A hot die casting water-soluble ceramic core for light alloy investment casting and a preparation method thereof

By using hot die-casting technology of materials such as electromelting corundum powder and potassium sulfate in investment casting, an alumina-based ceramic core with high collapse and stability was prepared, and the strength of the water-soluble salt core in investment casting was solved. The problem of insufficient stability meets the needs of complex shape cores and realizes an environmentally friendly production process.

CN114850412BActive Publication Date: 2024-11-29SOUTHEAST UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210446223.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-26
Publication Date
2024-11-29
Estimated Expiration
2042-04-26

AI Technical Summary

Technical Problem

The existing water-soluble salt cores have disadvantages such as low strength, large shrinkage, high brittleness, and strong hygroscopy in investment casting, which affects the shape and dimensional accuracy of the castings and is difficult to meet the needs of complex-shaped cores.

Method used

Using electromelting corundum powder as refractory aggregate and potassium sulfate as water-soluble salt binder, plasticizer, lubricant and surfactant are added, water-soluble ceramic cores are prepared through hot die-casting technology, combined with high-temperature sintering to improve crumbing Performance and stability.

Benefits of technology

Alumina-based ceramic core with good collapse, high dimensional accuracy and strong stability was obtained. It is suitable for the production of precision castings in complex shapes, reduces the amount of water-soluble salts, and has an environmentally friendly process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114850412B_ABST
    Figure CN114850412B_ABST
Patent Text Reader

Abstract

The present invention discloses a hot-die casting water-soluble ceramic core for light alloy investment casting and a preparation method thereof. The hot-die casting water-soluble ceramic core comprises fused corundum powder, potassium sulfate, plasticizer, lubricant and surfactant in a weight ratio of 60-80:7.7-30:10-15:1-2:1-2, wherein paraffin wax, beeswax, polyethylene, stearic acid and oleic acid are included in a weight ratio of 90-95:2-4:2-4:1-2:1-2. The core is formed by a hot-die casting method and then sintered at high temperature. The hot-die casting ceramic core of the present invention uses refractory aggregate and inorganic salt to form the base material of the ceramic core. Compared with the existing salt core, the core has the advantages of strong stability and high precision, reduces the amount of water-soluble salt used, and maintains good water-soluble disintegration. The hot-die casting process can meet the needs of actual production for complex-shaped cores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hot die casting water-soluble ceramic core for light alloy investment casting and a preparation method thereof, belonging to the field of investment precision casting. Background Art

[0002] With the rapid development of industries such as automobiles, aviation, and ships, the demand for load-bearing parts and structural parts with complex structures is increasing, which puts higher requirements on casting production. The use of aluminum and magnesium light alloy investment castings instead of composite parts helps to improve the reliability of equipment, but it also makes the casting structure more complicated, which brings certain difficulties to casting production, especially for thin-walled castings with complex structures. The selection and application of cores used to form the inner cavity are the key to obtaining high-quality castings. Aluminum and magnesium alloys have low strength, and large mechanical force cannot be used to remove the core. In addition, in many such castings, the size of the part of the core that communicates with the outside world is small, and it is not easy to apply mechanical force. In addition, the inner cavity of the casting often has an irregular shape, and it is difficult to transmit the force to the entire core. The use of cores with good water-soluble disintegration properties is the key to solving the forming and manufacturing of such light alloy investment castings with complex inner cavities.

[0003] In recent years, salt cores made of salts with good solubility in water have received much attention and have been used to a certain extent in actual production. However, it was found during use that water-soluble salt cores have disadvantages such as low strength, large shrinkage, large brittleness, and strong moisture absorption. During the long-term shell manufacturing process of investment casting, they are prone to moisture absorption and deliquescence and fall off, affecting the shape and dimensional accuracy of the castings, and even prematurely disintegrating, causing shell failure, which restricts the application of water-soluble salt cores in investment casting and also affects the development and application of related alloy castings.

[0004] Compared with the salt core prepared with pure water-soluble salt, the water-soluble ceramic core with refractory material as the matrix and water-soluble salt as the binder not only has good dimensional accuracy and higher stability in a humid environment while ensuring good water-soluble dispersibility, but also significantly reduces the amount of water-soluble salt used, which is more conducive to the recycling and reuse of the core material.

