Precisely depth-controlled surface embedded precision circuit packaging substrate and its processing technology
By forming a titanium or titanium/copper resist layer on the conventional copper foil carrier layer, the etching of the embedded circuit layer is solved, and the problem of high cost of ultra-thin copper foil and difficult to control the flatness of the circuit layer is achieved, and low cost and high efficiency are achieved Precisely controlled deep-controlled surface embedded precision line packaging load plate processing technology.
Patent Information
- Application Number
- CN202210324404.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-03-30
AI Technical Summary
In the prior art, ultra-thin copper foil processing cost is high and the end point of the embedded circuit layer is difficult to control, which can easily cause overetching and cause excessive concave erosion of the embedded circuit layer. Special control of flash corrosion parameters, equipment accuracy and production operation requirements are required. high.
The carrier layer is made using conventional copper foil and a titanium or titanium/copper resist layer is formed on its surface. The embedded circuit is made through electroplating and etching processes. The resist layer is used to control the erosion end point of the circuit, reduce material costs and ensure circuit boards. flatness of the surface.
Reduces material costs, improves product production yield, controls the height difference between the embedded circuit layer and the insulating layer, meets the design needs of high-end products, and is suitable for the minimum line width/line distance of double-sided panels and multi-layer boards. design.
Smart Images

Figure CN114828453B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a packaging carrier, and in particular to a packaging carrier with a surface layer embedded with precision circuits and a processing technology thereof with a precisely controlled depth. Background Art
[0002] With the continuous updates and iterations of the information age, the functional requirements for various chips are getting higher and higher, such as high-speed computing, high storage, high precision, high stability, etc. Correspondingly, the requirements for packaging substrates are also getting higher and higher, such as high-density wiring, thin plates, high flatness, etc.; in the prior art, in order to achieve the above design, a built-in precision circuit process based on ultra-thin copper foil (3μm, 5μm, etc.) layer addition has been developed, but this technology has two problems: one is the high procurement cost of ultra-thin copper processing; the other is that the termination point is difficult to control when the ultra-thin copper on the surface of the embedded circuit layer is removed, which can easily cause over-etching and lead to excessive concave etching of the embedded circuit layer. Special control of flash etching parameters is required, and high requirements are placed on equipment accuracy and production operation control.
[0003] Application Contents
[0004] In order to overcome the above-mentioned defects, the present application provides a processing technology for a surface-embedded precision circuit packaging carrier with precisely controlled depth. In the processing technology, conventional copper foil is used to make the carrier layer, and an anti-corrosion layer is formed on the surface of the copper foil, thereby reducing the material production cost, controlling the end point of the buried wire layer circuit corrosion, and thus ensuring the flatness of the circuit board surface.
[0005] The technical solution adopted by this application to solve its technical problems is:
[0006] A processing technology for a surface layer embedded precision circuit packaging substrate with precise depth control includes the following steps:
[0007] Step 1: Preparation of a carrier: prepare two conventional copper foils, and glue the two copper foils together to form a carrier, that is, the carrier includes a first copper foil layer and a second copper foil layer, and the two outer surfaces of the carrier are defined as outer surfaces, and the two inner surfaces of the carrier are defined as inner surfaces, and the two inner surfaces are glued together;
[0008] Step 2: Making an anti-corrosion layer: forming an anti-corrosion layer on at least one outer surface of the carrier by radiography, wherein the anti-corrosion layer is a titanium layer or a composite layer of titanium and copper;
[0009] Step 3: Preparation of the first buried wire layer:
[0010] 3.1 Preparation of anti-plating photosensitive layer: Through lamination, exposure and development, a photosensitive layer is formed, and the pattern circuit area on the resist layer where the pattern needs to be made is exposed;
[0011] 3.2 Electroplating: Electroplating is used to form the embedded first buried wire layer on the exposed pattern circuit area on the anti-corrosion layer of the carrier;
[0012] 3.3 De-filming: De-film the electroplated product to remove the photosensitive layer, exposing the graphic circuit and its spacing space;
[0013] Step 4: Post-processing
[0014] 4.1 Addition layer manufacturing: filling the first buried wire layer with an insulating medium to form an insulating medium layer 17;
[0015] 4.2 Production of the second buried wire layer:
[0016] ① Blind hole processing: Processing blind holes in the insulating dielectric layer;
[0017] ②Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer and the blind hole;
[0018] ③ Fabrication of graphic circuits: fabricating a second buried wiring layer on the seed layer;
[0019] 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer;
[0020] 4.4 Removing the carrier: firstly, the first copper foil layer and the second copper foil layer are separated, and then the first copper foil layer or the second copper foil layer is removed by etching to obtain a product with an anti-corrosion layer;
[0021] 4.5 Removal of the anti-corrosion layer: Use sulfuric acid or hydrochloric acid to remove the anti-corrosion layer 14 in the product to obtain a product with a buried wire layer on one side.
