Fluidized bed reactor and method for recovering active metals of lithium secondary battery using the same

By setting up a dispersion plate and a multi-layer injection column in the fluidized bed reactor, a uniform reaction area is formed, which solves the problems of uneven reaction and environmental pollution in the recovery of active metals of lithium secondary batteries, and achieves efficient and reliable lithium secondary Battery active metal recycling.

CN114845802BActive Publication Date: 2024-11-08SK INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080090214.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-03
Publication Date
2024-11-08
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

In the prior art, when recovering the active metals of lithium secondary batteries, the dry reaction is uneven due to the unreasonable design of the reactor, the recovery rate of active substances is low and the selectivity is low, and the wet method has a risk of environmental pollution.

Method used

A fluidized bed reactor including a dispersed plate is designed. By setting up a multi-layer injection column at the bottom of the reactor, a uniform reaction area is formed to ensure uniform diffusion and dispersion of the reaction gas, and preventing the reaction gas from being on the inner wall and bottom plate surface of the reactor. Dead zones are formed to inhibit the aggregation of active substance particles, thereby improving recycling efficiency.

Benefits of technology

The dry recycling of the active metal of lithium secondary battery is achieved with high purity and high yield, which improves the reaction efficiency, reduces the risk of environmental pollution, and enhances the reliability of the recycling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114845802B_ABST
    Figure CN114845802B_ABST
Patent Text Reader

Abstract

The fluidized bed reactor includes a reactor body and a dispersion plate connected to the bottom of the reactor body, the dispersion plate includes a bottom plate and an injection column protruding from the upper surface of the bottom plate. The injection column includes a first injection column arranged at the central part of the dispersion plate and a second injection column arranged at the peripheral part of the dispersion plate. The height of the second injection column is greater than the height of the first injection column. The reaction gas is uniformly injected into the wall surface of the reactor through the dispersion plate, thereby improving the recovery rate of the active metal of the lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fluidized bed reactor and a method for recovering active metals of a lithium secondary battery using the fluidized bed reactor. More specifically, the present invention relates to a fluidized bed reactor including a dispersion plate and a method for recovering active metals of a lithium secondary battery using the fluidized bed reactor. Background Art

[0002] Recently, secondary batteries have been widely used as power sources for mobile electronic devices such as camcorders, mobile phones, notebook computers, etc., and vehicles such as electric vehicles, hybrid vehicles, etc. Lithium secondary batteries have attracted much attention among secondary batteries due to their advantages such as high operating voltage and high energy density per unit weight, high charging rate, and compact size.

[0003] Lithium metal oxide can be used as an active material of a positive electrode of a lithium secondary battery. Lithium metal oxide may further contain a transition metal such as nickel, cobalt, manganese, and the like.

[0004] Since the above-mentioned high-cost valuable metals are used for the positive electrode active material, the production cost of manufacturing the positive electrode material is more than 20%. In addition, since environmental protection issues have recently attracted much attention, the recycling method of the positive electrode active material is being studied.

[0005] Conventionally, a method of sequentially recovering valuable metals by leaching spent positive electrode active materials in a strong acid such as sulfuric acid has been used, but the wet method may be disadvantageous in terms of regeneration selectivity and regeneration time, and may cause environmental pollution. Therefore, a method of recovering valuable metals by contact with a reaction gas using a dry reaction is being studied.

[0006] However, as the size of active material particles supplied for dry reaction becomes smaller, non-uniform reaction may occur due to aggregation. In addition, due to the local non-uniform supply of reaction gas in the reactor, the recovery rate of the active material may be reduced.

[0007] For example, Korean Registered Patent Publication No. 10-0709268 discloses an apparatus and method for recycling waste manganese batteries and alkaline batteries, but does not provide a dry method for regenerating valuable metals with high selectivity and high yield. Summary of the invention

[0008] [Technical goals]

[0009] According to one aspect of the present invention, a fluidized bed reactor having improved reaction efficiency and reliability is provided.

[0010] According to one aspect of the present invention, a method for recovering active metals of a lithium secondary battery using a fluidized bed reactor is provided.

