min at pH 3.6-4.2 to obtain an air intake grille to be electroplated with a semi-bright nickel layer, with a coating thickness of 35-50um;
[0046] The electroplating solution III is composed of the following components in weight percentage: NiSO4 28-32%, NiCl2 3.5-4.5%, H3BO3 3.5-4.5%, and the balance is water;
[0047] S5d, bright nickel layer:
[0048] Immerse the air intake grille to be electroplated with a semi-bright nickel layer in electroplating solution IV at a temperature of 55-60°C and a current density of 2-5A / dm 2 , electroplating for 13-16 minutes at pH 4.0-4.5 to obtain an air intake grille to be electroplated with a bright nickel layer, with a coating thickness of 20-35um;
[0049] The electroplating solution IV is composed of the following components in weight percentage: NiSO4 28-32%, NiCl2 4.0-7.0%, H3BO3 4.0-5.0%, and the balance is water;
[0050] S5e, microporous nickel layer:
[0051] Immerse the bright nickel-plated air intake grille into the electroplating solution V at a temperature of 55-60°C and a current density of 2-4A / dm 2 , electroplating for 3-6 minutes at pH 4.0-4.5 to obtain an air intake grille to be electroplated with a microporous nickel layer, with a coating thickness of 5-10 um;
[0052] The electroplating solution V is composed of the following components in weight percentage: NiSO4 28-32%, NiCl2 6.0-9.0%, H3BO3 4.0-5.0%, and the balance is water;
[0053] S5f, Chrome plating:
[0054] Immerse the air intake grille to be electroplated with a microporous nickel layer in electroplating solution VI at a temperature of 38-42°C and a current density of 8-15A / dm 2 Electroplating for 5-10 minutes under the conditions of , the air intake grille to be electroplated with a microporous nickel layer is obtained, and the coating film thickness is 25-40um;
[0055] The electroplating solution VI is composed of the following components in weight percentage: CrO3 26-32%, H2SO4 0.08-0.14%, and the balance is water.
[0056] By adopting the above technical scheme, the air intake grille to be electroplated is sequentially plated with pre-nickel, bright acid copper, semi-bright nickel, bright nickel, microporous nickel and chromium. While the multi-plating performance is good, the electroplated air intake grille is given excellent surface gloss and corrosion resistance through the composite of different performance plating layers.
[0057] In summary, this application has the following beneficial effects:
[0058] 1. The present application obtains a more stable and efficient activation rate through the above-mentioned specific pretreatment, roughening treatment and activation treatment steps, thereby reducing the negative impact of excessive activation rate difference on the conductivity and surface properties of electroplated plastic parts, and the obtained air intake grille has excellent surface properties and glossiness;
[0059] 2. The activated colloid composed of the above components in the present application can not only adhere to the surface of the air intake grille to be electroplated and form a large number of nuclei for the growth of metal crystals on the non-metal surface through the compounding of palladium salt, divalent tin, hydrochloric acid and tetrabutylammonium chloride, but also undergo a certain amount of micro-corrosion under the action of hydrochloric acid and tetrabutylammonium chloride, thereby promoting the formation of a conductive film layer and a catalytic center;
[0060] 3. After being sprayed on the surface of the air intake grille to be electroplated, the activated colloid in the present application can be evenly and stably adsorbed in the dovetail holes formed by the roughening of the surface of the air intake grille to be electroplated under the homogenizing effect of ultrasound and the corrosive effect of hydrochloric acid and tetrabutylammonium chloride, thereby providing a catalytic center (target) for the subsequent electroplating reaction, thereby ensuring the conductivity and surface quality of the conductive film layer. DETAILED DESCRIPTION
[0061] The present application is further described in detail below in conjunction with embodiments.
[0062] The raw materials used in the embodiments of the present application, except for the special instructions below, other equipment and raw materials used are common commercially available raw materials and models.
[0063] JF-CL188 was purchased from Shanghai Jianfei Environmental Protection Technology Co., Ltd.; PL-6A was purchased from Guangdong Bigley Technology Co., Ltd.
[0064] Preparation Example 1-6
[0065] An activated colloid, whose components and weights per 100 kg are shown in the following table, is prepared by stirring the above components at 2000 r / min for 30 min;
[0066] The target salt is palladium chloride; the divalent tin is tin dichloride; the average particle size of carbon black is 20nm; the starch is potato starch with an average particle size of 15um; and the dispersant is stearic acid.
[0067] Table: Components and weights of activated colloids in Preparation Examples 1-6 (kg)
[0068]
[0069]
[0070] Preparation Example 7-12
[0071] An activated colloid, which is different from Preparation Example 1 in that the target salt is selected differently, and the specific component selection is shown in the following table.