[0022] Preferably, in step 1: a frame is also prepared, and the first copper foil layer and the second copper foil layer are bonded together through the frame, specifically: at a temperature of 80-120°C, glue is coated on the upper and lower surfaces of the frame, and then two pieces of copper foil are respectively attached to the upper and lower surfaces of the frame to form a carrier, the frame is an annular structure with a hollow interior, the width of the frame is 5-15 mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16-18ppm / °C.
[0023] Preferably, the step 1 is specifically as follows: after a layer of glue is evenly coated around one of the copper foils near the edge area, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to solidify to form a carrier.
[0024] Preferably, the above step 4.4 specifically includes the following process:
[0025] ① Edge milling: perform edge milling 2-5mm away from the inner side of the frame to separate the first copper foil layer from the second copper foil layer;
[0026] ②Frame processing: After the milling frame is etched, the residual glue and impurities are removed to obtain a reusable frame;
[0027] ③Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
[0028] Preferably, the above step 4.4 specifically includes the following process:
[0029] ① Edge milling: perform edge milling 2-5mm from the inner side of the connection between the first copper foil layer and the second copper foil layer to separate the first copper foil layer from the second copper foil layer;
[0030] ②Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
[0031] Preferably, in the above step 2, when the anti-corrosion layer is a titanium layer, a titanium layer is directly projected on the outer surface of the carrier, and the thickness of the titanium layer is 0.05-0.2μm; when the anti-corrosion layer is a composite layer of titanium and copper, a titanium layer is first projected on the outer surface of the carrier, and the thickness of the titanium layer is 0.05-0.2μm, and then a copper layer is projected on the titanium layer, and the thickness of the copper layer is 0.5-0.2μm.
[0032] Preferably, in step 4.5: when the anti-corrosion layer is a titanium layer, the titanium layer can be directly removed using sulfuric acid or hydrochloric acid solution; when the anti-corrosion layer is a composite layer of titanium and copper, the titanium layer is first removed using sulfuric acid or hydrochloric acid solution, and then the copper layer is removed by a micro-etching process.
[0033] Preferably, the step 3.1 specifically includes the following process:
[0034] ① Lamination: Make a photosensitive layer, and evenly apply a photosensitive layer on the resist layer by lamination or coating;
[0035] ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution;
[0036] ③ Development: Remove the photosensitive layer in the unreacted area and retain the area where the photopolymerization reaction occurs, that is, expose the graphic circuit area to be produced, and cover the non-graphic circuit area with a photosensitive layer that resists electroplating.
[0037] Preferably, the step 4.1 specifically includes the following process:
[0038] ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding force between the circuit and the insulating medium and improve product performance;
[0039] ②Filling with insulating medium: forming an insulating medium layer on the graphic circuit layer through lamination or vacuum lamination combined with baking process;
[0040] In step 4.2, in step ①, a blind hole is made by laser window opening and laser drilling, and the alignment reference during the production process is a target hole with an inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference during the production process is an inner target; in step 4.2, in step ②, a seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when the pattern is produced, according to the pattern wiring density, an additive method combined with pattern electroplating or a subtractive method combined with whole-board electroplating and etching process is used to carry out pattern layer production.
[0041] The present invention also provides a surface-embedded precision circuit packaging carrier with accurately controlled depth, and the packaging carrier is processed by the above-mentioned processing technology.
