A flotation recovery method for high calcium, magnesium and high clay zinc carbonate

By using a combination of specific ore mud collectors and gangue inhibitors in zinc oxide ore, multiple flotations and sweeps are performed, the flotation problem caused by high calcium, magnesium and high mud in zinc oxide ore is solved, and high efficiency is achieved mineral recovery and concentrate grade enhancement.

CN114798185BActive Publication Date: 2024-11-08NORTHWEST RES INST OF MINING & METALLURGY INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210395531.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-15
Publication Date
2024-11-08
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

The presence of high calcium, magnesium and high mud in zinc oxide ore results in complex mineral surface properties, making it difficult to effectively inhibit ganglite and desilt through a single inhibitor, affecting the flotation characteristics and recycling efficiency.

Method used

Desludge flotation using lead-zinc sulfide flotation tailings, using ore sludge collectors (nitrosoammonium nitrosac, modified low-temperature flotation oleic acid, polypropylene glycol alkyl ether) and gangliaceous inhibitors (BN) Ammonium aminetetraacetate, sodium hexametaphosphate, sodium tripolyphosphate, sodium polyhydroxyacetate) combines multiple flotations and sweeps to optimize the slurry environment to improve the flotation effect of zinc oxide.

Benefits of technology

It realizes efficient separation of mineral mud and gangue, reduces agent consumption, improves the flotation recovery rate and concentrate grade of zinc oxide, reduces mineral losses, and simplifies subsequent dehydration operations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114798185B_ABST
    Figure CN114798185B_ABST
Patent Text Reader

Abstract

The present invention relates to a flotation recovery method for high calcium and magnesium high mud zinc carbonate, which comprises the following steps: (1) desludging flotation: using sulfide lead zinc flotation tailings as raw ore, adding a sludge collector, stirring and reacting for 3 to 6 minutes, and then desludging before zinc oxide flotation to obtain muddy pulp and desludging tailings pulp respectively; (2) zinc oxide roughing: adding adjusting agents sodium carbonate, sodium sulfide, gangue inhibitor, dodecylamine acetate and butyl xanthate to the desludging tailings pulp to carry out zinc roughing, respectively obtaining zinc rough concentrate pulp and roughing tailings pulp; (3) zinc oxide concentration: the zinc rough concentrate pulp is subjected to two concentration operations to obtain zinc oxide concentrate; (4) zinc oxide scavenging: the roughing tailings pulp is subjected to one zinc oxide scavenging operation to obtain zinc oxide scavenging tailings. The present invention can significantly enhance the floatability of zinc oxide minerals and obtain better mineral processing technical indicators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral flotation separation in nonferrous metal beneficiation, and in particular to a flotation recovery method for high-calcium, magnesium and high-mud zinc carbonate. Background Art

[0002] The ore composition of zinc oxide mines in my country is relatively complex. Gangue coexists with useful minerals, the zinc grade is low, mud is serious and desludging is difficult. Gangue coexists with useful minerals in many types and small particle sizes. It is difficult to achieve effective inhibition with a single inhibitor, which makes it difficult to enrich and efficiently recover zinc oxide minerals. At the same time, there are a large number of soluble salts in the oxide ore. After the soluble salts are dissolved, they are adsorbed on the surface of the target mineral, changing the surface properties of the mineral such as electrical properties and wettability. The change in the surface properties of the mineral directly affects the flotation characteristics of the mineral. Some conventional flotation processes and flotation reagents are difficult to adapt to the complex and changeable properties of zinc oxide mines. Therefore, under the multiple influences of factors such as ore mud, gangue and soluble salts, the difficulty of recovering zinc oxide will be greatly increased.

[0003] Flotation is one of the main methods for recovering zinc oxide ore. The main methods for flotation of smithsonite are sulfide-xanthate method, sulfide-amine method, fatty acid method, chelate flotation method and other flotation methods. The most effective flotation of zinc oxide ore in China is the sulfide-amine salt flotation method; the sulfide xanthate flotation method requires the addition of an activator before the zinc oxide ore is heated and sulfided, and the consumption of the chemical agent is large in some flotation processes, so it is not widely used in industry; fatty acid collectors have poor selectivity for zinc oxide ores with a large mud content, so they are almost not used in industry. The sulfide-first and then amine flotation method is currently a more effective method for recovering zinc oxide from mineral processing. This method is suitable for the flotation of zinc carbonate, with sodium sulfide as the activator and primary amine as the collector. This method does not require heating.