[0011] [Technical means]

[0012] The fluidized bed reactor according to an embodiment of the present invention comprises a reactor body and a dispersion plate connected to the bottom of the reactor body, the dispersion plate comprising a bottom plate and an injection column protruding from the upper surface of the bottom plate. The injection column comprises a first injection column arranged at the central part of the dispersion plate and a second injection column arranged at the peripheral part of the dispersion plate, the height of the second injection column being greater than the height of the first injection column.

[0013] In some embodiments, the first injection column may include a first column extending from the upper surface of the bottom plate, a first cap covering the upper portion of the first column, and a first injection hole passing through the first column. The second injection column may include a second column extending from the upper surface of the bottom plate, a second cap covering the upper portion of the second column, and a second injection hole passing through the second column.

[0014] In some embodiments, the first injection hole and the second injection hole may be inclined toward an upper surface of the bottom plate.

[0015] In some embodiments, a height of the second injection hole may be greater than a height of the first injection hole.

[0016] In some embodiments, the height of the second injection hole may be adjusted so that a straight line in an inclined direction of the second injection hole may contact the wall surface of the reactor body.

[0017] In some embodiments, the second injection hole may include an upper injection hole and a lower injection hole, and a height of the upper injection hole may be greater than a height of the first injection hole.

[0018] In some embodiments, the upper injection hole and the lower injection hole may be inclined toward the bottom plate.

[0019] In some embodiments, the upper injection hole may be inclined toward the bottom plate, and the lower injection hole may be inclined from the bottom plate toward the top of the reactor body.

[0020] In some embodiments, the injection pillars may be arranged at a constant pitch or in a constant grid shape.

[0021] In some embodiments, the fluidized bed reactor may further include a reaction gas flow path for supplying the reaction gas from a portion of the reactor body below the bottom plate.

[0022] In the method for recovering active metals of a lithium secondary battery according to an embodiment of the present invention, a waste positive electrode active material mixture obtained from a waste positive electrode of a lithium secondary battery is prepared. The waste positive electrode active material mixture is reacted in a fluidized bed reactor of the embodiment described above to form a primary precursor mixture. A lithium precursor is selectively recovered from the primary precursor mixture.

[0023] In some embodiments, in the formation of the primary precursor mixture, the reaction gas may be injected through an injection column included in a dispersion plate of a fluidized bed reactor.

[0024] In some embodiments, the reactant gas may include hydrogen.

[0025] In some embodiments, the primary precursor mixture may include primary lithium precursor particles and transition metal-containing particles.

[0026] In some embodiments, the primary lithium precursor particles may include at least one of lithium hydroxide, lithium oxide, and lithium carbonate.

[0027] In some embodiments, in the recovery of the lithium precursor, the primary lithium precursor particles may be washed with water.

[0028] [Effects of the invention]

[0029] According to the above exemplary embodiment, a dispersion plate may be disposed at the bottom of the fluidized bed reactor to promote diffusion and uniform dispersion of the reaction gas. The dispersion plate may include an injection column protruding from the bottom plate and including an injection flow path, and a higher injection column may be disposed at a peripheral portion of the bottom plate.

[0030] Accordingly, it is possible to prevent dead zones, which may not be reached by the reaction gas, from being generated on the surfaces of the inner wall and the bottom plate of the reactor, and to form a uniform reaction zone and fluidized bed.

[0031] The fluidized bed reactor according to the exemplary embodiment can be used in the recycling process by hydrogen reduction of the positive active material of the lithium secondary battery. Aggregation of active material particles can be suppressed by the dispersion plate, and active material recovery efficiency can be improved by forming a uniform reaction fluidized bed. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a schematic top view showing a dispersion plate of a fluidized bed reactor according to an exemplary embodiment.

[0033] Figure 2 is a schematic cross-sectional view illustrating a configuration of an injection column of a dispersion plate according to an exemplary embodiment.

[0034] Figure 3 is a schematic cross-sectional view for describing a configuration of a second injection column according to an exemplary embodiment.

[0035] Figure 4 and Figure 5 is a schematic cross-sectional view illustrating a configuration of a second injection column of a dispersion plate according to some exemplary embodiments.