[0072] Table: Comparison table of palladium salt selection in Examples 7-10
[0073] Group Palladium salts Example 7 Palladium sulfate Example 8 Sodium tetrachloropalladate Example 9 Diammonium palladium tetrachloride Example 10 Palladium chloride: palladium sulfate is mixed in a weight ratio of 1:1 Embodiment 11 Palladium chloride: sodium tetrachloropalladate are compounded in a weight ratio of 1:0.3 Example 12 Palladium chloride: diammonium palladium tetrachloride are compounded in a weight ratio of 1:0.3
[0074] Preparation Examples 13-17
[0075] A roughening liquid, whose components and weights per 100 kg are shown in the following table, is prepared by stirring and mixing the above components at room temperature, wherein the trivalent chromium salt is chromium chloride.
[0076] Table: Components and weights of the roughening solution in Preparation Examples 13-17 (kg)
[0077]
[0078] Preparation Examples 18-22
[0079] A neutralization reduction liquid, whose components and weights per 100 kg are shown in the following table, is prepared by stirring and mixing the above components at room temperature.
[0080] Table: Components and weights of the neutralized reduction solution in Preparation Examples 18-22 (kg)
[0081]
[0082] Performance testing
[0083] Three groups of high-gloss air intake grilles prepared in the following embodiments and comparative examples were selected as test objects, and then their appearance, thickness, coating corrosion resistance and bonding strength were tested. The average values of the test results were recorded in the following table. The specific detection method is as follows;
[0084] 1) Appearance: 6-10 points for bright silver-white coating, fine crystals and uniform color; 0-5 points for dull coating, striped surface and partial no coating. Ten people are selected as the judging panel and the average value of the test results is recorded.
[0085] 2) Thickness: Use a microcomputer multifunctional electrolytic thickness gauge for testing, take the average value of the test results and keep two significant figures (unit: um);
[0086] 3) Anti-corrosion ability of coating: Immerse the prepared high-gloss air intake grille in a 5% potassium sulfate solution, take it out after 5 minutes and wash it with pure water, then observe the surface of the high-gloss air intake grille. If there is no discoloration, yellowing or peeling on the surface, it is considered qualified:
[0087] 4) Adhesion strength: For specific testing steps and standards, refer to the cross-hatch method in ASTM D 3359-2009 "Determination of Adhesion by Tape Test".
[0088] Example
[0089] Example 1
[0090] A high-light electroplating process for an air intake grille comprises the following steps:
[0091] S1. Preprocessing:
[0092] S1a, firstly, punching micro-holes on the side wall of the grille to be electroplated, wherein the micro-hole density is 2 / cm2 and the hole diameter is 0.5mm;
[0093] S1b, then wash and degrease it at 54°C for 4 minutes to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is a 50g / L JF-CL188 aqueous solution.
[0094] S2, roughening treatment:
[0095] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 66° C. for 18 minutes until the surface gloss of the product is weakened and becomes rough, wherein the roughening solution is prepared in Preparation Example 13;
[0096] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 18°C for 2 minutes until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 18.
[0097] S3, activation treatment:
[0098] First, the activated colloid is applied to the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 50um. Then, it is ultrasonically treated at a power of 80W for 5 minutes until it is homogenized, and the reaction is continued at 24°C for 18 minutes until the surface of the product is completely dark brown. The activated air intake grille to be electroplated is obtained, wherein the activated colloid is prepared by Preparation Example 1.
[0099] S4, degumming treatment:
[0100] The activated air intake grille to be electroplated is immersed in a debonding agent, treated at 45°C for 8 minutes, and repeated twice until the surface of the product is light brown, to obtain the debonded air intake grille to be electroplated, wherein the debonding agent is 75ml / L PL-6A aqueous solution.
