A method for preparing nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength

The nano-micron particle composite hydrogel is prepared by wet grinding of nano carbon fiber and active industrial solid waste, which solves the problem of insufficient strength and water absorption capacity of the hydrogel, achieves efficient utilization of industrial solid waste resources and improves gel strength, extending the shorten the life cycle and reduce production costs.

CN114805857BActive Publication Date: 2024-10-29HUBEI UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210544118.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-10-29
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

Existing hydrogels have low strength, poor toughness, and are easily broken after absorbing water, resulting in a short life cycle and limited application. Moreover, the economic benefits and mechanical properties of existing nanoparticle composites are low.

Method used

Nano-carbon fiber and active industrial solid waste (such as blast furnace slag, fly ash) are used to prepare nano-micron particle composite hydrogel through wet grinding. Carbide slag grinding aid and acrylic acrylamide cross-linking agent are used to increase the cross-linking density and toughness.

Benefits of technology

It significantly improves the water absorption and storage capacity and gel strength of the hydrogel, extends the life cycle, realizes the resource utilization of industrial solid waste, reduces production costs and environmental pollution, and the process is simple and easy to adjust.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of water-absorbing gel materials, and in particular to a method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength, comprising the following steps: weighing nano-carbon fibers, active industrial solid waste, carbide slag, water, grinding aid balls, and a dispersant, and filtering to obtain a nano-micron particle grinding liquid after wet grinding; dissolving sodium hydroxide in water to obtain an alkaline solution, diluting acrylic acid with water and adding it to the alkaline solution, adding acrylamide to mix after the solution temperature is cooled to room temperature, and then adding a cross-linking agent and an initiator to continue stirring to obtain a hydrogel solution; taking the nano-micron particle grinding liquid and adding it to the hydrogel solution, stirring until the mixture is uniformly mixed; drying and crushing the mixture after the mixture is completely reacted at a certain temperature. The invention uses carbide slag to assist grinding, stimulates the activity of active industrial solid waste, has better adhesion and certain tensile strength and toughness, and improves the life cycle of the hydrogel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-absorbing gel materials, and in particular to a method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength. Background Art

[0002] Water-absorbent gel is a polymer that is widely used in various fields of daily life. Due to the action of hydrophilic groups such as -COOH, -OH, -CO-NH, and -NH2 in water and hydrogen bonds, it can absorb hundreds or thousands of times its dry weight of water. It is a water-insoluble gel with a three-dimensional cross-linked network hydrophilic structure. It can absorb and store a certain amount of water in different environments under a certain pressure. Therefore, it is used in medical care, agriculture, and construction industries.

[0003] In existing reports, there have been many studies on highly absorbent hydrogels, but the gel strength of the hydrogel after absorbing water is relatively low. While increasing the water absorption and water storage capacity of the hydrogel, there are few studies on strengthening the gel strength. Because the existing gels are generally low in strength and poor in toughness, although the gel has a certain water retention after absorbing water, it is easy to break. The existence of this problem makes the hydrogel material fragile and has a short life cycle, resulting in many products being disposable. For example, when used in dehydrating agents, plant water retaining agents, cement-based building materials and other materials, the gel will break after being squeezed or stirred to a certain extent, which not only causes a part of the water to be lost, but also causes defects in the water absorption and water retention of the material. These problems greatly limit the application scenarios of hydrogels. The present invention not only toughens the gel, but also improves the water absorption and water storage capacity of the gel, improves the vitality of the hydrogel, and allows the gel to be more conveniently recycled in some materials.

[0004] The Chinese patent with publication number 101712785A discloses a preparation method and use of a novel super absorbent resin / inorganic nanoparticle composite material, wherein the preparation method is as follows: firstly, the nanoparticles are dispersed in an acrylic acid aqueous solution (neutralization degree is 5-40%), and then an initiator, a crosslinking agent and an optional copolymer matrix (such as starch, cellulose and acrylic amine, etc.) are added. After heating and reacting under nitrogen for a period of time, the product is taken out, and the final super absorbent resin nanocomposite material is obtained after washing, drying and crushing. The above invention shows excellent water absorption performance and certain mechanical properties, but the nanoparticles are natural resources or artificially manufactured layered silicates, and the economic and environmental benefits are relatively low, and the improvement of mechanical properties is relatively low.

[0005] Therefore, the present application provides a method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength, which can recycle industrial solid waste and significantly improve gel strength, and is economical and environmentally friendly. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength, the preparation process is simple and easy to adjust.