[0036] Figure 6is a schematic diagram for describing a fluidized bed reactor and a method of recovering active metals of a lithium secondary battery using the fluidized bed reactor according to an exemplary embodiment. DETAILED DESCRIPTION

[0037] The embodiment of the present invention provides a fluidized bed reactor that can form a completely uniform reaction zone and fluidized bed by using a dispersion plate. In addition, the embodiment of the present invention provides a dry, high-purity, high-yield method for recovering active metals from lithium secondary batteries using a fluidized bed reactor.

[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, these embodiments are provided as examples, and the present invention is not limited to the specific embodiments described herein.

[0039] As used herein, the term "precursor" is used to generally refer to a compound containing a specific metal to provide the specific metal contained in an electrode active material.

[0040] Figure 1 is a schematic top view showing a dispersion plate of a fluidized bed reactor according to an exemplary embodiment. Figure 2 is a schematic cross-sectional view showing the configuration of an injection column of a dispersion plate according to an exemplary embodiment. For example, Figure 2 is along Figure 1 A cross-sectional view taken along line II'.

[0041] Reference Figure 1 and Figure 2 The dispersion plate may include a bottom plate 50 and a plurality of first injection pillars 60 and a plurality of second injection pillars 70 protruding from the bottom plate 50 .

[0042] The bottom plate 50 may be, for example, a circular plate or a polygonal plate formed of a metal material or a ceramic material.

[0043] The first injection pillars 60 and the second injection pillars 70 may have a shape protruding from the upper surface of the base plate 50. The first injection pillars 60 and the second injection pillars 70 may be regularly arranged on the upper surface of the base plate 50 with a constant arrangement (e.g., a constant grid arrangement) and arrangement interval for uniform diffusion and distribution of the reaction gas.

[0044] For example, the first injection pillars 60 and the second injection pillars 70 may have an array shape or a grid shape arranged at vertices of a polygon such as a triangle, a square, or a hexagon. Figure 1 As shown, the first injection pillars 60 and the second injection pillars 70 may be arranged, for example, based on an equilateral triangle pitch.

[0045] The first and second injection pillars 60 and 70 may include a first injection pillar 60 disposed within a predetermined radius from a central portion C of the bottom plate 50 and a second injection pillar 70 disposed at a peripheral portion or outside of the bottom plate 50 .

[0046] like Figure 2 As shown, each first injection column 60 may include a first column 62 and a first cap 64 and each second injection column 70 may include a second column 72 and a second cap 74. For example, the first injection column 60 and the second injection column 70 may have a bubble cap or tuyere structure.

[0047] The first injection column 60 may include a first column 62 and a first cap 64 covering an upper portion of the first column 62. The second injection column 70 may include a second column 72 and a second cap 74 covering an upper portion of the second column 72.

[0048] The first injection pillar 60 may include a first injection hole 66 passing through the first pillar 62. The second injection pillar 70 may include a second injection hole 76 passing through the second pillar 72.

[0049] like Figure 2 As shown, the first injection hole 66 and the second injection hole 76 may be formed to be inclined from the top of the first injection column 60 and the second injection column 70 toward the bottom plate 50. For example, the first injection hole 66 and the second injection hole 76 may have a shape extending from the top of the first injection column 60 and the second injection column 70 toward the bottom plate 50.

[0050] In one embodiment, an inclination angle between a vertical direction from the upper surface of the bottom plate 50 and the first and second injection holes 66 and 76 may be about 30° to 60°.

[0051] The first injection hole 66 and the second injection hole 76 are formed to be inclined with respect to the upper surface of the bottom plate 50 so that the reaction gas can be sprayed and diffused in a direction toward the bottom plate 50. Therefore, since reactants (e.g., precursor particles or active material particles) that may settle on the upper surface of the bottom plate 50 can move upward, the formation of the fluidized bed can be promoted.

[0052] In an exemplary embodiment, the height of the second injection pillars 70 disposed on the peripheral portion of the bottom plate 50 may be greater than that of the first injection pillars 60. Accordingly, the height of the second injection holes 76 may also be greater than that of the first injection holes 66.