[0004] The flotation conditions of zinc oxide ore can be effectively improved by pre-de-sliming the ore when flotating zinc oxide ore by sulfidation-amine method. The primary ore slime content of the oxidized ore is large and the hardness is low. The secondary ore slime produced in the process of grinding the ore has a large specific surface area and fine particle size. Some of the fine ore slime exists in a colloidal state and can be well adsorbed on the flotation reagent. If it is not pre-removed, the amount of reagent consumed will be greatly increased, which will hinder the interaction between the collector and the lead-zinc oxide minerals and affect the concentrate recovery rate and grade. Therefore, de-sliming treatment and effective suppression of gangue before flotation of zinc oxide ore have attracted more and more attention, and it is also an urgent problem to be solved in the flotation of zinc carbonate minerals by sulfidation-amine method. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a flotation recovery method for high-calcium-magnesium-high-mud zinc carbonate with significant effect.

[0006] In order to solve the above problems, the present invention provides a flotation recovery method for high calcium and magnesium high clay zinc carbonate, comprising the following steps:

[0007] ⑴ Desludging flotation:

[0008] The lead-zinc sulfide flotation tailings are used as the raw ore, and a slime collector is added in an amount of 50-80 g / t according to the dry weight of the raw ore, and the mixture is stirred for reaction for 3-6 minutes before desliming before zinc oxide flotation to obtain a slime-containing pulp and a deslimed tailings pulp, respectively.

[0009] ⑵Zinc oxide roughing:

[0010] In the tailings slurry after desliming, add 800-1000 g / t of sodium carbonate as an adjusting agent, 5000-10000 g / t of sodium sulfide, 1000-1500 g / t of gangue inhibitor, 60-80 g / t of dodecylamine acetate and 10-20 g / t of butyl xanthate to carry out zinc roughing, and obtain zinc rough concentrate slurry and roughing tailings slurry respectively;

[0011] ⑶ Zinc oxide selection:

[0012] The zinc rough concentrate slurry is subjected to two concentration operations to obtain zinc oxide concentrate;

[0013] ⑷Zinc oxide screening:

[0014] The roughing tailings slurry is subjected to a zinc oxide scavenging operation to obtain zinc oxide scavenging tailings.

[0015] In the step (1), the zinc content in the lead-zinc sulfide flotation tailings is ≤3.0%, the zinc oxidation rate is ≥80%, the magnesium oxide content is >15%, the calcium oxide content is >15%, and the -10 μm particle size content is ≥35%.

[0016] The sludge collector in step (1) refers to a homogeneous oily solution formed by mixing the following raw materials in parts by weight in a stirred tank at room temperature and pressure for 1.5 to 2 hours: 20 to 30 parts of nitrosonaphthylamine, 55 to 60 parts of modified low-temperature flotation oleic acid, and 15 to 20 parts of polypropylene glycol alkyl ether.

[0017] In the step (2), the stone inhibitor refers to mixing ammonium ethylenediaminetetraacetate, sodium hexametaphosphate, sodium tripolyphosphate, and sodium polyhydroxyacetate in a weight ratio of 2-4:2:3:1, and adding water to prepare a solution with a mass concentration of 5%-10%.

[0018] The two concentration operations in step (3) refer to adding 400-600 g / t of gangue inhibitor to the zinc rough concentrate slurry for a flotation operation based on the dry weight of the raw ore, respectively obtaining a primary concentrate slurry and a primary concentrated middling, which is returned to step (2) of zinc oxide roughing; and performing a secondary flotation operation on the primary concentrate slurry without adding any reagent, respectively obtaining a zinc concentrate and a secondary concentrated middling, which is returned to the primary concentration operation in step (3).