[0005] Water-soluble ceramic cores can be manufactured using a variety of forming processes, but different methods have their own limitations. For example, pressing is suitable for the manufacture of simple cores; slip casting can be used to manufacture complex cores, but because the slurry contains more water, it takes a long time to dry and sinter, and has large shrinkage; hot die casting can be used to manufacture complex cores, but it also has the disadvantage of a long production cycle. Of course, in order to meet the characteristics of different forming processes, the raw material composition of the ceramic core is also different. Summary of the invention

[0006] Purpose of the invention: The first purpose of the present invention is to provide a hot die casting water-soluble ceramic core for light alloy investment casting, which can be used for the production of aluminum and magnesium alloy investment castings with complex cavity structures; the second purpose of the present invention is to provide a hot die casting molding method for the hot die casting water-soluble ceramic core to guide the practical application of the hot die casting water-soluble ceramic core.

[0007] Technical solution: The hot-die casting water-soluble ceramic core for light alloy investment casting of the present invention comprises fused corundum powder, potassium sulfate, a plasticizer, a lubricant and a surfactant in a weight ratio of 60 to 80:7.7 to 30:10 to 15:1 to 2:1 to 2.

[0008] Wherein, the plasticizer comprises paraffin, beeswax, polyethylene, stearic acid and oleic acid, and the weight ratio thereof is 90-95:2-4:2-4:1-2:1-2.

[0009] Wherein, the lubricant is graphite powder or glycerol.

[0010] Wherein, the surfactant is sodium lauryl sulfate or stearamide.

[0011] The method for preparing the hot die casting water-soluble ceramic core for light alloy investment casting of the present invention adopts a hot die casting method to form the core, and then sintering the core at high temperature, comprising the following steps:

[0012] (1) mixing fused corundum powder, potassium sulfate and a surfactant, drying and ball milling to obtain a mixed ceramic powder;

[0013] (2) stirring and mixing the plasticizer and the lubricant, and adding the mixed ceramic powder in batches under stirring conditions, and continuing to stir to obtain a slurry with a certain fluidity;

[0014] (3) preheating the mold, pressing the slurry into the mold, maintaining the pressure for hot die casting, and opening the mold after the slurry solidifies to obtain a green billet;

[0015] (4) Sintering the green body to obtain a hot die-cast water-soluble ceramic core.

[0016] Preferably, in step (1), the drying temperature is 110-120° C., and the drying time is 1-3 hours.

[0017] Preferably, in step (1), the rotation speed of the ball mill during ball milling is 250 to 350 r / min, and the ball milling time is 1.5 to 2 h.

[0018] Preferably, in step (2), the temperature during stirring is 70-80° C., the speed of the stirrer during stirring is 200-300 r / min, and the continuous stirring time is 10-12 h.

[0019] Preferably, in step (3), the pressure-holding hot die casting process parameters are: temperature of 70-80° C., pressure of 0.2-0.4 MPa, and pressure-holding time of 6-8 s.

[0020] Preferably, in step (3), preheating the mold is to preheat the mold to 40-50°C.

[0021] Preferably, step (4) comprises slowly raising the temperature to 400° C. at a rate of 1° C. / min in an air atmosphere, keeping the temperature for 2 h, raising the temperature to 1000-1100° C. at a rate of 4° C. / min, and keeping the temperature for 0.5-1.0 h.

[0022] Preferably, in step (4), the sintering temperature is 1000-1100° C., and the sintering time is 0.5-1.5 h.

[0023] The present invention uses fused corundum powder as refractory aggregate, potassium sulfate as water-soluble salt binder, adds appropriate amount of plasticizer, lubricant and surfactant, adopts hot die casting process to prepare ceramic core blank, and then obtains water-soluble ceramic core through high temperature sintering. Since fused corundum powder is an amphoteric oxide, it will react with alkaline or acidic binder during high temperature sintering to generate water-insoluble substances, which affects the disintegration performance of the ceramic core. By using neutral potassium sulfate as binder, the prepared alumina-based ceramic core with good disintegration performance not only has good dimensional accuracy and suitable strength, but also has green and environmentally friendly sand cleaning method. The ceramic core using fused corundum powder as refractory aggregate and potassium sulfate as inorganic binder solves the shortcomings of soluble salt core, such as large brittleness, strong moisture absorption capacity and large shrinkage during forming, and has good water-soluble disintegration performance. The hot die casting forming method can meet the actual production needs for complex-shaped cores.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the alumina-based ceramic core with good disintegration prepared by the present invention not only has good dimensional accuracy and suitable strength, but also has the advantages of strong stability and high precision, reduces the amount of water-soluble salt used, and maintains good water-soluble disintegration, and the sand cleaning method is green and environmentally friendly. The water-soluble alumina-based ceramic core is obtained by hot die casting, and complex precision castings can be prepared to meet the needs of actual production for complex-shaped cores. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a sintering process diagram of the ceramic core of Example 1;

