Nano-iron oxide composite material capable of treating soil arsenic pollution, preparation method and application thereof
Through the use of nano-iron oxide composite materials, combined with materials such as biochar and citric acid, the problems of high cost and low efficiency in soil arsenic pollution treatment have been solved, and the arsenic content in soil has been significantly reduced and stability improved, meeting the needs of low-level soil arsenic pollution. cost and environmental requirements.
Patent Information
- Application Number
- CN202210471194.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-04-28
AI Technical Summary
Existing technologies are costly and inefficient in treating soil arsenic pollution, and the use of nano-zero-valent iron and nano-iron oxide has stability problems, making it difficult to effectively reduce arsenic content in soil.
Nano-iron oxide composite materials are used. The nano-iron oxide content does not exceed 5% of the overall content of the composite material. It is composed of biomass carbon-loaded nano-iron oxide, citric acid-loaded nano-iron oxide and silicon-containing substances. Through ultrasonic and oscillation methods, Preparation, combined with materials such as wollastonite, the resulting composite material is spread into the soil to reduce arsenic levels.
It has achieved a 70% reduction in soil arsenic content, is low-cost, environmentally friendly, will not cause secondary pollution, and increases the stability of the composite material and its adsorption capacity for arsenic.
Smart Images

Figure HDA0003622469470000011 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the field of farmland soil restoration, and in particular to a nano iron oxide composite material capable of treating soil arsenic pollution, a preparation method and application thereof. Background Art
[0002] Arsenic is a highly toxic and carcinogenic chemical element, and is listed as one of the toxic substances that the World Health Organization prioritizes. Once the soil is contaminated by As, As will enter the human body through the food chain, and has a greater toxic effect on the human body's internal organs and bones. At present, the materials used to solidify soil As mainly include iron-containing substances, sulfur-containing substances, rare earth materials, calcium salts, etc., among which iron-containing and sulfur-containing substances have better effects. In recent years, nano-iron has become a promising soil remediation material due to its large specific surface area and high reactivity. However, due to the small size and easy agglomeration of nanoparticles, their strong reducibility makes them easily oxidized in the presence of oxygen. Therefore, when implementing this technology, it is necessary to modify them, such as polymer coating, loading with other materials, adding stabilizers, etc. The Chinese invention patent application (application number 201810520363.6) discloses a soil arsenic and chromium pollution remediation agent based on an organic clay-loaded nano-iron oxide system. The repair agent is prepared by mixing two components: organic montmorillonite-loaded nano zero-valent iron and organic montmorillonite-loaded nano iron oxide. The weight percentage of each component is: organic montmorillonite-loaded nano zero-valent iron is 55-85%, and organic montmorillonite-loaded nano iron oxide is 15-45%. After using the repair agent, the stabilization efficiency of soil arsenic can be improved by 10-20%. However, the repair agent uses both nano zero-valent iron and nano iron oxide, which is costly, and the reduction efficiency is relatively low. It has many production steps and a complicated process, which is not conducive to large-scale promotion.
[0003] The paper "Modification of bentonite-loaded nano-iron and adsorption of As(V) in water" used hexadecyltrimethylammonium bromide to modify the surface of bentonite-loaded nano-zero-valent iron, and the surface-modified bentonite-loaded nano-iron had a removal rate of 90% for As in water. However, the modified nano-zero-valent iron was only studied for the removal of arsenic in water, and no research was conducted on the remediation of As in soil. There are large differences between water and soil systems, so the remediation effect of this material on soil As is very uncertain.