[0019] The zinc scavenging operation in step (4) refers to adding 1000-2000 g / t of sodium sulfide and 10-20 g / t of collector dodecylamine acetate to the roughing tailings slurry according to the dry weight of the raw ore to carry out a zinc scavenging operation, respectively obtaining the zinc oxide scavenging tailings and the primary scavenging ore, and the primary scavenging ore enters the step (2) zinc oxide roughing.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The ore slime collector of the present invention is made of nitroso-naphthoic acid ammonium, modified low-temperature flotation oleic acid, and polypropylene glycol alkyl ether. Therefore, no adjusting agent needs to be added during desliming, and efficient flotation separation of ore slime and smithsonite can be achieved, and the loss of zinc oxide minerals in the deslimed concentrate is relatively small. At the same time, the collector can increase the surface difference of the sorted particles, effectively prevent the mutual coagulation of fine ore particles and coarse ore particles, reduce the competitive adsorption of ore slime and collector, and increase the adsorption amount of collector on the surface of zinc oxide minerals during subsequent zinc oxide flotation, providing a relatively good pulp flotation environment for subsequent zinc oxide flotation; in addition, the removal of ore slime can reduce the stability of flotation foam, shorten the half-life of flotation foam, and facilitate the subsequent dehydration of zinc oxide concentrate.

[0022] ⑴ Nitrosonaphthalene ammonium is an iron oxide mineral collector, which can prevent the dissolution of Fe from fine-grained iron oxide minerals (mainly limonite) 3+ , Fe 2+ In the form of hydroxyl complex or with OH in the pulp — The generated hydroxide precipitate covers the surface of smithsonite, which makes the surface hydrophilicity of smithsonite enhanced.

[0023] ⑵ Modified low-temperature flotation oleic acid can effectively remove calcium-magnesium gangue fine mud; at the same time, modified low-temperature flotation oleic acid can react with Ca in the pulp 2+ Mg 2+ (In order to adjust the pH value of the ore pulp during zinc sulfide flotation, a large amount of lime and calcium-magnesium gangue are often added. A large amount of Ca2+ is also dissolved during the grinding and flotation process. 2+ Mg 2+ ) react to generate fatty acid calcium and fatty acid magnesium, preventing Ca in the slurry 2+ Mg 2+The activation of quartz results in a low concentrate grade; Ca in the slurry 2+ Mg 2+ After the concentration is reduced, the negative charge on the surface of smithsonite is enhanced, which can significantly increase the adsorption amount of amine collectors on its surface; at the same time, the modified low-temperature oleic acid has a wider adaptability to slurry temperature and can also play a good role in collecting calcium-magnesium gangue fine mud in low-temperature slurry.

[0024] ⑶ The polar group of polypropylene glycol alkyl ether is an inert group with relatively stable chemical properties. It is insensitive to the inevitable ions in the ore pulp. When used in combination with nitrosonaphthalene ammonium hydroxylamine and modified low-temperature flotation oleic acid, the foam is fine and not easy to merge. It has a strong load capacity for ore mud, moderate flotation foam stability, and little effect on the subsequent zinc oxide flotation foam.

[0025] 2. The gangue inhibitor in the present invention is made of ammonium ethylenediaminetetraacetate, sodium hexametaphosphate, sodium tripolyphosphate and sodium polyhydroxyacetate. The inhibitor has a strong inhibitory effect on calcium-magnesium gangue, and can enhance the difference in floatability between calcium-magnesium gangue minerals and zinc oxide minerals; at the same time, the inhibitor can enhance the electronegativity of the surface of the ore particles, increase the repulsive force between the ore particles, make the surface of the gangue mineral present a strong hydrophilicity, prevent the aggregation of the ore particles, and make it easier for sodium sulfide to form a sulfide film on the surface of the zinc oxide mineral, thereby significantly enhancing the floatability of the zinc oxide mineral.

[0026] ⑴ EDTA promotes the surface Zn 2+ The dissolution of EDTA can reduce the potential of the mineral surface, thereby improving the flotation recovery rate of smithsonite. EDTA exists in the solution as an anion, which can react with Zn on the surface of smithsonite. 2+ Chelate and form a stable water-soluble chelate, which is easier to transfer into the slurry, making the CO 3 2- The exposure enhances the negative charge of the smithsonite surface, which is beneficial to the adsorption of cationic collectors on the smithsonite surface.

[0027] (2) Sodium hexametaphosphate is adsorbed on the surface of the mineral in the form of negative ions in alkaline minerals, which increases the electronegativity of the mineral surface. Negatively charged minerals are separated from each other due to the electrostatic repulsion, and the adsorption of amine collectors on the mineral surface is enhanced. The complex anions formed by sodium hexametaphosphate in the slurry can be selectively adsorbed on the surface of calcium-magnesium gangue minerals to enhance their surface hydrophilicity.