[0026] Figure 2 This is the relationship between the bending strength of the ceramic core and the amount of potassium sulfate added;

[0027] Figure 3 This is the relationship between the shrinkage rate of the ceramic core and the amount of potassium sulfate added;

[0028] Figure 4 This is a graph showing the relationship between the mass loss rate of the ceramic core after dissolution and the amount of potassium sulfate added. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0030] The present invention adopts a microcomputer-controlled electronic universal testing machine and a three-point bending method to test the room temperature bending strength, and the parameters are: a gauge length of 30 mm and a loading rate of 0.5 mm / min.

[0031] Measure the length of the sample before and after sintering, according to the formula Measure the shrinkage S of the ceramic core before and after sintering L , where L0 is the length before sintering (mm) and L1 is the length after sintering (mm).

[0032] The mass of the ceramic core before and after dissolution was measured by weighing, and the mass loss rate of the ceramic core after dissolution was calculated. The specific steps were as follows: weigh the weight of the sample before immersion, m1, soak it in 80℃ water for 3h, ultrasonically clean it for 3min, then wash away the small particles on the surface, dry it in a 120℃ oven for 5h, weigh the remaining sample mass m2, and calculate the mass loss rate according to the formula Calculate the mass loss rate W of the ceramic core.

[0033] Example 1

[0034] (1) Weigh fused corundum powder, potassium sulfate, sodium lauryl sulfate, paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid according to the following weight parts, wherein the fused corundum powder is 70 weight parts, potassium sulfate is 30 weight parts, sodium lauryl sulfate is 1 weight part, plasticizer is 13 weight parts, and graphite powder is 1 weight part; the plasticizer includes 90 weight parts of paraffin, 4 weight parts of beeswax, 4 weight parts of polyethylene, 1 weight part of stearic acid and 2 weight parts of oleic acid;

[0035] (2) placing the weighed fused corundum powder, potassium sulfate and sodium dodecyl sulfate in an oven and drying them at 110° C. for 1 h, placing the dried mixture into a ball mill of a planetary ball mill, and ball milling them at a speed of 250 r / min for 1.5 h to obtain a mixed ceramic powder;

[0036] (3) Paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid are added to a stainless steel stirring tank in sequence at a mixing temperature of 70°C. After the plasticizer and lubricant are evenly mixed, the mixed ceramic powder is added in batches at a stirrer speed of 200 r / min. After all the mixed ceramic powder is added, the mixture is stirred continuously for 10 hours to obtain a slurry with a certain fluidity;

[0037] (4) Preheating the mold in a blast oven at 40°C for 1 h, pressing the slurry into the mold with a wax injection machine, and preparing the ceramic core by hot die casting. The holding pressure hot die casting process parameters are: the temperature of the wax injection machine is 70°C, the hot die casting pressure is 0.2 MPa, and the holding pressure time is 6 s. After the slurry solidifies, the mold is opened to take out the green blank;

[0038] (5) The obtained green body was placed in a box furnace and sintered according to the set program: the temperature was slowly raised to 100°C at a rate of 1°C / min in an air atmosphere, kept at that temperature for 1 h, then slowly raised to 200°C at a rate of 1°C / min, kept at that temperature for 1 h, then slowly raised to 400°C at a rate of 1°C / min, kept at that temperature for 2 h to remove the organic volatiles in the green body, then raised to 600°C at a rate of 4°C / min, kept at that temperature for 0.5 h, and then raised to 800°C at a rate of 4°C / min, kept at that temperature for 1 h. The temperature was raised to 1050°C at a rate of 4°C / min and kept at this temperature for 1.0h to obtain a hot-die-cast water-soluble ceramic core. The flexural strength was measured by a microcomputer-controlled electronic universal testing machine, and the flexural strength was 4.01MPa. The shrinkage of the hot-die-cast ceramic core was -1.34%. The mass of the die-cast water-soluble ceramic core before and after dissolution was measured by weighing, and the mass loss rate of the dissolution of the die-cast water-soluble ceramic core was calculated. The die-cast water-soluble ceramic core was completely collapsed after being dissolved in a water bath at 80°C for 6h.