[0053] As described above, if the first injection pillars 60 and the second injection pillars 70 are arranged at a predetermined pitch (e.g., a triangular arrangement) on the bottom plate 50, an area where the injection pillars may not be arranged at a predetermined pitch may be generated at a peripheral portion or an outer portion of the bottom plate 50. Figure 1As shown by the dotted oval in FIG. , a dead zone D may be generated where the reaction gas may not be able to reach.

[0054] In this case, the reaction gas may not reach the wall surface of the reactor body, and the fluidized bed may not be uniformly generated. In addition, the aggregated reactant particles may adhere to the wall surface of the reactor body, thereby reducing the reaction yield.

[0055] However, according to the exemplary embodiment, the second injection pillar having a relatively increased height may be disposed on the peripheral portion of the bottom plate 50 where the dead zone D is easily generated. Therefore, the injection distance and injection height of the reaction gas may be increased in the peripheral portion.

[0056] Accordingly, the reaction gas can reach the wall surface of the reactor body to prevent the stagnation and agglomeration of the reactant particles, thereby promoting the formation of a fluidized bed. Figure 1 The dead zone D at the peripheral portion shown can be significantly reduced or eliminated.

[0057] exist Figure 1 In the central portion C of the dispersion plate shown, a support or injection column of the dispersion plate can be provided. For example, a first injection column 60 can also be arranged in the central portion C, and as described above, the first injection column 60 can be arranged at a predetermined distance from the central portion C in the radial direction.

[0058] Figure 3 is a schematic cross-sectional view for describing a configuration of a second injection column according to an exemplary embodiment.

[0059] Reference Figure 3 In the second injection column 70 , the height H of the second injection hole 76 may be adjusted so that the reaction gas may contact the wall surface of the reactor body 110 .

[0060] For example, the minimum height of the second injection hole 76 may be a height at which a straight line extending from the second injection hole 76 can reach the lowest point of the reactor body 110 .

[0061] Figure 4 and Figure 5 is a schematic cross-sectional view illustrating a configuration of a second injection column of a dispersion plate according to some exemplary embodiments.

[0062] Reference Figure 4 and Figure 5 , the second injection pillar 70 may include a plurality of injection holes located at different heights.

[0063] like Figure 4As shown, the second injection column 70 may include an upper injection hole 76a and a lower injection hole 76b. In some embodiments, the height of the upper injection hole 76a may be set so that a straight line in the injection direction can contact the wall surface of the reactor body, as shown in FIG. Figure 3 The height of the upper injection hole 76 a may be greater than the height of the first injection hole 66 of the first injection pillar 60 .

[0064] The lower injection hole 76b may be added to the second injection column 70 so that the reaction gas may be additionally supplied to the Figure 1 The dead zone D is shown. Therefore, the effects of preventing particles from stagnating / aggregating on the wall surface of the reactor body 110 through the upper injection hole 76a and reducing / removing the dead zone D through the lower injection hole 76b can be achieved together.

[0065] like Figure 5 As shown, the lower injection hole 76c may be inclined upward. For example, the lower injection hole 76c may extend from the bottom plate 50 toward the top of the reactor body 110. In this case, the rising action of the fluidized bed may be promoted by the lower injection hole 76c.

[0066] Figure 6 is a schematic diagram for describing a fluidized bed reactor and a method of recovering active metals of a lithium secondary battery using the fluidized bed reactor according to an exemplary embodiment.

[0067] In the following, reference will be made to Figure 6 A method of recovering active metals of a lithium secondary battery and a configuration / structure of a fluidized bed reactor including the above-mentioned dispersion plate are described together.

[0068] Reference Figure 6 , a waste positive electrode active material mixture may be prepared from waste positive electrodes of lithium secondary batteries (eg, in the process of S10 ).

[0069] A lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator layer between the positive electrode and the negative electrode. The positive electrode and the negative electrode may include a positive electrode active material layer coated on a positive electrode current collector and a negative electrode active material layer coated on a negative electrode current collector, respectively.

[0070] For example, the positive electrode active material included in the positive electrode active material layer may include an oxide containing lithium and a transition metal.