[0042] The beneficial effects of this application are:
[0043] 1) Compared with the existing technology, the present application uses conventional copper foil to replace the high-cost ultra-thin copper, which greatly reduces the material cost, and the frame used can be reused, so the overall cost is very low. By utilizing the difference between the thermal expansion coefficients of the frame and the copper foil, the copper foil layer in the carrier is in a taut state, which improves the quality of the carrier and thus improves the production yield of the product;
[0044] 2) During the processing, titanium or titanium / copper layer is used as the anti-corrosion layer, which does not have high requirements for etching solution and equipment accuracy, and can effectively prevent the solution from attacking the surface circuit, and control the height difference between the embedded circuit layer and the insulating layer in the finished product. The height difference between the surface embedded circuit layer and the insulating layer can be controlled to be less than 1μm; therefore, the buried wire layer circuit is protected by the anti-corrosion layer, and when the carrier copper foil is removed, the buried wire layer will not be attacked through the anti-corrosion layer, thereby ensuring the flatness of the entire board surface and meeting the design requirements of high-end products;
[0045] 3) This processing technology is suitable for double-sided boards and multi-layer boards, and can meet the minimum line width / line spacing 8 / 8um design requirements. During the processing, double-sided processing can be performed on the carrier part, which improves product production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a schematic diagram of the structure of the present application without a frame carrier;
[0047] Figure 2This is a schematic diagram of the structure of the frame carrier component in this application;
[0048] Figure 3 This is a schematic diagram of the structure of the carrier component after the anti-corrosion layer is projected in this application;
[0049] Figure 4 This is a schematic diagram of the structure of the carrier component after the photosensitive layer is made in this application;
[0050] Figure 5 This is a schematic diagram of the structure of the carrier component after the first buried wire layer is formed in the present application;
[0051] Figure 6 This is a schematic diagram of the structure of the carrier member in this application after removing the photosensitive layer;
[0052] Figure 7 It is a schematic diagram of the structure of the n-layer board in this application;
[0053] Figure 8 This is a schematic diagram of the structure of the n-layer board after removing the carrier member in this application;
[0054] Fig. 9 This is a schematic diagram of the structure of the n-layer board after the copper foil layer is removed in this application;
[0055] Fig.10 This is a schematic diagram of the structure of the n-layer board after the anti-etching layer is removed in this application;
[0056] In the figure: 10-carrier, 11-first copper foil layer, 12-second copper foil layer, 13-frame, 14-anti-corrosion layer, 15-photosensitive layer, 16-first buried wire layer, 17-insulating dielectric layer, 18-graphic circuit area, 21-second buried wire layer, 22-external graphic circuit layer. DETAILED DESCRIPTION
[0057] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0058] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the following drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0059] Embodiment: A processing technology for a surface layer embedded precision circuit packaging carrier with accurate depth control comprises the following steps:
[0060] Step 1: Preparation of carrier 10: Figure 1 Or as shown in 2, two conventional copper foils are prepared, and the two copper foils are glued together to form a carrier 10, that is, the carrier 10 includes a first copper foil layer 11 and a second copper foil layer 12, the two outer surfaces of the carrier 10 are defined as outer surfaces, and the two inner surfaces of the carrier 10 are defined as inner surfaces, and the two inner surfaces are glued together; the first copper foil layer 11 and the second copper foil layer 12 both have a first surface and a second surface relative to each other, the second surfaces of the first copper foil layer and the second copper foil layer are glued together, the two second surfaces are the inner surfaces of the carrier, the first surfaces of the first copper foil layer and the second copper foil layer are far away from each other, the two first surfaces are the outer surfaces of the carrier, and the outer surfaces are used for subsequent circuit production;
[0061] Step 2: Preparation of the anti-corrosion layer 14: Figure 3 As shown, an anti-corrosion layer 14 is formed by photolithography on at least one outer surface of the carrier 10, and the anti-corrosion layer 14 is a titanium layer or a composite layer of titanium and copper; a dense anti-corrosion layer is formed on the surface of the carrier, which can effectively prevent the etching solution from attacking the embedded circuit copper layer when removing the copper foil layer; and the titanium can be removed by sulfuric acid or hydrochloric acid solution without affecting the circuit copper layer, and the height difference between the embedded circuit layer and the insulating dielectric layer can be accurately controlled;
[0062] Step 3: Making the first buried wiring layer 16: that is, making the surface embedded wiring.