[0039] Example 2

[0040] The effect of potassium sulfate addition on the performance of hot die casting ceramic core was studied. The specific preparation process was the same as in Example 1, and the other weight parts remained unchanged. The potassium sulfate was 30 weight parts, 23.3 weight parts, 17.5 weight parts, 12.3 weight parts and 7.7 weight parts respectively. The flexural strength of the hot die casting ceramic core was as follows: Figure 2 As shown, the shrinkage rate is Figure 3 As shown in the figure, the mass loss rate of dissolution in a water bath at 80℃ for 6h is as follows Figure 4 shown.

[0041] Figure 2 is the relationship between the bending strength of the ceramic core and the amount of potassium sulfate added, Figure 2 It can be seen that with the increase of potassium sulfate addition, the bending strength of the ceramic core continues to decrease; it can be adjusted according to actual needs.

[0042] Figure 3 is the relationship between the shrinkage of the ceramic core and the amount of potassium sulfate added, Figure 3 It can be seen that with the increase of potassium sulfate addition, the shrinkage of the ceramic core continues to decrease;

[0043] Figure 4 is the relationship between the mass loss rate of the ceramic core after dissolution and the amount of potassium sulfate added, Figure 4It can be seen that with the increase of potassium sulfate addition, the mass loss rate of the ceramic core after dissolution continues to increase.

[0044] Example 3

[0045] (1) Weigh fused corundum powder, potassium sulfate, sodium lauryl sulfate, paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid according to the following weight parts, wherein the fused corundum powder is 80 weight parts, potassium sulfate is 20 weight parts, sodium lauryl sulfate is 2 weight parts, plasticizer is 12 weight parts, and graphite powder is 1 weight part; the plasticizer includes 90 weight parts of paraffin, 2 weight parts of beeswax, 2 weight parts of polyethylene, 2 weight parts of stearic acid and 1 weight part of oleic acid;

[0046] (2) placing the weighed fused corundum powder, potassium sulfate and sodium dodecyl sulfate in an oven and drying them at 120° C. for 1 h, placing the dried mixture into a ball mill of a planetary ball mill, and ball milling them at a speed of 300 r / min for 2 h to obtain a mixed ceramic powder;

[0047] (3) Paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid are added to a stainless steel stirring tank in sequence at a mixing temperature of 70°C. After the plasticizer and lubricant are evenly mixed, the mixed ceramic powder is added in batches at a stirrer speed of 250 r / min. After all the mixed ceramic powder is added, the mixture is stirred continuously for 10 hours to obtain a slurry with a certain fluidity;

[0048] (4) Preheating the mold in a blast oven at 50° C. for 1 h, pressing the slurry into the mold with a wax injection machine, and preparing the ceramic core by hot die casting. The holding pressure hot die casting process parameters are: the temperature of the wax injection machine is 70° C., the hot die casting pressure is 0.4 MPa, and the holding pressure time is 7 s. After the slurry solidifies, the mold is opened to take out the green blank;

[0049] (5) The obtained green body is placed in a box furnace, and the specific sintering procedure is as follows: the final sintering temperature is 1000°C, the holding time is 1h, and the other heating procedures are the same as in Example 1, to obtain a die-cast water-soluble ceramic core. The bending strength is measured by a microcomputer-controlled electronic universal testing machine, and the bending strength is 7.42MPa. The shrinkage rate of the hot die-cast ceramic core is -1.44%. The mass of the die-cast water-soluble ceramic core before and after dissolution is measured by weighing, and the mass loss rate of the die-cast water-soluble ceramic core is calculated. The mass loss rate of the die-cast water-soluble ceramic core is 59.93% after dissolution in a water bath at 80°C for 6h.

[0050] Example 4

[0051] (1) Weigh fused corundum powder, potassium sulfate, sodium lauryl sulfate, paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid according to the following weight parts, wherein the fused corundum powder is 60 weight parts, potassium sulfate is 20 weight parts, sodium lauryl sulfate is 1 weight part, plasticizer is 14 weight parts, and graphite powder is 1 weight part; the plasticizer includes 95 weight parts of paraffin, 4 weight parts of beeswax, 2 weight parts of polyethylene, 1 weight part of stearic acid and 2 weight parts of oleic acid.