[0004] The Chinese invention patent application (application number 201911358166.X) discloses a method for preparing soil heavy metal passivation materials by green synthetic nano-iron (nano zero-valent iron or nano iron oxide) complexed attapulgite. Compared with the control, the green synthetic nano-iron complexed attapulgite prepared soil heavy metal passivation material can increase corn biomass by 36.5%, and the application of the passivator reduces the cadmium content of the aboveground part of corn by 33.7%. The passivator only verifies the remediation efficiency of heavy metal cadmium, while the properties of cadmium and arsenic are quite different, and the passivator may not be suitable for the remediation of heavy metal arsenic. And the dosage of the passivator needs to reach 4% of the soil amount. If the amount added is too large, the cost will be high. Summary of the invention
[0005] In view of the deficiencies in the above-mentioned prior art and products, the purpose of the present invention is to provide a nano-iron oxide composite material, a preparation method and its application that can treat soil arsenic contamination. The content of nano-iron oxide in the nano-iron oxide composite material prepared by the present invention does not exceed 5% of the total content of the composite material, and the obtained nano-iron oxide composite material is spread on arsenic-contaminated soil at a rate of 100-150 kg / mu, and the maximum reduction of crop arsenic content can reach 70%.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A nano iron oxide composite material for treating soil arsenic pollution is made of several components with the following weight percentages:
[0008] Raw material weight percentage
[0009] Biochar-loaded nano-iron oxide 10-22%
[0010] Citric acid loaded nano iron oxide 2-8%
[0011] Silicon-containing substances 70-85%
[0012] Preferably, the nano iron oxide composite material is made of several components in the following weight percentages:
[0013] Raw material weight percentage
[0014] Biomass charcoal loaded with nano iron oxide 20%
[0015] Citric acid loaded nano iron oxide 2.2%
[0016] Silicon-containing substances 78.8%
[0017] Furthermore, the particle size of the nano iron oxide is 10-50 nm, preferably 30±5 nm.
[0018] Furthermore, the silicon-containing substance is wollastonite, diatomaceous earth, etc.
[0019] Furthermore, the composite material is sieved through a 60-80 mesh sieve.
[0020] Furthermore, the method for preparing the biochar-supported nano iron oxide comprises the following steps:
[0021] (1) waste biomass (e.g., rice husk and / or wheat straw) is used as raw material and carbonized at 600°C in an oxygen-deficient environment for 2-3 hours. The obtained carbonized product is acid-washed, washed with water until neutral, dried, ground into powder, washed with deionized water for multiple times, and dried at 90°C-100°C to obtain biochar;
[0022] (2) Dissolve nano-iron oxide in distilled water, ultrasonicate at 230-260 r / min for 0.5-1 h, add biochar (the mass ratio of biochar to nano-iron oxide is 9:1) under nitrogen protection, and drop a small amount of 0.1 mol / L NaBH4, stir evenly, and continue ultrasonicate at 230-260 r / min for 0.5-1 h. After ultrasonication, place it in a constant temperature shaking shaker (25°C, 100-130 r / min) and oscillate for 12-24 h. After oscillation, precipitate for 24-48 h, pour out the supernatant and wash with anhydrous ethanol for at least 3 times, and finally place it in a drying oven at 110°C for 12-24 h to obtain biochar-loaded nano-iron oxide.
[0023] Furthermore, the preparation method of the citric acid-loaded nano-iron oxide comprises the following steps: dissolving the nano-iron oxide in distilled water, ultrasonicating at a speed of 200-260 r / min for 0.5-1 h, adding citric acid (the mass ratio of citric acid to nano-iron oxide is 1:10) and stirring evenly, placing the nano-iron oxide in a shaker and rotating at a speed of 150-180 r / min for 10-12 h, and then standing for 24-48 h, pouring out the supernatant, washing with anhydrous ethanol for at least 3 times, and finally placing the nano-iron oxide in a drying oven at 110°C and drying for 12-24 h to obtain the citric acid-loaded nano-iron oxide.
[0024] The method for preparing the nano iron oxide composite material capable of treating soil arsenic pollution comprises the following steps:
[0025] The silicon-containing material is ground into powder; nano iron oxide loaded on biochar, nano iron oxide loaded on citric acid and wollastonite powder are respectively taken in a certain mass percentage, mixed evenly, and ground through a 60-80 mesh sieve to obtain the product.