[0071] In some embodiments, the positive active material may include a compound represented by Chemical Formula 1 below.

[0072] [Chemical formula 1]

[0073] Li x M1 a M2 b M3c O y

[0074] In Chemical Formula 1, M1, M2, and M3 may each be a transition metal selected from Ni, Co, Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, or B. In Chemical Formula 1, 0 < x ≤ 1.1, 2 ≤ y ≤ 2.02, 0 < a < 1, 0 < b < 1, 0 < c < 1, and 0 < a + b + c ≤ 1.

[0075] In some embodiments, the positive electrode active material may be an NCM-based lithium oxide including nickel, cobalt, and manganese.

[0076] The spent positive electrode can be recovered by separating the positive electrode from the spent lithium secondary battery. The spent positive electrode may include the positive electrode current collector (e.g., aluminum (Al)) and the positive electrode active material layer as described above, and the positive electrode active material layer may include a conductive material, a binder, and the positive electrode active material as described above.

[0077] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, and carbon nanotubes. The binder may include a resin material such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, and the like.

[0078] In an exemplary embodiment, the recovered spent positive electrode may be pulverized to produce a spent positive electrode active material mixture. Accordingly, the spent positive electrode active material mixture may be prepared in a powder form. As described above, the spent positive electrode active material mixture may include powders of lithium-transition metal oxides such as powders of NCM-based lithium oxides (e.g., Li(NCM)O2).

[0079] The term "spent positive electrode active material mixture" used in the present application may refer to a raw material that is put into the fluidized bed reaction treatment described later after substantially removing the positive electrode current collector from the spent positive electrode. In one embodiment, the spent positive electrode active material mixture may include positive electrode active material particles such as NCM-based lithium oxides. In one embodiment, the spent positive electrode active material mixture may include component parts derived from the binder or the conductive material. In one embodiment, the spent positive electrode active material mixture may consist essentially of positive electrode active material particles.

[0080] In some embodiments, the average particle size (D50) of the spent positive electrode active material mixture may be 5 μm to 100 μm. Within the above range, lithium-transition metal oxides to be recovered such as Li(NCM)O2 can be easily separated from the positive electrode current collector, the conductive material, and the binder contained in the spent positive electrode active material mixture.

[0081] In some embodiments, the spent positive electrode active material mixture may be heat treated before being put into the fluidized bed reactor described later. Impurities such as conductive materials and binders contained in the spent positive electrode active material mixture may be substantially removed or reduced by heat treatment, so that the lithium-transition metal oxide may be introduced into the fluidized bed reactor with high purity.

[0082] The temperature of the heat treatment may be, for example, about 100° C. to 500° C., preferably about 350° C. to 450° C. Within the above range, impurities may be substantially removed while preventing the lithium-transition metal oxide from being decomposed and damaged.

[0083] For example, during S20 , the spent positive electrode active material mixture may react in the fluidized bed reactor 100 to form a primary precursor mixture 90 .

[0084] like Figure 6 As shown, the fluidized bed reactor 100 may be divided into a reactor body 110, a lower reactor section 120, and an upper reactor section 130. The reactor body 110 may include a heating means such as a heater or may be integrated with a heating means such as a heater.

[0085] The dispersion plate may be connected to the bottom of the reactor body 110. Therefore, a lower portion of the reactor body 110 below the dispersion plate may be defined as a lower reactor portion 120.

[0086] The spent positive active material mixture may be supplied to the reactor body 110 through the supply flow path 106a and the supply flow path 106b. The spent positive active material mixture may be dripped through the first supply flow path 106a connected to the upper reactor part 130, or may be introduced through the second supply flow path 106b connected to the reactor body 110. In one embodiment, the first supply flow path 106a and the second supply flow path 106b may be used together to supply the spent positive active material mixture.

[0087] The reaction gas for converting the spent positive active material mixture into the primary precursor can be supplied to the reactor body 110 through the reaction gas flow path 102 connected to the lower reactor part 120. In some embodiments, the reaction gas can include a reducing gas. For example, hydrogen (H2) can be supplied.