[0063] 3.1 Preparation of anti-plating photosensitive layer: Figure 4 As shown, a photosensitive layer 15 is formed by lamination, exposure, and development, and a pattern circuit area 18 on the resist layer 14 where a pattern needs to be made is exposed;
[0064] 3.2 Electroplating: Figure 5 As shown, the embedded first buried wire layer 16 is formed by electroplating on the exposed pattern circuit area 18 on the anti-corrosion layer 14 of the carrier, that is, the embedded circuit is formed;
[0065] 3.3 De-filming: Figure 6 As shown, the electroplated product is subjected to a film stripping process to remove the photosensitive layer 15, exposing the pattern circuit and its spacing space;
[0066] Step 4: Post-processing
[0067] 4.1 Addition layer manufacturing: filling the first buried wire layer 16 with an insulating medium to form an insulating medium layer 17;
[0068] 4.2 Preparation of the second buried wire layer 21:
[0069] ① Blind hole processing: processing a blind hole in the insulating dielectric layer 17;
[0070] ②Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer 17 and the blind hole;
[0071] ③ Fabrication of graphic circuits: fabricating a second buried wiring layer 21 on the seed layer;
[0072] 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer 22; that is, the preparation of filling the insulating medium and the graphic circuit layer is repeated, and one layer of board is added each time steps 4.1 and 4.2 are repeated. When the number of repetitions is 0, the formed board is a double-layer board, and when the number of repetitions is greater than or equal to 1, the formed board is a multi-layer board, such as Figure 7 As shown, the third buried wire layer to the n-1th buried wire layer and the insulating dielectric layer therebetween are omitted in the figure;
[0073] 4.4 Removing the carrier 10: Figure 8 As shown, firstly, the first copper foil layer 11 and the second copper foil layer 12 are separated, and then the first copper foil layer 11 or the second copper foil layer 12 is removed by etching to obtain a product having an anti-corrosion layer 14, such as Fig. 9 As shown; when single-sided manufacturing is performed, for example, a circuit is made on the outer surface of the first copper foil layer, the carrier 10 is separated, the second copper foil layer 12 is removed, and the first copper foil layer 11 is etched away to obtain a plate with an anti-corrosion layer; when double-sided manufacturing is performed, circuits are made on both the first copper foil layer and the second copper foil layer, the carrier 10 is separated to obtain two plates, and the first copper foil layer or the second copper foil layer is etched away respectively to obtain two plates with an anti-corrosion layer;
[0074] 4.5 Removal of the resist layer 14: Fig.10As shown, sulfuric acid or hydrochloric acid is used to remove the anti-corrosion layer 14 in the product to obtain a product with a buried wire layer on one side. According to the product design requirements, the following post-processing steps are performed: solder mask → surface treatment → molding → finished product testing → finished product inspection → packaging and shipment to form a finished board, and the final finished product is the package carrier board.
[0075] In one embodiment, in step 1: a frame 13 is also prepared, and the first copper foil layer 11 and the second copper foil layer 12 are bonded together through the frame 13, specifically: at a temperature of 80-120°C, glue is applied to the upper and lower surfaces of the frame 13, and then two pieces of copper foil are respectively bonded to the upper and lower surfaces of the frame to form a carrier 10, the frame 13 is an annular structure with a hollow interior, the width of the frame is 5-15mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16-18ppm / °C. Figure 2 As shown, the carrier component 10 is composed of a first copper foil layer 11, a frame 13 and a second copper foil layer 12. Preferably, the thickness of the conventional copper foil is 17.5 μm or 35 μm. When the temperature returns to room temperature, the copper foil has a larger CTE and shrinks more when cooled to room temperature, so that the copper foil is in a taut state, thereby improving the quality of the carrier component and thus improving the production yield of the product. At this time, the carrier component is completed and the subsequent production process can be single-sided or double-sided processing.