[0028] ⑶ Effect of sodium tripolyphosphate on Ca in slurry 2+ Mg 2+ It has strong chelating effect and is easy to bind with Ca 2+ Mg 2+ Form a complex and adsorb on the surface of calcium-magnesium gangue particles, change the surface electrical properties of calcium-magnesium gangue particles, inhibit Ca2+ Mg 2+ dissolution, reducing the Ca content in the slurry 2+ Mg 2+ content, enhancing the hydrophilicity of calcium-magnesium gangue.

[0029] (4) Sodium polyhydroxy acetate is adsorbed on the surface of calcite and magnesite through carboxyl groups. Its multiple hydroxyl groups combine with water molecules through hydrogen bonds to form a water film, which has a strong inhibitory effect on calcium-magnesium gangue. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0031] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0032] like Figure 1 As shown, a flotation recovery method for high calcium and magnesium high clay zinc carbonate comprises the following steps:

[0033] ⑴ Desludging flotation:

[0034] The sulfide lead-zinc flotation tailings are used as the original ore. According to the dry weight of the original ore, 50-80 g / t of the slime collector is added. After stirring for 3-6 minutes, desliming is carried out before zinc oxide flotation to obtain muddy slurry and deslimed tailings slurry (for zinc oxide flotation).

[0035] Among them: the zinc content in the sulfide lead-zinc flotation tailings is ≤3.0%, the zinc oxidation rate is ≥80%, the magnesium oxide content is >15%, the calcium oxide content is >15%, and the -10μm particle size content is ≥35%.

[0036] The sludge collector refers to a homogeneous oily solution formed by mixing the following raw materials in parts by weight (g) in a stirred kettle at room temperature and pressure for 1.5 to 2 hours: 20 to 30 parts of nitrosonaphthylamine ammonium, 55 to 60 parts of modified low-temperature flotation oleic acid, and 15 to 20 parts of polypropylene glycol alkyl ether.

[0037] Nitrosonaphthoic acid ammonium, namely N-nitrosonaphthoic acid ammonium, is a new cupraloline reagent synthesized on the basis of cupraloline reagent.

[0038] Modified low-temperature flotation oleic acid is a conventional collector produced by Hebei Weixian Hengchuang Mineral Products Co., Ltd.

[0039] Polypropylene glycol alkyl ether is a conventional ether reagent. For details, please refer to Table 11-22 on P604 of Mining Reagents (written by Zhang Jingsheng and Que Xuanlan, published by Metallurgical Industry Press).

[0040] ⑵Zinc oxide roughing:

[0041] In the tailings slurry after desliming, adjusters such as sodium carbonate 800-1000 g / t, sodium sulfide 5000-10000 g / t, gangue inhibitor 1000-1500 g / t, dodecylamine acetate 60-80 g / t and butyl xanthate 10-20 g / t are added for zinc roughing to obtain zinc rough concentrate slurry and roughing tailings slurry, respectively.

[0042] Among them: the gangue inhibitor refers to the mixture of ammonium ethylenediaminetetraacetate, sodium hexametaphosphate, sodium tripolyphosphate and sodium polyhydroxyacetate in a weight ratio (g / g) of 2~4:2:3:1, and adding water to form a solution with a mass concentration of 5%~10%.

[0043] Sodium polyglycolate is the reaction product of polyglycolic acid and sodium salt and is a conventional chemical agent.

[0044] ⑶ Zinc oxide selection:

[0045] The zinc rough concentrate pulp undergoes two concentration operations to obtain zinc oxide concentrate. The specific process is as follows:

[0046] The double concentration operation refers to adding 400-600 g / t of gangue inhibitor to the zinc rough concentrate slurry for a flotation operation based on the dry ore weight of the original ore, respectively obtaining a primary concentrate slurry and a primary concentrated middling ore, which is returned to step (2) zinc oxide roughing; and performing a secondary flotation operation on the primary concentrate slurry without adding any reagents, respectively obtaining a zinc concentrate and a secondary concentrated middling ore, which is returned to step (3) of the primary concentration operation.

[0047] ⑷Zinc oxide screening:

[0048] The roughing tailings slurry is subjected to a zinc oxide scavenging operation to obtain zinc oxide scavenging tailings. The specific process is as follows:

[0049] The primary zinc scavenging operation refers to adding 1000-2000 g / t of sodium sulfide and 10-20 g / t of collector dodecylamine acetate to the roughing tailings slurry according to the dry ore weight of the original ore to carry out a primary zinc scavenging operation to obtain zinc oxide scavenging tailings and primary scavenging ore respectively, and the primary scavenging ore enters step (2) zinc oxide roughing.