[0101] S5. Electroplating film forming:
[0102] S5a, pre-nickel layer:
[0103] First, immerse the debonded air intake grille into the electroplating solution I and heat it at 45℃ and current density 1.5A / dm 2 Electroplating for 6 minutes under the conditions of , to obtain the air intake grille to be electroplated with a pre-nickel layer;
[0104] The electroplating solution I is composed of the following components in weight percentage: NiSO4 24%, NiCl 25.0%, H3BO 35.0%, and the balance is water;
[0105] S5b, bright acid copper layer:
[0106] The pre-nickel-plated air intake grille to be electroplated is immersed in electroplating solution II at a temperature of 22°C and a current density of 4A / dm 2 Electroplating for 60 minutes under the conditions of , the air intake grille to be electroplated with a bright acid copper layer is obtained;
[0107] The electroplating solution II is composed of the following components in weight percentage: CuSO4 20%, H2SO4 7.0%, and the balance is water;
[0108] S5c, semi-bright nickel layer:
[0109] The air intake grille to be electroplated with a bright acid copper layer is immersed in electroplating solution III at a temperature of 55°C and a current density of 4A / dm 2 , pH 4.2, and electroplating for 23 minutes to obtain an air intake grille to be electroplated with a semi-bright nickel layer;
[0110] The electroplating solution III is composed of the following components in weight percentage: NiSO4 30%, NiCl2 4.0%, H3BO 34.0%, and the balance is water;
[0111] S5d, bright nickel layer:
[0112] The air intake grille to be electroplated with a semi-bright nickel layer is immersed in electroplating solution IV at a temperature of 55°C and a current density of 5A / dm 2 , pH 4.5 for 16 minutes to obtain an air intake grille to be electroplated with a bright nickel layer;
[0113] The electroplating solution IV is composed of the following components in weight percentage: NiSO4 30%, NiCl2 6.0%, H3BO3 4.50%, and the balance is water;
[0114] S5e, microporous nickel layer:
[0115] The air intake grille to be electroplated with bright nickel layer is immersed in electroplating solution V at a temperature of 55°C and a current density of 4A / dm 2 , and electroplating for 6 minutes under the condition of pH 4.5 to obtain the air intake grille to be electroplated with a microporous nickel layer;
[0116] The electroplating solution V is composed of the following components in weight percentage: NiSO4 30%, NiCl2 7.5%, H3BO 34.5%, and the balance is water;
[0117] S5f, Chrome plating:
[0118] The air intake grille to be electroplated with a microporous nickel layer is immersed in the electroplating solution VI at a temperature of 40°C and a current density of 15A / dm 2 Electroplating for 10 minutes under the conditions of , to obtain the air intake grille to be electroplated with a microporous nickel layer;
[0119] The electroplating solution VI is composed of the following components in weight percentage: CrO3 29%, H2SO4 0.011%, and the balance is water.
[0120] Embodiment 2-6
[0121] A high-gloss electroplating process for an air intake grille is different from that of Example 1 in that the activated colloid used is used differently, and the specific corresponding relationship is shown in the table below.
[0122] Table: Comparison table of activated colloid usage in Examples 2-6
[0123] Group Activated colloid Example 2 Prepared from Preparation Example 2 Example 3 Prepared from Preparation Example 3 Example 4 Prepared by Preparation Example 4 Example 5 Prepared from Preparation Example 5 Example 6 Prepared from Preparation Example 6
[0124] Comparative Example 1
[0125] A high-light electroplating process for an air intake grille is different from Example 1 in that the activated colloid used, calculated based on 100 kg, has the following components and weights: 0.02 kg of palladium chloride, 0.2 kg of tin dichloride, 25 kg of hydrochloric acid and 74.78 kg of water.
[0126] Comparative Example 2
[0127] A high-gloss electroplating process for an air intake grille is different from that in Example 1 in that the activation treatment step in S3 is as follows: immersing the air intake grille to be electroplated in an activated colloid and reacting at 24-72° C. for 2-18 minutes until the surface of the product is completely dark brown.
[0128] The high-gloss air intake grilles prepared in the above-mentioned Examples 1-6 and Comparative Examples 1-2 were selected, and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above-mentioned measurement steps and measurement standards. The average value of the test results was recorded in the following table.
[0129] Table: Test results of high-light plating process performance of air intake grille in Examples 1-6 and Comparative Example 1
[0130]
[0131] It can be seen from the above table that the high-gloss air intake grilles prepared in Examples 1-6 all have excellent surface properties and bonding strength, which are better than those in Comparative Example 1. Their appearance is as high as 9.5-9.8 points, that is, the coating is bright silver-white, with fine crystals and uniform color; the thickness is 24-32um; the corrosion resistance is qualified; and the bonding strength is 5B.
[0132] It can be seen that the activated colloid composed of the above components can not only significantly reduce the loss and preparation cost while ensuring the quality of electroplating, and reduce the palladium content to 0.002-0.003%, but also can form a large number of crystal nuclei for the growth of metal crystals on the non-metallic surface through the compounding of palladium salt, divalent tin, hydrochloric acid and tetrabutylammonium chloride, and under the micro-corrosion of hydrochloric acid and tetrabutylammonium chloride, the catalytic center can be stably and evenly adsorbed in the dovetail holes on the surface of the air intake grille to be electroplated.
[0133] It can also be seen from the above table that Examples 3-5 are preferred embodiments, and the compounding relationship of the components is optimal. The appearance is as high as 9.7-9.8 points, that is, the coating is bright silver-white, the crystals are fine, and the color is uniform; the thickness is 30-32um; the corrosion resistance is qualified; the bonding strength is 5B;
[0134] In addition, it can be seen from Example 4 and Comparative Example 2 that the coating activation used in the present application has higher activation efficiency and more complete reaction than the immersion activation, while effectively saving the amount of activated colloid. The starch, carbon black and dispersant give the activated colloid a certain viscosity, so that it can adhere to the surface of the air intake grille to be electroplated in the form of paint for reaction, and under the above-mentioned operating temperature and conditions, the starch will gradually peel off due to gelatinization and other reasons, and it is not easy to affect the conductivity and surface quality of the conductive film layer.