[0076] When the carrier 10 is composed of the first copper foil layer 11, the frame 13 and the second copper foil layer 12, the above step 4.4 specifically includes the following processes:
[0077] ① Edge milling: edge milling is performed along the distance of 2-5mm from the inner side of the frame 13 to separate the first copper foil layer from the second copper foil layer; (i.e., the frame is partially removed by edge milling. If it is double-sided molding, it is separated into two boards, i.e., two products after edge milling. If it is single-sided molding, it is separated into one board and one copper foil after edge milling. The first copper foil layer and the second copper foil layer are connected by the frame, which is more convenient for the board separation process;)
[0078] ② Frame processing: The frame 13 after the milling process is etched, the residual glue is removed, and the impurities are removed to obtain a reusable frame 13; (The processed frame can be recycled and reused, which reduces the production cost of the product;)
[0079] ③Remove the copper foil layer: Remove the first copper foil layer or the second copper foil layer by alkaline etching. (In this process, the etching solution will not attack the anti-corrosion layer, thereby effectively preventing the etching solution from attacking the embedded circuits on the surface.)
[0080] In another embodiment, the step 1 is specifically as follows: after a layer of glue is evenly coated around one of the copper foils near the edge area, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to form the carrier 10. (As shown in FIG. Figure 1 As shown, the carrier 10 is composed of a first copper foil layer 11 and a second copper foil layer 12. The two copper foils are bonded together only near the edge area by glue to facilitate subsequent board separation. Preferably, glue is applied within a range of about 10 mm near the edge of the copper foil. The thickness of the conventional copper foil is 17.5μm or 35μm.
[0081] When the carrier 10 is composed of the first copper foil layer 11 and the second copper foil layer 12, the above step 4.4 specifically includes the following processes:
[0082] ① Edge milling: The first copper foil layer 11 and the second copper foil layer 12 are connected by milling at a distance of 2-5 mm from the inside, and the first copper foil layer 11 and the second copper foil layer 12 are separated; (that is, the connecting portion of the first copper foil layer 11 and the second copper foil layer 12 is removed by milling. If it is double-sided molding, it is separated into two boards, i.e., two products after milling. If it is single-sided molding, it is separated into one board and one copper foil after milling;)
[0083] ②Remove the copper foil layer: remove the first copper foil layer or the second copper foil layer by alkaline etching. (In this process, the etching liquid will not attack the anti-corrosion layer, thereby effectively preventing the etching liquid from attacking the embedded circuits on the surface.)
[0084] In the above step 2, when the anti-corrosion layer is a titanium layer, a titanium layer is directly projected on the outer surface of the carrier 10, and the thickness of the titanium layer is 0.05-0.2 μm; when the anti-corrosion layer is a composite layer of titanium and copper, a titanium layer is first projected on the outer surface of the carrier 10, and the thickness of the titanium layer is 0.05-0.2 μm, and then a copper layer is projected on the titanium layer, and the thickness of the copper layer is 0.5-0.2 μm. Because titanium is easily oxidized, copper is used to protect it.
[0085] In step 4.5: when the anti-corrosion layer is a titanium layer, sulfuric acid or hydrochloric acid solution can be directly used to remove the titanium layer; when the anti-corrosion layer is a composite layer of titanium and copper, sulfuric acid or hydrochloric acid solution is first used to remove the titanium layer, and then the copper layer is removed by micro-etching process. When sulfuric acid or hydrochloric acid solution is used to remove titanium, the copper layer of the circuit is not affected, and the height difference between the embedded circuit layer on the surface and the insulating dielectric layer can be accurately controlled; when removing the copper layer in the anti-corrosion layer, the micro-etching process in conventional pre-treatment can be used to remove it, and the amount of micro-etching can be controlled within 0.5μm, without the need for special flash etching solution or high-precision equipment.
[0086] The step 3.1 specifically includes the following processes:
[0087] ① Lamination: making a photosensitive layer 15, uniformly coating a layer of photosensitive layer 15 on the anti-etching layer 14 by lamination or coating; the photosensitive layer is directly formed on the anti-etching layer of the carrier;
[0088] ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution;
[0089] ③ Development: The photosensitive layer in the unreacted area is removed, and the area where the photopolymerization reaction occurs is retained, that is, the graphic circuit area 18 to be produced is exposed, and the non-graphic circuit area is covered with the anti-plating photosensitive layer 15.
[0090] The step 4.1 specifically includes the following process:
[0091] ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding strength between the circuit and the insulating medium and improve product performance; the graphic circuit layer is the first, second, third... buried wire layer. If the final carrier board is a three-layer board, the graphic circuit layer here is the first buried wire layer and the second buried wire layer. If the final carrier board is a four-layer board, the graphic circuit here is the first, second buried wire layer and the third buried wire layer, and so on.