[0007] The scheme adopted by the present invention to achieve the purpose is: a method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength, comprising the following steps:

[0008] Step 1, weigh 10-25 parts of carbon nanofiber, 20-50 parts of active industrial solid waste, 2-8 parts of carbide slag, 80-120 parts of water, 200 parts of grinding balls, 1-2 parts of dispersant, wet-grind and filter to obtain nano-micron particle grinding liquid;

[0009] Step 2: dissolving 4 to 8 parts of sodium hydroxide in 10 to 15 parts of water to prepare an alkaline solution, diluting 10 to 20 parts of acrylic acid with 10 to 20 parts of water and adding the mixture dropwise to the alkaline solution, adding 3 to 5 parts of acrylamide to mix and stir after the solution temperature is cooled to room temperature, and then adding 0.006 to 0.126 parts of a cross-linking agent and 0.2 to 0.6 parts of an initiator and continuing to stir to obtain a hydrogel solution;

[0010] Step 3: Take 1 to 10 parts of the nano-micron particle grinding liquid in step 1 and add it to the hydrogel solution prepared in step 2, and stir at a certain temperature and under the protection of inert gas until the mixture is uniform;

[0011] Step 4: After the mixture uniformly mixed in step 3 is completely reacted at a certain temperature, it is dried and crushed to obtain the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

[0012] Preferably, in step 1, the active industrial solid waste is any one of blast furnace slag, fly ash and coal gangue.

[0013] Preferably, in step 1, the dispersant is at least one of a lignin sulfonate water reducer, a benzene-based high-efficiency water reducer, and a melamine-based high-efficiency water reducer.

[0014] Preferably, in step 1, the auxiliary grinding balls are wet grinding balls.

[0015] Preferably, in step 2, the cross-linking agent is N,N-methylene-bisacrylamide.

[0016] Preferably, in step 2, the initiator is potassium persulfate and / or ammonium persulfate.

[0017] Preferably, in step three, the stirring temperature is 55-75°C.

[0018] Preferably, in step 4, the reaction temperature is 55-75°C.

[0019] The present invention has the following advantages and beneficial effects:

[0020] 1. The composite hydrogel prepared by the preparation method of the present invention, in the wet grinding stage, is assisted by carbide slag to stimulate the activity of active industrial solid waste on the one hand, and further refine the active industrial solid waste on the other hand; the nano-carbon fiber plays a dispersing role in the wet grinding process, and enhances the uniformity of the grinding liquid. In the hydrogel matrix, the nano-micron-scale active industrial solid waste particles obtained after grinding will cause cross-linking between the hydrogels, and have better adhesion. When the hydrogel is under pressure, the carbon fiber will disperse the stress on the hydrogel, provide a buffer for the breakage of the hydrogel, have a certain tensile strength and toughness, and improve the life cycle of the hydrogel.

[0021] 2. The composite hydrogel prepared by the preparation method of the present invention has a higher water absorption and storage capacity. The composite hydrogel is modified by using active industrial solid waste particles, and the active industrial solid waste particles are combined with the free hydroxyl groups in the water-absorbing resin synthesized from acrylic acid and acrylamide to form binding sites, thereby enhancing the cross-linking density and improving the water absorption performance and hydrolysis resistance of the water-absorbing resin.

[0022] 3. The raw materials added and used in the preparation method of the present invention are active industrial solid waste, which realizes the resource utilization of industrial solid waste, reduces the stacking of solid waste and environmental pollution, is both environmentally friendly and economical, and the preparation process does not require high temperature and other conditions, has low cost and simple process. DETAILED DESCRIPTION

[0023] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0024] Example 1

[0025] 1) 10 parts of carbon fiber, 20 parts of fly ash, 2 parts of carbide slag, 20 parts of wet grinding balls and 1 part by weight of dispersant are mixed, and a mixture is obtained at a solid content ratio of 0.4. After stirring evenly, the mixture is put into a vertical ball mill for wet grinding for 40 minutes, and a nano-micron particle grinding liquid with a particle size of ≤150nm is obtained after filtering.

[0026] 2) 15 parts of deionized water were placed in a beaker, the beaker was placed in a magnetic stirrer at 500 r / min, 5.5 parts of sodium hydroxide were added, and the mixture was stirred evenly to obtain a sodium hydroxide solution. 15 parts of acrylic acid were diluted with 15 parts of deionized water, and the mixture was added dropwise to the sodium hydroxide solution. After the solution was stirred on the magnetic stirrer until it reached room temperature, 4 parts of acrylamide, 0.006 parts of N,N-methylenebisacrylamide, and 0.25 parts of potassium persulfate were added in sequence for cross-linking polymerization to obtain a hydrogel solution.