[0135] Examples 7-12
[0136] A high-gloss electroplating process for an air intake grille is different from that of Example 1 in that the activated colloid used is used differently, and the specific corresponding relationship is shown in the table below.
[0137] Table: Comparison table of activated colloid usage in Examples 7-12
[0138] Group Activated colloid Example 7 Prepared from Preparation Example 7 Example 8 Prepared from Preparation Example 8 Example 9 Prepared from Preparation Example 9 Example 10 Prepared from Preparation Example 10 Embodiment 11 Prepared from Preparation Example 11 Example 12 Prepared from Preparation Example 12
[0139] The high-gloss air intake grilles prepared in the above Examples 7-12 were selected, and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above measurement steps and measurement standards. The average values of the test results were recorded in the following table.
[0140] Table: Test results of high-light electroplating process performance of air intake grille in Examples 7-12
[0141]
[0142] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1, 7-12 all have excellent surface properties and bonding strength, with an appearance score of up to 9.2-9.8 points; a thickness of 24-30um; qualified corrosion resistance; and a bonding strength of 5B.
[0143] It can be seen that the palladium salt composed of the above components, in addition to providing the palladium ions required for the replacement reaction, can also be compounded with other components to allow the reducing ions to maintain their reducing ability for a longer period of time under certain conditions, and allow a large number of crystal nuclei for the growth of metal crystals to form on the non-metallic surface, thereby ensuring the efficient and stable progress of the electroplating operation.
[0144] It can also be seen from the above table that multi-component palladium salts have a certain compounding effect, among which the compounding effect of divalent palladium salts and tetravalent palladium chloride complexes is the most significant, see Examples 11-12, whose appearance is as high as -9.8 points; thickness is 28-30um; corrosion resistance is qualified; bonding strength is 5B; compared with the use of either divalent palladium salt or tetravalent palladium chloride complex alone, it is significantly improved, see Examples 1, 7-10.
[0145] Embodiment 13
[0146] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S1 are as follows:
[0147] S1a, firstly punch and open micro-holes on the side wall of the grille to be plated, wherein the density of opening micro-holes is 3 / cm 2 , the aperture is 0.4mm;
[0148] S1b, then wash and degrease it at 57°C for 3 minutes to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is a 60g / L JF-CL188 aqueous solution.
[0149] Embodiment 14
[0150] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S1 are as follows:
[0151] S1a, firstly punch and open micro-holes on the side wall of the grille to be plated, wherein the density of opening micro-holes is 4 / cm 2 , the aperture is 0.3mm;
[0152] S1b, then wash and degrease it at 60℃ for 4 minutes to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is 80g / L JF-CL188 aqueous solution.
[0153] Embodiment 15
[0154] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S1 are as follows:
[0155] S1a, firstly punch and open micro-holes on the side wall of the grille to be plated, wherein the density of opening micro-holes is 8 / cm 2 , the aperture is 0.3mm;
[0156] S1b, then wash and degrease it at 65°C for 5 minutes to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is a 100g / L JF-CL188 aqueous solution.
[0157] The high-gloss air intake grilles prepared in the above Examples 13-15 were selected, and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above measurement steps and measurement standards. The average value of the test results was recorded in the following table.
[0158] Table: Test results of high-light electroplating process performance of air intake grille in Examples 13-15
[0159]
[0160] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1 and 13-15 all have excellent surface properties and bonding strength, with an appearance score of up to 9.5-9.6 points; a thickness of 28um; qualified corrosion resistance; and a bonding strength of 5B.
[0161] It can be seen that the above-mentioned aqueous degreasing treatment can not only effectively remove harmful substances such as grease, dust and sweat stains on the surface of the air intake grille to be electroplated, thereby ensuring the effect of subsequent process treatments, but also provide binding sites for subsequent electroplating and activation through the micropores opened on the air intake grille to be electroplated.
[0162] In addition, it can be seen from the above table that the influence of various parameters in water-based oil removal on the final performance is relatively low, and various performances are basically stable. However, considering the comprehensive production cost, the optimal micropore opening density is 2-4 / cm 2 , pore size is 0.3-0.5mm; water washing and oil removal are carried out at 54-60℃ for 1.5-4min; and 5-20g / L JF-CL188 aqueous solution.
[0163] Example 16
[0164] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S2 are as follows:
[0165] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 70° C. for 6 minutes until the surface gloss of the product is weakened and roughened, wherein the roughening solution is prepared in Preparation Example 13;
[0166] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 35°C for 0.5 min until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 18.
[0167] Embodiment 17
[0168] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S2 are as follows:
[0169] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 66° C. for 18 minutes until the surface gloss of the product is weakened and becomes rough, wherein the roughening solution is prepared in Preparation Example 14;
[0170] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 18°C for 2 minutes until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 19.