[0092] ② Filling with insulating medium: forming an insulating medium layer 17 on the graphic circuit layer through a process of pressing or vacuum pressing combined with baking; the process of filling with insulating medium is not limited to the above two methods, as long as it matches the processing characteristics of the insulating medium.
[0093] In step 4.2, in step ①, a blind hole is made by laser windowing and laser drilling, and the alignment reference in the production process is the target hole with the inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference in the production process is the inner target; in step 4.2, in step ②, the seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when making the pattern, according to the pattern wiring density, the additive method is combined with the pattern electroplating or the subtractive method is combined with the whole board electroplating and etching process to carry out the pattern layer addition. Of course, the blind hole processing method is not limited to laser windowing plus laser drilling process or LDD (Laser Direct Drilling); the seed layer production is not limited to the copper deposition process and the sputtering process, and the same conduction function can be achieved; the pattern wiring is not limited to the additive method or the subtractive method, and the pattern production can be achieved, wherein the additive method, the pattern electroplating, the semi-additive method, the subtractive method, the whole board electroplating and etching are all conventional processes in this field, and will not be introduced in detail here.
[0094] like Fig.10 As shown, a surface-embedded precision circuit packaging carrier with accurately controlled depth is manufactured using the above-mentioned processing technology.
[0095] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present application, and these modifications and improvements are all within the scope of protection of the present application. Therefore, the scope of protection of the patent of the present application shall be subject to the attached claims.
Claims
1. A processing technology for surface-embedded precision circuit packaging substrate with precise depth control, Features: The steps include: Step 1: Preparation of a carrier member (10): preparing two conventional copper foils, and bonding the two copper foils together by glue to form a carrier member (10), that is, the carrier member (10) comprises a first copper foil layer (11) and a second copper foil layer (12), the two outer surfaces of the carrier member (10) are defined as outer surfaces, and the two inner surfaces of the carrier member (10) are defined as inner surfaces, and the two inner surfaces are bonded together; Step 2: Preparation of an anti-corrosion layer (14): forming an anti-corrosion layer (14) on at least one outer surface of the carrier (10) by radiography, wherein the anti-corrosion layer (14) is a titanium layer or a composite layer of titanium and copper; Step 3: Preparation of the first buried wire layer (16): 3.1 Preparation of anti-plating photosensitive layer: by lamination, exposure and development, a photosensitive layer (15) is formed, and the pattern circuit area (18) on the resist layer (14) where the pattern needs to be made is exposed; 3.2 Electroplating: Electroplating is used to form an embedded first buried wire layer (16) on the exposed pattern circuit area (18) on the anti-corrosion layer (14) of the carrier; 3.3 De-filming: De-filming the electroplated product to remove the photosensitive layer (15) to expose the pattern circuit and its spacing space; Step 4: Post-processing 4.1 Addition layer production: filling the first buried wire layer (16) with an insulating medium to form an insulating medium layer (17); 4.2 Preparation of the second buried wire layer (21): ① Blind hole processing: processing a blind hole in the insulating dielectric layer (17); ② Seed layer preparation: a seed layer is prepared on the surface of the insulating dielectric layer (17) and the blind hole; ③ Fabrication of graphic circuits: fabricating a second buried wiring layer (21) on the seed layer; 4.3 Repeat steps 4.1 and 4.2 until an n-layer board is formed, where n ≥ 2, and n is a natural number, and the outermost layer of the product is the outer graphic circuit layer (22); 4.4 Removing the carrier (10): firstly, separating the first copper foil layer (11) and the second copper foil layer (12), and then removing the first copper foil layer (11) or the second copper foil layer (12) by etching, so as to obtain a product having an anti-corrosion layer (14); 4.5 Removing the anti-corrosion layer (14): using sulfuric acid or hydrochloric acid to remove the anti-corrosion layer (14) in the product, and obtaining a product with a buried wiring layer on one side; The step 3.1 specifically includes the following processes: ① Lamination: making a photosensitive layer (15), uniformly coating a photosensitive layer (15) on the anti-corrosion layer (14) by lamination or coating; ②Exposure: The finished graphics that do not need to be produced are transferred by image transfer, so that light and the photosensitive layer undergo polymerization reaction, forming a pattern that cannot be removed by the developer