[0088] The reaction gas may be discharged into the reactor body 110 through the first injection column 60 and the second injection column 70 included in the dispersion plate. The reaction gas may be supplied from the bottom of the fluidized bed reactor 100 to contact the spent positive active material mixture, so that the spent positive active material mixture may react with the reaction gas while moving to the upper reactor section 130 to be converted into a primary precursor.

[0089] In some embodiments, the lithium-transition metal oxide can be reduced by hydrogen to produce a primary lithium precursor including, for example, lithium hydroxide (LiOH), lithium oxide (e.g., Li2O) and a transition metal or transition metal oxide. For example, Ni, Co, NiO, CoO and MnO can be produced together with the primary lithium precursor by a reduction reaction.

[0090] The reduction reaction in the reactor body 110 may be performed at a temperature of about 400 to 700° C., preferably 450 to 550° C. Within the reaction temperature range, the reduction reaction may be promoted without causing reaggregation and recombination of the primary lithium precursor and the transition metal / transition metal oxide.

[0091] In some embodiments, a carrier gas may be supplied through the carrier gas flow path 104 together with the reaction gas from the lower reactor section 120. For example, the carrier gas may include an inert gas such as nitrogen (N2) or argon (Ar). The carrier gas may also be discharged and supplied through the first injection column 60 and the second injection column 70 of the dispersion plate to promote the formation of the fluidized bed. For example, the formation of a cyclone by the carrier gas may be promoted.

[0092] A primary precursor mixture 90 including primary lithium precursor particles 94 and transition metal-containing particles 92 (eg, transition metal or transition metal oxide) may be formed in the upper reactor section 130. The primary lithium precursor particles 94 may include, for example, lithium hydroxide, lithium oxide, and / or lithium carbonate.

[0093] In one embodiment, the transition metal-containing particles 92 including nickel, cobalt, or manganese may be relatively heavier than the primary lithium precursor particles 94, so that the primary lithium precursor particles 94 may be previously collected through the first outlet 160a and the second outlet 160b.

[0094] In one embodiment, the primary lithium precursor particles 94 may be discharged through the first outlet 160a connected to the upper reactor section 130. In this case, selective recovery of the primary lithium precursor particles 94 according to a weight gradient may be facilitated.

[0095] In one embodiment, the primary precursor mixture 90 including the primary lithium precursor particles 94 and the transition metal-containing particles 92 may be collected through the second outlet 160b connected to the upper reactor section 130. In this case, the primary precursor mixture 90 may be directly recovered from the fluidized bed formation area to increase the yield.

[0096] In one embodiment, the primary precursor mixture 90 may be collected together through the first outlet 160a and the second outlet 160b.

[0097] According to the above exemplary embodiment, the second injection column 70 disposed on the peripheral portion of the bottom plate 50 can facilitate the supply of reaction gas to the primary precursor mixture 90 accumulated or stagnant on the wall surface of the reactor body 110, thereby allowing the formation of the fluidized bed to be uniformly expanded.

[0098] Therefore, the total reaction area in the reactor body 110 may be increased to improve the reaction yield.

[0099] The primary lithium precursor particles 94 collected through the first outlet 160 a and the second outlet 160 b may be recovered as a lithium precursor (eg, during S30 ).

[0100] In some embodiments, the primary lithium precursor particles 94 may be washed with water. The primary lithium precursor particles in the form of lithium hydroxide (LiOH) may be substantially dissolved in water by the washing process, separated from the transition metal precursor, and recovered in advance. The lithium precursor substantially consisting of lithium hydroxide may be obtained by a crystallization process in which lithium hydroxide is dissolved in water, or the like.

[0101] In one embodiment, primary lithium precursor particles in the form of lithium oxide and lithium carbonate may be substantially removed by a washing process. In one embodiment, primary lithium precursor particles in the form of lithium oxide and lithium carbonate may be at least partially converted to lithium hydroxide by a washing process.

[0102] In some embodiments, the primary lithium precursor particles 94 can react with a carbon-containing gas such as carbon monoxide (CO), carbon dioxide (CO2), etc. to obtain lithium carbonate (e.g., Li2CO3) as a lithium precursor. A crystalline lithium precursor can be obtained by reacting with a carbon-containing gas. For example, lithium carbonate can be collected by injecting a carbon-containing gas together during a washing process.