[0027] 3) Take 3.75 parts of the nano-micron particle grinding liquid in step 1) and add it to the hydrogel solution prepared in step 2), seal the beaker with plastic wrap, and continue stirring for 15 minutes.

[0028] 4) placing the beaker of step 4) in a water bath and heating at a constant temperature for 90 minutes, taking it out and drying it in a blower dryer to a constant weight, and crushing it to obtain a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

[0029] The composite hydrogel prepared in Example 1 has a water absorption rate of 512 g / g for deionized water and a gel strength (compressive strength of the hydrogel after water absorption) of 141 g / cm 2 .

[0030] Example 2

[0031] 1) Take 15 parts of carbon fiber, 30 parts of fly ash, 4 parts of calcium carbide slag, 30 parts of wet grinding balls and 1 part of dispersant, and add water at a solid content ratio of 0.5 to obtain a mixture. After stirring evenly, put it into a vertical ball mill for wet grinding for 40 minutes, and filter to obtain a nano-micron particle grinding liquid with a particle size of ≤150nm.

[0032] 2) 15 parts of deionized water were placed in a beaker, the beaker was placed in a magnetic stirrer at 550 r / min, 5.5 parts of sodium hydroxide were added, and the mixture was stirred to obtain a sodium hydroxide solution. 15 parts of acrylic acid were diluted with 15 parts of deionized water, and the mixture was added dropwise to the sodium hydroxide solution. After the solution was stirred on the magnetic stirrer until it reached room temperature, 4 parts of acrylamide, 0.046 parts of N,N-methylenebisacrylamide, and 0.25 parts of potassium persulfate were added in sequence for cross-linking polymerization to obtain a hydrogel solution.

[0033] 3) Take 4.5 parts of the nano-micron particle grinding liquid in step 1) and add it to the hydrogel solution prepared in step 2), seal the beaker with plastic wrap, and continue stirring for 20 minutes.

[0034] 4) placing the beaker of step 4) in a water bath and heating it at a constant temperature for 100 minutes, taking it out and drying it in a blower dryer to a constant weight, and crushing it to obtain a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

[0035] The composite hydrogel prepared in Example 2 has a water absorption rate of 543 g / g for deionized water and a gel strength of 187 g / cm 2 .

[0036] Example 3

[0037] 1) Take 20 parts of carbon fiber, 40 parts of fly ash, 6 parts of calcium carbide slag, 40 parts of wet grinding balls and 1 part of dispersant, and add water at a water-to-solid weight ratio of 0.6 to obtain a mixture. After stirring evenly, put it into a vertical ball mill for wet grinding for 40 minutes, and filter to obtain a nano-micron particle grinding liquid with a particle size of ≤150nm.

[0038] 2) 15 parts of deionized water were placed in a beaker, the beaker was placed in a magnetic stirrer at 600 r / min, 5.5 parts of sodium hydroxide were added, and the mixture was stirred evenly to obtain a sodium hydroxide solution. 15 parts of acrylic acid were diluted with 15 parts of deionized water, and the mixture was added dropwise to the sodium hydroxide solution. After the solution was stirred on the magnetic stirrer until it reached room temperature, 4 parts of acrylamide, 0.086 parts of N,N-methylenebisacrylamide, and 0.25 parts of potassium persulfate were added in sequence for cross-linking polymerization to obtain a hydrogel solution.

[0039] 3) Take 5 parts of the nano-micron particle grinding liquid in step 2) and add it to the hydrogel solution prepared in step 2), seal the beaker with plastic wrap, and continue stirring for 25 minutes.

[0040] 4) placing the beaker of step 4) in a water bath and heating at a constant temperature for 110 min, taking it out and drying it in a blower dryer to constant weight, and crushing it to obtain a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

[0041] The composite hydrogel prepared in Example 3 has a water absorption rate of 594 g / g for deionized water and a gel strength of 242 g / cm 2 .

[0042] Example 4

[0043] 1) Take 25 parts of carbon fiber, 50 parts of fly ash, 8 parts of calcium carbide slag, 130 parts of wet grinding balls and 1 part of dispersant, and add water at a water-to-solid weight ratio of 0.7 to obtain a mixture. After stirring evenly, put it into a vertical ball mill for wet grinding for 40 minutes, and filter to obtain a nano-micron particle grinding liquid with a particle size of ≤150nm.