[0171] Embodiment 18
[0172] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S2 are as follows:
[0173] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 66° C. for 18 minutes until the surface gloss of the product is weakened and becomes rough, wherein the roughening solution is prepared in Preparation Example 15;
[0174] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 18°C for 2 minutes until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 20.
[0175] Embodiment 19
[0176] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S2 are as follows:
[0177] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 66° C. for 18 minutes until the surface gloss of the product is weakened and becomes rough, wherein the roughening solution is prepared in Preparation Example 16;
[0178] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 18°C for 2 minutes until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 21.
[0179] Embodiment 20
[0180] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S2 are as follows:
[0181] Then, the pretreated air intake grille to be electroplated is immersed in a roughening solution and subjected to a roughening treatment at 66° C. for 18 minutes until the surface gloss of the product is weakened and roughened, wherein the roughening solution is prepared in Preparation Example 17;
[0182] S2b. The product with reduced gloss and rough surface is then neutralized and reduced at 18°C for 2 minutes until there is no residual roughening liquid on the surface of the product and in the pore walls, wherein the neutralization and reduction liquid is prepared by Preparation Example 22.
[0183] The high-gloss air intake grilles prepared in the above Examples 16-20 were selected and tested for appearance, thickness, coating corrosion resistance and bonding strength according to the above measurement steps and measurement standards. The average values of the test results were recorded in the following table.
[0184] Table: Test results of high-light electroplating process performance of air intake grille in Examples 16-20
[0185]
[0186] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1 and 16-20 all have excellent surface properties and bonding strength, with an appearance score of up to 9.5-9.7 points; a thickness of 28-30um; qualified corrosion resistance; and a bonding strength of 5B. It can be seen that the above-mentioned roughening and neutralization steps can give the air intake grilles excellent electroplating properties, and all properties are basically stable.
[0187] In summary, after the above-mentioned process roughening, the surface gloss of the air intake grille to be electroplated is significantly weakened, and a large number of dense microscopic rough structures (dovetail holes) are formed on the surface, which can significantly increase the contact area and bonding force between the electroplated surface and the air intake grille to be electroplated;
[0188] And when the surface of the electroplated air intake grille is hydrophilic, the reducing property of the solution can be used to reduce and remove the residual chromic acid on the surface of the part in the subsequent reaction with the neutralizing reducing solution, thereby ensuring the normal progress of the subsequent processes and preventing plastic exposure due to residual chromic acid.
[0189] Embodiment 21
[0190] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S3 are as follows:
[0191] First, the activated colloid is applied to the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 100um. Then, it is ultrasonically treated at a power of 100W for 4 minutes until it is homogenized, and the reaction is continued at 48°C for 10 minutes until the surface of the product is completely dark brown, thereby obtaining the activated air intake grille to be electroplated.
[0192] Embodiment 22
[0193] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S3 are as follows:
[0194] First, the activated colloid is applied to the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 150um. Then, it is ultrasonically treated at a power of 120W for 3 minutes until it is homogenized, and the reaction is continued at 72°C for 10 minutes until the surface of the product is completely dark brown, thereby obtaining the activated air intake grille to be electroplated.
[0195] Embodiment 23
[0196] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S3 are as follows:
[0197] First, the activated colloid is applied to the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 200um. Then, it is ultrasonically treated at a power of 150W for 10 minutes until it is homogenized, and the reaction is continued at 90°C for 20 minutes until the surface of the product is completely dark brown, thereby obtaining the activated air intake grille to be electroplated.
[0198] The high-gloss air intake grilles prepared in the above Examples 21-23 were selected and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above measurement steps and measurement standards. The average value of the test results was recorded in the following table.
[0199] Table: Test results of high-light electroplating process performance of air intake grille in Examples 21-23
[0200]
[0201] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1 and 21-23 all have excellent surface properties and bonding strength, with an appearance score of up to 9.3-9.6 points; a thickness of 24-30um; qualified corrosion resistance; and a bonding strength of 5B. It can be seen that the above activation steps can give the air intake grilles excellent electroplating properties.
[0202] In summary, it can be seen that after the activated colloid is sprayed on the surface of the air intake grille to be electroplated, it can effectively ensure the conductivity and surface quality of the conductive film layer. The reason may be that the activated colloid can be evenly and stably adsorbed in the dovetail holes on the surface of the air intake grille to be electroplated under the homogenization effect of ultrasound and the corrosion effect of hydrochloric acid and tetrabutylammonium chloride, thereby providing a catalytic center for the subsequent electroplating reaction, that is, a large number of crystal nuclei for the growth of metal crystals can be formed on the non-metallic surface.
[0203] In addition, it can be seen from the above table that the various parameter conditions during the activation treatment process have an impact on the final performance. After exceeding a specific range, the performance will decrease slightly. Referring to Example 23, the preferred conditions are: coating thickness is 50-150um; 80-120W power ultrasonic treatment for 3-5min; 24-72℃ reaction for 2-18min.