[0103] In some embodiments, a transition metal precursor may be obtained from the collected transition metal-containing particles 92 (eg, during S40 ).

[0104] For example, primary lithium precursor particles 94 may be collected through first outlet 160a and second outlet 160b, and then transition metal-containing particles 92 may be recovered. Thereafter, transition metal-containing particles 92 may be treated with an acid solution to form a precursor in the form of an acid salt of each transition metal.

[0105] In one embodiment, sulfuric acid can be used as the acid solution. In this case, NiSO4, MnSO4 and CoSO4 can each be recovered as a transition metal precursor.

[0106] As described above, the lithium precursor can be collected by a dry process, and then the transition metal precursor can be selectively extracted using an acid solution, so that the purity and selectivity of each metal precursor can be improved, and the wet process load can be reduced, and the amount of wastewater and by-products can also be reduced.

Claims

1. A fluidized bed reactor, comprising: Reactor body; and a dispersion plate connected to the bottom of the reactor body, the dispersion plate comprising a bottom plate and an injection column protruding from an upper surface of the bottom plate; The injection column comprises: a first injection column disposed at a central portion of the dispersion plate; and a second injection column arranged at a peripheral portion of the dispersion plate, the height of the second injection column being greater than the height of the first injection column, The first injection column includes a first column extending from the upper surface of the bottom plate, a first cap covering the upper portion of the first column, and a first injection hole penetrating through the first column. The second injection column includes a second column extending from the upper surface of the bottom plate, a second cap covering an upper portion of the second column, and a second injection hole penetrating through the second column. The height of the second injection hole is adjusted so that a straight line in an inclined direction of the second injection hole contacts a wall surface of the reactor body. 2 . The fluidized bed reactor according to claim 1 , wherein the first injection hole and the second injection hole are inclined toward an upper surface of the bottom plate. 3 . The fluidized bed reactor according to claim 1 , wherein a height of the second injection hole is greater than a height of the first injection hole. 4 . The fluidized bed reactor according to claim 1 , wherein the second injection hole comprises an upper injection hole and a lower injection hole, and a height of the upper injection hole is greater than a height of the first injection hole. 5 . The fluidized bed reactor according to claim 4 , wherein the upper injection hole and the lower injection hole are inclined toward the bottom plate. 6 . The fluidized bed reactor according to claim 4 , wherein the upper injection hole is inclined toward the bottom plate, and the lower injection hole is inclined from the bottom plate toward the top of the reactor body.

7. The fluidized bed reactor according to claim 1, wherein the injection columns are arranged at a constant interval or in a constant grid shape.

8. The fluidized bed reactor according to claim 1, further comprising a reaction gas flow path for supplying a reaction gas from a portion of the reactor body below the bottom plate.

9. A method for recovering active metals from a lithium secondary battery, comprising: preparing a waste positive electrode active material mixture obtained from waste positive electrodes of lithium secondary batteries; reacting the spent positive electrode active material mixture in the fluidized bed reactor of claim 1 to form a primary precursor mixture; and A lithium precursor is selectively recovered from the primary precursor mixture.

10. The method for recovering active metals from lithium secondary batteries according to claim 9, wherein: Forming the primary precursor mixture includes injecting a reaction gas through an injection column included in a dispersion plate of the fluidized bed reactor.

11. The method for recovering active metals from lithium secondary batteries according to claim 10, wherein: The reaction gas includes hydrogen.

12. The method for recovering active metals from lithium secondary batteries according to claim 9, wherein: The primary precursor mixture includes primary lithium precursor particles and transition metal-containing particles.

13. The method for recovering active metals from lithium secondary batteries according to claim 12, wherein: The primary lithium precursor particles include at least one of lithium hydroxide, lithium oxide and lithium carbonate.

14. The method for recovering active metals from lithium secondary batteries according to claim 12, wherein: The recovering of the lithium precursor includes washing the primary lithium precursor particles with water.