[0044] 2) 15 parts of deionized water were placed in a beaker, the beaker was placed in a magnetic stirrer at 650 r / min, 5.5 parts of sodium hydroxide were added, and the mixture was stirred evenly to obtain a sodium hydroxide solution, 15 parts of acrylic acid were diluted with 15 parts of deionized water, and the mixture was added dropwise to the sodium hydroxide solution, the solution was stirred on the magnetic stirrer until it reached room temperature, and then 4 parts of acrylamide, 0.126 parts of N,N-methylenebisacrylamide, and 0.25 parts of potassium persulfate were added in sequence for cross-linking polymerization to obtain a hydrogel solution.

[0045] 3) 5.36 parts of the nano-micron particle grinding liquid in step 1) were added to the hydrogel solution prepared in step 2), the beaker was sealed with plastic wrap, and stirring was continued for 30 minutes.

[0046] 4) placing the beaker of step 4) in a water bath and heating at a constant temperature for 120 min, taking it out and drying it in a blower dryer to constant weight, and crushing it to obtain a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

[0047] The composite hydrogel prepared in Example 4 has a water absorption rate of 542 g / g for deionized water and a gel strength of 181 g / cm 2 .

[0048] Comparative Example

[0049] This sample group is a hydrogel without any addition of nano-micro particles.

[0050] 1) 15 parts of deionized water are placed in a beaker, the beaker is placed in a magnetic stirrer at 500 r / min, 5.5 parts of sodium hydroxide are added, and the mixture is stirred evenly to obtain a sodium hydroxide solution. 15 parts of acrylic acid are diluted with 15 parts of deionized water, and the mixture is added dropwise to the sodium hydroxide solution. After the solution is stirred on the magnetic stirrer until it reaches room temperature, 4 parts of acrylamide, 0.015 parts of N,N-methylenebisacrylamide, and 0.25 parts of potassium persulfate are added in sequence for cross-linking polymerization, and the beaker is sealed with a plastic wrap to obtain a hydrogel solution.

[0051] 2) The beaker of step 1) is placed in a water bath and heated at a constant temperature for 90 minutes. After being taken out, it is placed in a blast dryer and dried to a constant weight. The ordinary hydrogel can be obtained by crushing.

[0052] The composite hydrogel prepared in Comparative Example 1 has a water absorption rate of 311 g / g for deionized water and a gel strength of 84 g / cm 2 .

[0053] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A method for preparing a nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength, Features: The following steps are involved: Step 1, weigh 10-25 parts of carbon nanofiber, 20-50 parts of active industrial solid waste, 2-8 parts of carbide slag, 80-120 parts of water, 200 parts of grinding balls, 1-2 parts of dispersant, wet-grind and filter to obtain nano-micron particle grinding liquid; Step 2: dissolving 4 to 8 parts of sodium hydroxide in 10 to 15 parts of water to prepare an alkaline solution, diluting 10 to 20 parts of acrylic acid with 10 to 20 parts of water and adding the mixture dropwise to the alkaline solution, adding 3 to 5 parts of acrylamide to mix and stir after the solution temperature is cooled to room temperature, and then adding 0.006 to 0.126 parts of a cross-linking agent and 0.2 to 0.6 parts of an initiator and continuing to stir to obtain a hydrogel solution; Step 3: Take 1 to 10 parts of the nano-micron particle grinding liquid in step 1 and add it to the hydrogel solution prepared in step 2, and stir at a certain temperature and under the protection of inert gas until the mixture is uniform; Step 4: After the mixture uniformly mixed in step 3 is completely reacted at a certain temperature, it is dried and crushed to obtain the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength.

2. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 1, the active industrial solid waste is any one of blast furnace slag, fly ash and coal gangue.

3. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 1, the dispersant is at least one of a lignin sulfonate water reducer, a benzene-based high-efficiency water reducer, and a melamine-based high-efficiency water reducer.

4. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 1, the auxiliary grinding balls are wet grinding balls.

5. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 2, the cross-linking agent is N,N-methylene-bisacrylamide.

6. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 2, the initiator is potassium persulfate and / or ammonium persulfate.

7. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 3, the stirring temperature is 55-75°C.

8. The method for preparing the nano-micron particle composite hydrogel with enhanced water absorption and storage capacity and gel strength according to claim 1, Features: In the step 4, the reaction temperature is 55-75°C.

Citation Information

Patent Citations

  • Novel super absorbent resin / inorganic nanoparticle composite material, preparation method thereof and usage thereof

    CN101712785A

  • Method for preparation of fracture-resisting and toughened wet grinding pasty admixtures utilizing waste

    CN107459311A

  • Hydrogel adsorption material prepared from industrial solid wastes, and preparation method thereof

    CN108295814A

  • Preparation method of silicon dioxide nano-star modified composite gel material

    CN109734366A

  • Water-absorbent resin as well as preparation method and application thereof

    CN113667061A