[0026] Application of the nano iron oxide composite material and the nano iron oxide composite material prepared by the method in the remediation of arsenic contaminated soil.
[0027] In specific application, before planting crops, the nano iron oxide composite material is evenly spread into the soil at a spreading rate of 100-150 kg / mu, and water is appropriately sprinkled according to soil conditions to maintain the soil moisture content at 15-25% so that the nano iron oxide composite material is fully dissolved in the soil.
[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0029] (1) The present invention uses nano iron oxide, the iron content of which is three times that of ordinary iron. It has a large specific surface area and high reactivity, and can effectively adsorb arsenic in the soil for a long time. Considering the easy polymerization of nano iron oxide, the present invention uses biochar for modification, which increases the stability of nano iron oxide without destroying the high reactivity of nano iron oxide. At the same time, the addition of biochar further enhances the adsorption of soil arsenic by the composite material.
[0030] (2) Citric acid is added in the present invention. Citric acid is a rhizosphere secretion. In the present invention, it is used as a biocompatible material to cover the nano-iron oxide, thereby increasing the stability of the nano-iron oxide. When the nano-iron oxide loaded with citric acid is applied to the soil, on the one hand, it can adsorb arsenic in the soil, and on the other hand, citric acid can promote the formation of iron film on the root surface of the crop root system, thereby further preventing the migration of arsenic in the soil to the crops.
[0031] (3) The addition of silicon-containing materials such as wollastonite in the present invention has a reinforcing effect on the composite material's repair of arsenic. Inorganic arsenic in the soil mainly exists in the form of trivalent arsenic compounds and pentavalent arsenic compounds. Whether in terms of toxicity or plant effectiveness, trivalent arsenic is far greater than pentavalent arsenic. Trivalent arsenic is mainly absorbed by crops through the channels of silicon, and there is a certain competitive relationship between trivalent arsenic and silicon. Therefore, increasing the effective silicon content in the soil and promoting the absorption of silicon by crops can reduce the absorption of trivalent arsenic by crop roots to a large extent.
[0032] (4) The composite material of the present invention is low-cost, environmentally friendly, and will not cause secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a transmission electron microscope image of nano-iron oxide. DETAILED DESCRIPTION
[0034] The applicant will further explain the technical solution of the present invention in detail below in conjunction with specific embodiments, with the aim of enabling those skilled in the art to have a clearer understanding and recognition of the present application.
[0035] The raw materials used in the following examples are described as follows:
[0036] Biochar: Use waste rice husk as raw material, carbonize it at 600℃ in an oxygen-deficient environment for 3h, wash the carbonized product with acid, wash it with water until neutral, dry it, grind it into powder, wash it with deionized water 4 times, and dry it at 90℃ to obtain biochar.
[0037] Nano iron oxide: purchased from Zhitai Purification Technology, it is γ iron oxide, reddish brown, spherical, with a particle size of about 30nm and a specific surface area of 85.2m 2 / g, its transmission electron microscope image is as follows Figure 1 shown.
[0038] Citric acid: purity ≥99.0%, molecular formula C6H8O7·H2O, purchased from Shaanxi Yangyuanshen Biotechnology Co., Ltd.
[0039] Wollastonite: purchased from Hunan Hongcheng Ore Powder Co., Ltd., calcium silicate content ≥95%.
[0040] Iron powder: purchased from Lingshou County Shifeng Mining Processing Plant, 80-100 mesh, iron content ≥97%.
[0041] Biochar-loaded nano-iron oxide: Take 2g of nano-iron oxide with a particle size of about 30nm and dissolve it in 1L of distilled water. Ultrasonicate at 250r / min for 1h. Under nitrogen protection, add 18g of biochar and add 5mL0.1mol / LNaBH4 dropwise and stir evenly (the purpose is to play a reducing role and increase the purity of nano-iron oxide). Continue to ultrasonicate at 250r / min for 1h. After the ultrasonication is completed, put it in a constant temperature shaking shaker (25℃, 120r / min) and oscillate for 24h. After the oscillation is completed, precipitate it for 24h, pour out the supernatant and wash it with anhydrous ethanol 3 times, and finally put it in a 110℃ drying oven to dry for 12h to obtain biochar-loaded nano-iron oxide.