[0050] Embodiment 1:

[0051] The Zn content in a sulfide lead-zinc flotation tailing in Sichuan is about 1.50%, the zinc minerals are mainly smithsonite, followed by hemimorphite, hydrozincite, etc., the zinc oxidation rate is 80%, the main gangue minerals are quartz, calcite, dolomite, chlorite, mica, etc., the CaO and MgO contents in the ore sample are relatively high, and the calcium and magnesium gangue minerals are very easy to be muddy, wherein the CaO content is 24.3%, the MgO content is 18.2%, and the -10μm particle size content reaches 40.5%, which belongs to high calcium and magnesium high mud zinc tailings. The closed circuit test results of Example 1 are shown in Table 1.

[0052] The specific process is as follows:

[0053] ⑴ Desludging flotation:

[0054] The lead-zinc sulfide flotation tailings are used as the raw ore, and 50 g / t of the slime collector (a) is added according to the dry weight of the raw ore. After stirring for 3 to 6 minutes, desliming is performed before zinc oxide flotation to obtain muddy slurry and deslimed tailings slurry (for zinc oxide flotation), respectively.

[0055] Wherein: the sludge collector refers to a homogeneous oily solution formed by mixing 30 g of nitrosonaphthylamine ammonium, 55 g of modified low-temperature flotation oleic acid, and 15 g of polypropylene glycol alkyl ether in a stirred tank at room temperature and pressure for 1.5 to 2 hours.

[0056] ⑵Zinc oxide roughing:

[0057] In the tailings slurry after desliming, adjusting agents sodium carbonate (b) 800 g / t, sodium sulfide (c) 5000 g / t, gangue inhibitor (d) 1000 g / t, dodecylamine acetate (e) 60 g / t and butyl xanthate (f) 10 g / t were added for zinc roughing to obtain zinc rough concentrate slurry and roughing tailings slurry, respectively.

[0058] Among them: the gangue inhibitor refers to mixing 2 g of ammonium ethylenediaminetetraacetate, 2 g of sodium hexametaphosphate, 3 g of sodium tripolyphosphate, and 1 g of sodium polyhydroxyacetate evenly, and adding water to make a solution with a mass concentration of 5%~10%.

[0059] ⑶ Zinc oxide selection:

[0060] The zinc rough concentrate pulp undergoes two concentration operations to obtain zinc oxide concentrate. The specific process is as follows:

[0061] The double concentration operation means that according to the dry weight of the original ore, 400g / t of gangue inhibitor is added to the zinc rough concentrate slurry for a flotation operation to obtain a primary concentrate slurry and a primary concentrated middling ore respectively, and the primary concentrated middling ore is returned to step (2) zinc oxide roughing; the primary concentrate slurry is subjected to a secondary flotation operation without adding any reagents to the primary concentrate slurry to obtain a zinc concentrate and a secondary concentrated middling ore respectively, and the secondary concentrated middling ore is returned to the primary concentration operation of step (3).

[0062] ⑷Zinc oxide screening:

[0063] The roughing tailings slurry is subjected to a zinc oxide scavenging operation to obtain zinc oxide scavenging tailings. The specific process is as follows:

[0064] The primary zinc scavenging operation refers to adding 1000 g / t of sodium sulfide (c) and 10 g / t of collector dodecylamine acetate (e) to the roughing tailings slurry according to the dry ore weight of the raw ore to carry out a primary zinc scavenging operation to obtain zinc oxide scavenging tailings and primary scavenging ore respectively, and the primary scavenging ore enters step (2) zinc oxide roughing.

[0065] Embodiment 2:

[0066] The Zn content in a sulfide lead-zinc flotation tailing in Gansu is about 3.0%, the oxidation rate of zinc is 90%, of which the CaO content is 19.5%, the MgO content is 16.8%, and the -10μm particle size content reaches 35.0%. The main metal minerals in the ore sample are smithsonite, willemite, hemimorphite, limonite, cerussite, sphalerite, galena, etc., and the gangue minerals are mainly quartz, dolomite, calcite, clay minerals, sericite, kaolin, etc. The gangue minerals mica and clay minerals have good floatability, which will increase the use of flotation reagents and reduce the grade of zinc concentrate during the flotation process. The closed-circuit test results of Example 2 are shown in Table 1.