[0204] Embodiment 24
[0205] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S4 are as follows:
[0206] The activated air intake grille to be electroplated is immersed in a debonding agent, treated at 50°C for 6 minutes, and repeated twice until the surface of the product is light brown, to obtain the debonded air intake grille to be electroplated, wherein the debonding agent is a 100ml / L PL-6A aqueous solution.
[0207] Embodiment 25
[0208] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S4 are as follows:
[0209] The activated air intake grille to be electroplated is immersed in a debonding agent, treated at 55°C for 2 minutes, and repeated 3 times until the surface of the product is light brown, thereby obtaining the debonded air intake grille to be electroplated, wherein the debonding agent is a 125ml / L PL-6A aqueous solution.
[0210] Embodiment 26
[0211] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S4 are as follows:
[0212] The activated air intake grille to be electroplated is immersed in a debonding agent and treated at 60° C. for 2 minutes until the surface of the product turns light brown, thereby obtaining the debonded air intake grille to be electroplated, wherein the debonding agent is a 60 ml / L PL-6A aqueous solution.
[0213] The high-gloss air intake grilles prepared in the above Examples 24-26 were selected and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above measurement steps and measurement standards. The average value of the test results was recorded in the following table.
[0214] Table: Test results of high-light electroplating process performance of air intake grille in Examples 24-26
[0215]
[0216]
[0217] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1 and 24-26 all have excellent surface properties and bonding strength, with an appearance score of up to 9.4-9.6 points; a thickness of 26-30um; qualified corrosion resistance; and a bonding strength of 5B. It can be seen that the above-mentioned degumming steps can give the air intake grilles excellent electroplating properties and effectively activate the catalytic activity of palladium.
[0218] In summary, it can be seen that after the above-mentioned debonding treatment, the air intake grille to be electroplated, in addition to the residual binder components on its surface being effectively stripped off, the divalent tin around the palladium can also be dissolved, and the palladium is exposed to the outside, thereby activating the catalytic activity of the palladium. However, it can be seen from the above table that its various parameters must meet specific ranges, otherwise each of them will decrease slightly. Referring to Example 26, the preferred conditions are: treatment at 45-55°C for 2-8min, and repeated 2-3 times; the debonding agent is 75-125ml / L of PL-6A aqueous solution.
[0219] Embodiment 27
[0220] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S4 are as follows:
[0221] S5a, pre-nickel layer:
[0222] First, immerse the debonded air intake grille into the electroplating solution I and place it at a temperature of 50°C and a current density of 1.5A / dm 2 Electroplating for 5 minutes under the conditions of , to obtain the air intake grille to be electroplated with a pre-nickel layer;
[0223] S5b, bright acid copper layer:
[0224] The pre-nickel-plated air intake grille to be electroplated is immersed in electroplating solution II at a temperature of 24°C and a current density of 3A / dm 2 Electroplating for 50 minutes under the conditions of , the air intake grille to be electroplated with a bright acid copper layer is obtained;
[0225] S5c, semi-bright nickel layer:
[0226] The air intake grille to be electroplated with a bright acid copper layer is immersed in electroplating solution III at a temperature of 60°C and a current density of 3A / dm 2 , pH 4.0 for 22 minutes to obtain an air intake grille to be electroplated with a semi-bright nickel layer;
[0227] S5d, bright nickel layer:
[0228] The air intake grille to be electroplated with a semi-bright nickel layer is immersed in electroplating solution IV at a temperature of 58°C and a current density of 3A / dm 2 , pH 4.2 for 15 minutes to obtain an air intake grille to be electroplated with a bright nickel layer;
[0229] S5e, microporous nickel layer:
[0230] The air intake grille to be electroplated with bright nickel layer is immersed in electroplating solution V at a temperature of 58°C and a current density of 3A / dm 2 , electroplating for 5 minutes under the condition of pH 4.2 to obtain the air intake grille to be electroplated with a microporous nickel layer;
[0231] S5f, Chrome plating:
[0232] The air intake grille to be electroplated with a microporous nickel layer is immersed in the electroplating solution VI at a temperature of 40°C and a current density of 10A / dm 2 The electroplating was carried out for 8 minutes under the conditions of , and the air intake grille to be electroplated with a microporous nickel layer was obtained.