[0042] Citric acid-loaded nano-iron oxide: Take 2g of nano-iron oxide with a particle size of about 30nm and dissolve it in 1L of distilled water. Ultrasonicate at 250r / min for 1h, then add 0.2g of citric acid and stir evenly. Put it in a shaker and rotate it at 160r / min for 12h. After standing for 24h, pour out the supernatant, wash it with anhydrous ethanol 3 times, and finally put it in a drying oven at 110℃ and dry it for 12h to obtain citric acid-loaded nano-iron oxide.
[0043] Embodiment A:
[0044] A method for preparing a nano iron oxide composite material capable of treating soil arsenic pollution. The nano iron oxide composite material is made of three raw materials in the following weight percentages:
[0045] Raw materials and weight percentage
[0046] Biochar-supported nano-iron oxide: 20%
[0047] Citric acid loaded nano iron oxide: 2.2%
[0048] Wollastonite: 77.8%
[0049] The specific preparation method is as follows: grind wollastonite into powder, take nano iron oxide loaded on biochar, nano iron oxide loaded on citric acid and wollastonite powder respectively according to the weight percentage of the above raw materials, mix them evenly, grind them through a 60-mesh sieve, and obtain the product.
[0050] Embodiment B:
[0051] A method for preparing an iron composite material capable of treating soil arsenic pollution, wherein the iron composite material is made of four raw materials in the following weight percentages:
[0052] Raw materials and weight percentage
[0053] Biochar: 18%
[0054] Citric acid: 0.2%
[0055] Iron powder: 12%
[0056] Wollastonite: 69.8%
[0057] The specific preparation method is as follows: grind wollastonite into powder, take biochar, citric acid, iron powder and wollastonite powder respectively according to the weight percentage of the above raw materials, mix them evenly, grind them through a 60-mesh sieve, and obtain the product.
[0058] Example C:
[0059] A method for preparing a nano iron oxide composite material capable of treating soil arsenic pollution. The nano iron oxide composite material is made of two raw materials in the following weight percentages:
[0060] Raw materials and weight percentage
[0061] Biochar-supported nano-iron oxide: 40%
[0062] Wollastonite: 60%
[0063] The specific preparation method is as follows: grind wollastonite into powder, take the nano iron oxide loaded on biochar and wollastonite powder respectively according to the weight percentage of the above raw materials, mix them evenly, grind them through a 60-mesh sieve, and obtain the product.
[0064] Embodiment D:
[0065] A method for preparing a nano iron oxide composite material capable of treating soil arsenic pollution. The nano iron oxide composite material is made of three raw materials in the following weight percentages:
[0066] Raw materials and weight percentage
[0067] Biochar-supported nano-iron oxide: 40%
[0068] Citric acid: 0.2%
[0069] Wollastonite: 59.8%
[0070] The specific preparation method is as follows: grind wollastonite into powder, take the nano iron oxide loaded on biochar, citric acid and wollastonite powder respectively according to the weight percentage of the above raw materials, mix them evenly, grind them through a 60-mesh sieve, and obtain the product.
[0071] Application Examples
[0072] From April to June 2021, a potted experiment was carried out in a potted test room. The potted soil was collected from a township in Shimen County, Hunan Province. The soil organic matter content was 25.8 g / kg, pH 6.05, total As 242 mg / kg, and effective arsenic 19.51 mg / kg. The crop variety was: Water spinach (willow leaf white stem). The experiment had 9 treatments, each with 3 replicates, for a total of 27 pots. The experiment adopted a completely randomized arrangement design, with 7.5 kg of dry soil in each pot.