[0067] The specific process is as follows:

[0068] ⑴ Desludging flotation:

[0069] The lead-zinc sulfide flotation tailings are used as the raw ore, and 50 g / t of the slime collector (a) is added according to the dry weight of the raw ore. After stirring for 3 to 6 minutes, desliming is performed before zinc oxide flotation to obtain muddy slurry and deslimed tailings slurry (for zinc oxide flotation), respectively.

[0070] Wherein: the sludge collector refers to a homogeneous oily solution formed by mixing 20 g of nitrosonaphthylamine ammonium, 60 g of modified low-temperature flotation oleic acid, and 20 g of polypropylene glycol alkyl ether in a stirred tank at room temperature and pressure for 1.5 to 2 hours.

[0071] ⑵Zinc oxide roughing:

[0072] In the tailings slurry after desliming, adjusting agents sodium carbonate (b) 1000 g / t, sodium sulfide (c) 10000 g / t, gangue inhibitor (d) 1500 g / t, dodecylamine acetate (e) 80 g / t and butyl xanthate (f) 20 g / t were added for zinc roughing to obtain zinc rough concentrate slurry and roughing tailings slurry, respectively.

[0073] Among them: the gangue inhibitor refers to mixing 4 g of ammonium ethylenediaminetetraacetate, 2 g of sodium hexametaphosphate, 3 g of sodium tripolyphosphate, and 1 g of sodium polyhydroxyacetate evenly, and adding water to make a solution with a mass concentration of 5%~10%.

[0074] ⑶ Zinc oxide selection:

[0075] The zinc rough concentrate pulp undergoes two concentration operations to obtain zinc oxide concentrate. The specific process is as follows:

[0076] The double concentration operation means that according to the dry weight of the original ore, 600g / t of gangue inhibitor is added to the zinc rough concentrate slurry for a flotation operation to obtain a primary concentrate slurry and a primary concentrated middling ore respectively, and the primary concentrated middling ore is returned to step (2) zinc oxide roughing; the primary concentrate slurry is subjected to a secondary flotation operation without adding any reagents to the primary concentrate slurry to obtain a zinc concentrate and a secondary concentrated middling ore respectively, and the secondary concentrated middling ore is returned to the primary concentration operation of step (3).

[0077] ⑷Zinc oxide screening:

[0078] The roughing tailings slurry is subjected to a zinc oxide scavenging operation to obtain zinc oxide scavenging tailings. The specific process is as follows:

[0079] The primary zinc scavenging operation refers to adding 2000g / t of sodium sulfide (c) and 20g / t of collector dodecylamine acetate (e) to the roughing tailings slurry according to the dry ore weight of the original ore to carry out a primary zinc scavenging operation to obtain zinc oxide scavenging tailings and primary scavenging ore respectively, and the primary scavenging ore enters step (2) zinc oxide roughing.

[0080] Table 1 Technical indicators of closed-circuit ore dressing in Examples 1 and 2 of the present invention

[0081] The test results in Table 1 show that both Example 1 and Example 2 of the present invention achieve good mineral processing technical indicators. In order to compare with the closed-circuit results of Example 1 of the present invention, the desludging technical solution (xanthate, 2 # The mineral processing technical indicators of the technical solutions of desludging with and without desludging are listed.

[0082] Comparative Example 1:

[0083] The sulfide lead-zinc flotation tailings of the same grade in Example 1 were deslimed, and the products produced included deslimed pulp and deslimed tailings pulp. The sludge collector used a conventional agent for desliming, and the test results were compared with the desliming collector of the present invention. In the comparative example, the sulfide lead-zinc flotation tailings were used as the original ore for desliming flotation operation, and other reagent conditions were as shown in Example 1. The test comparison results of the conventional collector and the collector of the present invention in the desliming flotation operation of the sulfide lead-zinc flotation tailings are shown in Table 2.

[0084] Table 2 Comparison of test results of conventional collectors and collectors of the present invention in desludging flotation operations

[0085] The test results in Table 2 show that when the desludging agent dosage is 60 g / t, the yield of the ore mud of the collector of the present invention is basically the same as that of the conventional desludging agent and the desludging agent scheme used on site, but the zinc content in the ore mud is quite different. The zinc grade in the ore mud removed by the ore mud collector of the present invention is only 1.74%, and the loss of zinc metal in the desludging operation is relatively small.