but can be removed by the stripping solution; ③ Development: removing the photosensitive layer in the unreacted area and retaining the area where the photopolymerization reaction occurs, that is, exposing the pattern circuit area (18) to be produced, and covering the non-pattern circuit area with the anti-plating photosensitive layer (15); The step 4.1 specifically includes the following process: ① Pre-treatment: Clean and roughen the surface of the graphic circuit layer to increase the bonding force between the circuit and the insulating medium and improve product performance; ② Filling with insulating medium: forming an insulating medium layer (17) on the pattern circuit layer by lamination or vacuum lamination combined with baking; In step 4.2, in step ①, a blind hole is made by laser window opening and laser drilling, and the alignment reference during the production process is a target hole with an inner target as the reference; or a blind hole is made by laser direct blind hole formation, and the alignment reference during the production process is an inner target; in step 4.2, in step ②, a seed layer is made by copper deposition or sputtering; in step 4.2, in step ③, when the pattern is produced, according to the pattern wiring density, an additive method combined with pattern electroplating or a subtractive method combined with whole-board electroplating and etching process is used to carry out pattern layer production.
2. According to the processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control as described in claim 1, Features: In step 1: a frame (13) is also prepared, and the first copper foil layer (11) and the second copper foil layer (12) are bonded together through the frame (13), specifically: at a temperature of 80 to 120°C, glue is applied to the upper surface and the lower surface of the frame (13), and then two pieces of copper foil are respectively bonded to the upper surface and the lower surface of the frame to form a carrier (10), the frame (13) is an annular structure with a hollow interior, the width of the frame is 5 to 15 mm, the material of the frame is 316 stainless steel or Invar alloy, the thermal expansion coefficient of the frame is ≤12ppm / °C, the thickness of the conventional copper foil is 17.5μm, 35μm or 50μm, and the thermal expansion coefficient of the conventional copper foil is 16 to 18ppm / °C.
3. According to the processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control as described in claim 1, Features: The step 1 specifically comprises: after a layer of glue is evenly coated around the edge area of one of the copper foils, another copper foil is aligned and attached to the surface of the copper foil coated with glue, and then flattened and baked to solidify to form a carrier (10).
4. According to claim 2, the processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control, Features: The above step 4.4 specifically includes the following processes: ① Edge milling: edge milling is performed along the distance 2-5 mm from the inner side of the frame (13) to separate the first copper foil layer from the second copper foil layer; ② Frame processing: etching, removing residual glue and impurities from the frame (13) after edge milling to obtain a reusable frame (13); ③Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
5. According to claim 3, the processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control, Features: The above step 4.4 specifically includes the following processes: ① Edge milling: edge milling is performed along the inner side of the connection between the first copper foil layer (11) and the second copper foil layer (12) at a distance of 2-5 mm, so as to separate the first copper foil layer (11) and the second copper foil layer (12); ②Removing the copper foil layer: removing the first copper foil layer or the second copper foil layer by alkaline etching.
6. The processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control according to claim 1, Features: In the above step 2, when the anti-corrosion layer is a titanium layer, a titanium layer is directly projected on the outer surface of the carrier (10), and the thickness of the titanium layer is 0.05-0.2 μm; when the anti-corrosion layer is a composite layer of titanium and copper, a titanium layer is first projected on the outer surface of the carrier (10), and the thickness of the titanium layer is 0.05-0.2 μm, and then a copper layer is projected on the titanium layer, and the thickness of the copper layer is 0.5-0.2 μm.
7. The processing technology of the surface layer embedded precision circuit packaging carrier with accurate depth control according to claim 1, Features: In step 4.5: when the anti-corrosion layer is a titanium layer, the titanium layer can be directly removed using sulfuric acid or hydrochloric acid solution; when the anti-corrosion layer is a composite layer of titanium and copper, the titanium layer is first removed using sulfuric acid or hydrochloric acid solution, and then the copper layer is removed by a micro-etching process.
8. A surface-embedded precision circuit packaging substrate with precise depth control, Features: The method is manufactured by using the processing technology described in any one of claims 1 to 7.