[0233] Embodiment 28
[0234] A high-gloss electroplating process for an air intake grille, which is different from that of embodiment 1 in that the specific steps of S4 are as follows:
[0235] S5a, pre-nickel layer:
[0236] First, immerse the debonded air intake grille into the electroplating solution I and place it at a temperature of 55°C and a current density of 1A / dm 2 Electroplating for 4 minutes under the conditions of , to obtain the air intake grille to be electroplated with a pre-nickel layer;
[0237] S5b, bright acid copper layer:
[0238] The pre-nickel-plated air intake grille to be electroplated is immersed in electroplating solution II at a temperature of 26°C and a current density of 2A / dm 2 Electroplating for 40 minutes under the conditions of , the air intake grille to be electroplated with a bright acid copper layer is obtained;
[0239] S5c, semi-bright nickel layer:
[0240] The air intake grille to be electroplated with a bright acid copper layer is immersed in electroplating solution III at a temperature of 60°C and a current density of 2A / dm 2 , pH 3.6 for 20 minutes to obtain an air intake grille to be electroplated with a semi-bright nickel layer;
[0241] S5d, bright nickel layer:
[0242] The air intake grille to be electroplated with a semi-bright nickel layer is immersed in the electroplating solution IV at a temperature of 60°C and a current density of 2A / dm 2 , pH 4.0 for 13 minutes to obtain an air intake grille to be electroplated with a bright nickel layer;
[0243] S5e, microporous nickel layer:
[0244] The bright nickel-plated air intake grille to be electroplated is immersed in electroplating solution V at a temperature of 60°C and a current density of 2A / dm 2 , electroplating for 3 minutes under the condition of pH 4.0 to obtain the air intake grille to be electroplated with a microporous nickel layer;
[0245] S5f, Chrome plating:
[0246] The air intake grille to be electroplated with a microporous nickel layer is immersed in the electroplating solution VI at a temperature of 42°C and a current density of 8A / dm 2 The electroplating was carried out for 5 minutes under the conditions of , and the air intake grille to be electroplated with a microporous nickel layer was obtained.
[0247] The high-gloss air intake grilles prepared in the above Examples 27-28 were selected and their appearance, thickness, coating corrosion resistance and bonding strength were tested according to the above measurement steps and measurement standards. The average value of the test results was recorded in the following table.
[0248] Table: Test results of high-light electroplating process performance of air intake grille in Examples 27-28
[0249]
[0250] It can be seen from the above table that the high-gloss air intake grilles obtained in Examples 1 and 27-28 have excellent surface properties and bonding strength, with an appearance score of up to 9.5-9.6 points; a thickness of 28um; qualified corrosion resistance; and a bonding strength of 5B. It can be seen that when the composition of the electroplating solution is certain, the above-mentioned electroplating process steps can give the air intake grille excellent electroplating properties and ensure the surface performance of the plated parts.
[0251] And from the performance of Examples 1, 27-28, it can be seen that the air intake grille to be electroplated, which is sequentially plated with pre-nickel, bright acid copper, semi-bright nickel, bright nickel, microporous nickel and chromium, has good multi-layer bonding performance. At the same time, the electroplated air intake grille is given excellent surface gloss and corrosion resistance through the composite between coatings with different performances.
[0252] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-gloss electroplating process for an air intake grille, characterized in that: The steps include: S1. Pretreatment: firstly, the side wall of the air intake grille to be electroplated is punched to open micropores, and then the side wall is washed and degreased to obtain the pretreated air intake grille to be electroplated; S2, roughening treatment: then immerse the pre-treated air intake grille to be electroplated in a roughening liquid for roughening treatment, and neutralize it until there is no residual roughening liquid on the surface and the hole wall; S3, activation treatment: coating the activated colloid on the surface of the air intake grille to be electroplated, and after ultrasonic homogenization, reacting at 24-72°C for 2-18 minutes until the surface of the product is completely dark brown, thus obtaining the activated air intake grille to be electroplated; The activated colloid is composed of the following components in weight percentage: 0.002-0.003% palladium salt, 0.2-0.4% divalent tin, 4-6% carbon black, 20-28% starch, 25-30% hydrochloric acid, 1-3% tetrabutylammonium chloride, 0.5-1% stearic acid, and the balance is deionized water; S4, debonding treatment: immerse the activated air intake grille to be electroplated in a debonding agent and extract and rinse repeatedly until the surface of the product turns light brown, thereby obtaining the debonded air intake grille to be electroplated; S5. Electroplating film formation: immerse the air intake grille to be electroplated after debonding into the electroplating solution, and plate pre-plated nickel, bright acid copper, semi-bright nickel, bright nickel, microporous nickel and chromium on the air intake grille to be electroplated in sequence to obtain a high-gloss air intake grille.
2. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The palladium salt is one or more of palladium chloride, palladium sulfate, sodium tetrachloropalladate and diammonium palladium tetrachloride.
3. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The specific steps of S1 are as follows: S1a, firstly punch and open micro-pores on the side wall of the grille to be plated, wherein the density of opening micro-pores is 2-4 / cm 2 , pore diameter is 0.3-0.5mm; S1b, then wash and degrease it at 54-60℃ for 1.5-4min to obtain the pre-treated air intake grille to be electroplated. During the operation, it is necessary to ensure that the surface of the product is completely covered with a water film. The degreasing agent used is a 50-80g / L JF-CL188 aqueous solution.
4. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The specific steps of S2 are as follows: S2a, then immerse the pre-treated air intake grille to be electroplated in the roughening solution, and perform the roughening treatment at 66-70°C for 6-18 minutes until the surface gloss of the product is weakened and roughened: The roughening liquid is composed of the following components in weight percentage: Composition: CrO3 38-44%, H2SO4 38-42%, trivalent chromium salt 0-2%, the balance is water; S2b, then neutralize and reduce the product with reduced gloss and rough surface at 18-35°C for 0.5-2min until there is no residual roughening liquid on the product surface and pore wall; The neutralization reduction solution is composed of the following components in weight percentage: 0.5-3% sodium sulfite, 2-3% HCl, and the balance is water.
5. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The specific steps of S3 are as follows: First, the activated colloid is applied to the surface of the air intake grille to be electroplated by spraying, and the coating thickness is controlled to be 50-150um. Then, it is ultrasonically treated at a power of 80-120W for 3-5min until it is homogenized, and the reaction is continued at 24-72℃ for 2-18min until the surface of the product is completely dark brown, thereby obtaining the activated air intake grille to be electroplated.
6. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The specific steps of S4 are as follows: The activated air intake grille to be electroplated is immersed in a debonding agent, treated at 45-55°C for 2-8 minutes, and repeated 2-3 times until the surface of the product is light brown, to obtain the debonded air intake grille to be electroplated, wherein the debonding agent is 75-125ml / L PL-6A aqueous solution.
7. The high-gloss electroplating process for the air intake grille according to claim 1, characterized in that: The specific steps of S5 are as follows: S5a, pre-nickel plating layer: First, immerse the debonded air intake grille into the electroplating solution I and heat it at a temperature of 45-55°C and a current density of 1-1.5 A / dm 2 Electroplating for 4-6 minutes under the conditions of , the air intake grille to be electroplated with a pre-nickel layer is obtained; The electroplating solution I is composed of the following components in weight percentage: Composition: NiSO4 22-26%, NiCl2 4.0-5.5%, H3BO3 4.0-5.5%, the balance is water; S5b, bright acid copper layer: Immerse the pre-nickel-plated air intake grille in the electroplating solution II at a temperature of 22-26°C and a current density of 2-4 A / dm 2 Electroplating for 40-60 minutes under the conditions of , the air intake grille to be electroplated with a bright acid copper layer is obtained; The electroplating solution II is composed of the following components in percentage by weight: Composition: CuSO4 18-22%, H2SO4 6.0-7.5%, the balance is water; S5c, semi-bright nickel layer: Immerse the air intake grille to be electroplated with a bright acid copper layer into electroplating solution III at a temperature of 55-60°C and a current density of 2-4A / dm 2 , electroplating for 20-23 minutes at pH 3.6-4.2 to obtain an air intake grille to be electroplated with a semi-bright nickel layer; The electroplating solution III is composed of the following components in percentage by weight: Composition: NiSO4 28-32%, NiCl2 3.5-4.5%, H3BO3 3.5-4.5%, the balance is water; S5d, bright nickel layer: Immerse the air intake grille to be electroplated with a semi-bright nickel layer in electroplating solution IV at a temperature of 55-60°C and a current density of 2-5A / dm 2 , electroplating for 13-16 minutes at pH 4.0-4.5 to obtain an air intake grille to be electroplated with a bright nickel layer; The electroplating solution IV is composed of the following components in weight percentage: Composition: NiSO4 28-32%, NiCl2 4.0-7.0%, H3BO3 4.0-5.0%, the balance is water; S5e, microporous nickel layer: Immerse the bright nickel-plated air intake grille into the electroplating solution V at a temperature of 55-60°C and a current density of 2-4 A / dm 2 , electroplating for 3-6 minutes under the condition of pH 4.0-4.5 to obtain the air intake grille to be electroplated with a microporous nickel layer; The electroplating solution V is composed of the following components in percentage by weight: Composition: NiSO4 28-32%, NiCl2 6.0-9.0%, H3BO3 4.0-5.0%, the balance is water; S5f, Chrome plating: Immerse the air intake grille to be electroplated with a microporous nickel layer in electroplating solution VI at a temperature of 38-42°C and a current density of 8-15A / dm 2 Electroplating for 5-10 minutes under the conditions of , the air intake grille to be electroplated with a microporous nickel layer is obtained; The electroplating solution VI is composed of the following components in percentage by weight: Composition: CrO3 26-32%, H2SO4 0.08-0.14%, and the balance is water.
Citation Information
Patent Citations
Electroplating method for spraying and activating of surface of ABS plastic
CN106567114A
Trivalent white chromium and pearl nickel electroplating technology
CN107475714A