[0086] Comparative Example 2:

[0087] After desliming the sulfide lead-zinc flotation tailings of the same grade as in Example 1, the deslimed tailings slurry was subjected to zinc roughing. Conventional depressants were used in the zinc roughing operation, and the test results were compared with the depressants of the present invention. In the comparative example, the deslimed tailings slurry was used as feed ore to carry out zinc flotation operation, and other reagent conditions were as shown in Example 1. The test comparison results of the conventional depressants and the depressants of the present invention in the zinc roughing operation of the sulfide lead-zinc flotation tailings are shown in Table 3.

[0088] Table 3 Comparison of test results of conventional inhibitors and inhibitors of the present invention in zinc roughing operation

[0089] The test results in Table 3 show that, under the condition of equivalent zinc grade in the feed ore, in zinc roughing operation, the inhibitor of the present invention is superior to conventional inhibitors and inhibitor solutions used on site in zinc rough concentrate and operation recovery rate indicators.

Claims

1. A flotation recovery method for high calcium and magnesium high clay zinc carbonate, comprising the following steps: ⑴ Desliming flotation: The lead-zinc sulfide flotation tailings are used as the raw ore, and a sludge collector is added in an amount of 50-80 g / t according to the dry weight of the raw ore, and the mixture is stirred for reaction for 3-6 minutes before desliming before zinc oxide flotation to obtain a sludge-containing pulp and a desludged tailing pulp, respectively; the zinc content in the lead-zinc sulfide flotation tailings is ≤3.0%, the zinc oxidation rate is ≥80%, the magnesium oxide content is >15%, the calcium oxide content is >15%, and the -10 μm particle size content is ≥35%; the sludge collector refers to a homogeneous oily solution formed by stirring and mixing the following raw materials in parts by weight in a stirred tank at room temperature and pressure for 1.5-2 hours: 20-30 parts of nitrosonaphthylamine ammonium, 55-60 parts of modified low-temperature flotation oleic acid, and 15-20 parts of polypropylene glycol alkyl ether; ⑵Zinc oxide roughing: In the tailings slurry after desliming, adjusting agents such as sodium carbonate 800-1000 g / t, sodium sulfide 5000-10000 g / t, gangue inhibitor 1000-1500 g / t, dodecylamine acetate 60-80 g / t and butyl xanthate 10-20 g / t are added to carry out zinc roughing to obtain zinc rough concentrate slurry and roughing tailings slurry respectively; the gangue inhibitor refers to ammonium ethylenediaminetetraacetate, sodium hexametaphosphate, sodium tripolyphosphate and sodium polyglycolate mixed in a weight ratio of 2-4:2:3:1, and water is added to form a solution with a mass concentration of 5%-10%; ⑶ Zinc oxide selection: The zinc rough concentrate slurry is subjected to two concentration operations to obtain zinc oxide concentrate; ⑷Zinc oxide screening: The roughing tailings slurry is subjected to a zinc oxide scavenging operation to obtain zinc oxide scavenging tailings.

2. A flotation recovery method for high calcium and magnesium high clay zinc carbonate according to claim 1, characterized in that: The two concentration operations in step (3) refer to adding 400-600 g / t of gangue inhibitor to the zinc rough concentrate slurry for a flotation operation based on the dry weight of the raw ore, respectively obtaining a primary concentrate slurry and a primary concentrated middling, which is returned to step (2) of zinc oxide roughing; and performing a secondary flotation operation on the primary concentrate slurry without adding any reagent, respectively obtaining a zinc concentrate and a secondary concentrated middling, which is returned to the primary concentration operation in step (3).

3. A flotation recovery method for high calcium and magnesium high clay zinc carbonate according to claim 1, characterized in that: The zinc scavenging operation in step (4) refers to adding 1000-2000 g / t of sodium sulfide and 10-20 g / t of collector dodecylamine acetate to the roughing tailings slurry according to the dry weight of the raw ore to carry out a zinc scavenging operation, respectively obtaining the zinc oxide scavenging tailings and the primary scavenging ore, and the primary scavenging ore enters the step (2) zinc oxide roughing.