[0073] Treatment 1: blank (CK), conventional fertilization;
[0074] Treatments A1, B1, C1, and D1: conventional fertilization + 4 g / pot of the test composite material (equivalent to about 100 kg / mu) as basal fertilization;
[0075] Treatments A2, B2, C2, and D2: conventional fertilization + 6 g / pot of the test composite material (equivalent to about 150 kg / mu) as basal fertilization;
[0076] It should be noted that:
[0077] 1) The composite materials tested in treatments A1 (A2), B1 (B2), C1 (C2), and D1 (D2) refer to the composite materials prepared in Examples A, B, C, and D, respectively;
[0078] 2) Conventional fertilization: Add 0.8g / pot compound fertilizer (equivalent to about 20kg / mu) and 0.16g / pot urea (equivalent to about 4kg / mu) during the seedling stage and apply them together. During the harvest period, use 0.32g / pot compound fertilizer (equivalent to about 8kg / mu) as topdressing after each harvest; the compound fertilizer is: monoammonium phosphate, the main ingredient is NH4H2PO4, the effective ingredient is % (N-P2O5-K2O) 12-60-0.
[0079] Application method of the test composite material: on the basis of conventional fertilization, fully mix the potting soil with the composite material, sprinkle water appropriately according to the soil conditions, and maintain the soil moisture content at 15-25%.
[0080] The tested water spinach was harvested after about 60 days. After the experiment, soil samples from each pot and the aboveground part of water spinach were collected to measure the soil pH value, soil available arsenic content, and total arsenic content of water spinach.
[0081] Sample processing and analysis:
[0082] Soil pH determination method: Use water as the extractant, collect a small amount of soil and mix the water and soil in a mass ratio of 2.5:1, and measure it using the potentiometric method (refer to NY / T1377-2007).
[0083] Determination of available arsenic in soil: refer to DB35 / T 1459-2014;
[0084] Determination of arsenic in food: refer to GB5009.11-2014.
[0085] Main results and analysis:
[0086] 1. Effects of different treatments on soil pH
[0087] The effects of different treatments on soil pH are shown in Table 1. Compared with CK, soil pH in treatment A decreased by 0.32 and 0.38, with a decrease of 5.29% and 6.28%, respectively; soil pH in treatment B decreased by 0.33 and 0.39, with a decrease of 5.45% and 6.45%, respectively; soil pH in treatment C decreased by 0.16 and 0.20, with a decrease of 2.64% and 3.31%, respectively; soil pH in treatment D decreased by 0.34 and 0.40, with a decrease of 5.62% and 6.61%, respectively. This shows that the composite materials can reduce the content of soil pH to a certain extent, and the effect of reducing pH in implementation case A and implementation cases B and D is not much different, and the value of reducing pH in implementation case D is the largest.
[0088] Table 1 Effects of different treatments on soil pH
[0089]
[0090]
[0091] 2. Effects of different treatments on soil available arsenic content
[0092] The effects of different treatments on the available arsenic content in the soil are shown in Table 2. The average available arsenic content in the soil of the CK treatment was 16.93 mg / kg, and the available arsenic in the soil of the treatment A was reduced by 4.14 mg / kg and 5.41 mg / kg, respectively, with a reduction of 24.45% and 31.96%, respectively; the available arsenic in the soil of the treatment B was reduced by 3.51 mg / kg and 4.44 mg / kg, respectively, with a reduction of 20.73% and 26.23%, respectively; the available arsenic in the soil of the treatment C was reduced by 2.97 mg / kg and 4.06 mg / kg, respectively, with a reduction of 17.54% and 23.98%, respectively; the available arsenic in the soil of the treatment D was reduced by 3.57 mg / kg and 4.52 mg / kg, respectively, with a reduction of 21.08% and 26.69%, respectively. This shows that the composite material can reduce the content of available arsenic in the soil to a certain extent, and the implementation case effect is A>D>B>C.
[0093] Table 2 Effects of different treatments on soil available arsenic
[0094]
[0095] 3. Effects of different treatments on total arsenic content in water spinach
[0096] The effects of different treatments on the total arsenic content of water spinach are shown in Table 3. The average total arsenic content of water spinach in CK treatment was 1.07 mg / kg, and the total arsenic of water spinach in treatment A was reduced by 0.59 mg / kg and 0.75 mg / kg, respectively, with a decrease of 55.14% and 70.09%, respectively; the total arsenic in soil in treatment B was reduced by 0.43 mg / kg and 0.53 mg / kg, respectively, with a decrease of 40.19% and 49.53%, respectively; the total arsenic content of water spinach in treatment C was reduced by 0.40 mg / kg and 0.51 mg / kg, respectively, with a decrease of 37.38% and 47.66%, respectively; the total arsenic content of water spinach in treatment D was reduced by 0.46 mg / kg and 0.55 mg / kg, respectively, with a decrease of 42.99% and 51.40%, respectively. This shows that the composite material can reduce the total arsenic content of water spinach to a certain extent, and the implementation case effect A>D>B>C. The total arsenic in treatment A water spinach meets the standard of GB2762-2017 "National Food Safety Standard Limits of Contaminants in Food" (total arsenic 0.5 mg / kg).
[0097] Table 3 Effects of different treatments on total arsenic in water spinach
[0098]
Claims
1. Application of nano-iron oxide composite materials in the remediation of arsenic-contaminated soil, characterized by: Before planting crops, the nano-iron oxide composite material is evenly spread into the soil at a spreading rate of 100-150 kg / mu, and water is appropriately sprinkled according to the soil conditions to maintain the soil moisture content at 15-25%, so that the nano-iron oxide composite material is fully dissolved in the soil; The nano iron oxide composite material is made of three components in the following weight percentages: 20% of nano iron oxide supported by biomass charcoal; 2.2% of nano iron oxide supported by citric acid; and 77.8% of wollastonite. The preparation method thereof comprises the following steps: grinding the wollastonite into powder, mixing the powder with the nano iron oxide supported by biomass charcoal and the nano iron oxide supported by citric acid, and grinding the powder through a 60-80 mesh sieve to obtain the composite material; The method for preparing the biochar-supported nano iron oxide comprises the following steps: (1) Using rice husk and / or wheat straw as raw materials, carbonizing them at 600°C in an oxygen-deficient environment for 3 hours, washing the obtained carbonized product with acid, washing with water until neutral, drying, grinding into powder, and then washing with deionized water for multiple times, and drying at 90°C-100°C to obtain biochar; (2) Dissolve γ-type nano-iron oxide with a particle size of 30±5 nm in distilled water, ultrasonicate at a speed of 230-260 r / min for 0.5-1 h, add biochar under nitrogen protection, the mass ratio of biochar to nano-iron oxide is 9:1, and add a small amount of 0.1 mol / L NaBH4 dropwise, stir evenly, continue ultrasonicate at a speed of 230-260 r / min for 0.5-1 h, and after the ultrasonicate is completed, place it in a constant temperature oscillating shaker at a temperature of 25°C and a speed of 100-130 r / min for 12-24 h. After the oscillation is completed, precipitate it for 24-48 h, pour off the supernatant and wash it with anhydrous ethanol for at least 3 times, and finally place it in a drying oven at 110°C for 12-24 h to obtain biochar-loaded nano-iron oxide; The preparation method of citric acid-loaded nano iron oxide comprises the following steps: dissolving γ-type nano iron oxide with a particle size of 30±5nm in distilled water, ultrasonicating for 0.5-1h at a rotation speed of 200-260r / min, adding citric acid, wherein the mass ratio of citric acid to nano iron oxide is 1:10, stirring evenly, placing in a shaking table and rotating at a rotation speed of 150-180r / min for 10-12h, standing for 24-48h, pouring out the supernatant, washing with anhydrous ethanol for at least 3 times, and finally placing in a drying oven at 110°C and drying for 12-24h to obtain citric acid-loaded nano iron oxide.