[0052] (2) placing the weighed fused corundum powder, potassium sulfate and sodium dodecyl sulfate in an oven and drying them at 120° C. for 3 h, placing the dried mixture into a ball mill of a planetary ball mill, and ball milling them at a speed of 350 r / min for 1.5 h to obtain a mixed ceramic powder;

[0053] (3) Paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid are added to a stainless steel stirring tank in sequence at a mixing temperature of 80°C. After the plasticizer and lubricant are evenly mixed, the mixed ceramic powder is added in batches at a stirrer speed of 300 r / min. After all the mixed ceramic powder is added, the mixture is stirred continuously for 12 hours to obtain a slurry with a certain fluidity;

[0054] (4) Preheating the mold in a blast oven at 45°C for 1 h, pressing the slurry into the mold with a wax injection machine, and preparing the ceramic core by hot die casting. The holding pressure hot die casting process parameters are: wax injection machine temperature of 80°C, hot die casting pressure of 0.2 MPa, holding pressure time of 7 s, and opening the mold to take out the green blank after the slurry solidifies;

[0055] (5) The obtained green body is placed in a box furnace, and the specific sintering procedure is as follows: the final sintering temperature is 1100°C, the holding time is 1h, and the other heating procedures are the same as in Example 1, to obtain a die-cast water-soluble ceramic core. The bending strength is measured by a microcomputer-controlled electronic universal testing machine, and the bending strength is 5.01MPa. The shrinkage rate of the hot die-cast ceramic core is -0.64%. The mass of the die-cast water-soluble ceramic core before and after dissolution is measured by weighing, and the mass loss rate of the die-cast water-soluble ceramic core is calculated. The mass loss rate of the die-cast water-soluble ceramic core is 31.78% after dissolution in a water bath at 80°C for 6h.

[0056] Example 5

[0057] (1) Weigh fused corundum powder, potassium sulfate, sodium lauryl sulfate, paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid according to the following weight parts, wherein the fused corundum powder is 60 weight parts, potassium sulfate is 10 weight parts, sodium lauryl sulfate is 1 weight part, plasticizer is 12 weight parts, and graphite powder is 1 weight part; the plasticizer includes 90 weight parts of paraffin, 4 weight parts of beeswax, 2 weight parts of polyethylene, 1 weight part of stearic acid and 2 weight parts of oleic acid;

[0058] (2) placing the weighed fused corundum powder, potassium sulfate and sodium dodecyl sulfate in an oven and drying them at 120° C. for 1 h, placing the dried mixture into a ball mill of a planetary ball mill, and ball milling them at a speed of 300 r / min for 2 h to obtain a mixed ceramic powder;

[0059] (3) Paraffin, beeswax, polyethylene, stearic acid, graphite powder and oleic acid are added to a stainless steel stirring tank in sequence at a mixing temperature of 70°C. After the plasticizer and lubricant are evenly mixed, the mixed ceramic powder is added in batches at a stirrer speed of 250 r / min. After all the mixed ceramic powder is added, the mixture is stirred continuously for 10 hours to obtain a slurry with a certain fluidity;

[0060] (4) Preheating the mold in a blast oven at 50° C. for 1 h, pressing the slurry into the mold with a wax injection machine, and preparing the ceramic core by hot die casting. The holding pressure hot die casting process parameters are: the temperature of the wax injection machine is 70° C., the hot die casting pressure is 0.4 MPa, and the holding pressure time is 7 s. After the slurry solidifies, the mold is opened and the green blank is taken out;

[0061] (5) The obtained green body is placed in a box furnace, and the specific sintering procedure is as follows: the final sintering temperature is 1000°C, the holding time is 1h, and the other heating procedures are the same as in Example 1, to obtain a die-cast water-soluble ceramic core. The bending strength is measured by a microcomputer-controlled electronic universal testing machine, and the bending strength is 10.29MPa. The shrinkage rate of the hot die-cast ceramic core is -1.68%. The mass of the die-cast water-soluble ceramic core before and after dissolution is measured by weighing, and the mass loss rate of the die-cast water-soluble ceramic core is calculated. The mass loss rate of the die-cast water-soluble ceramic core is 31.23% after dissolution in a water bath at 80°C for 6h.

[0062] Comparative Example 1

[0063] The influence of the type of binder on the performance of the ceramic core was compared. The specific process was the same as in Example 1, except that the binder was sodium carbonate, and the bending strength of the obtained ceramic core was 5.01 MPa. The mass loss rate of the ceramic core was 20% after 6 hours in a water bath at 80°C. Compared with the ceramic core in Example 1 that was dissolved in a water bath at 80°C for 6 hours and completely collapsed, the ceramic core with potassium sulfate as the binder had better water-soluble disintegration performance.

[0064] Comparative Example 2

[0065] The influence of refractory aggregate on the performance of ceramic core was studied. The specific process was the same as in Example 1, except that the refractory aggregate was mullite powder. The bending strength of the obtained ceramic core was 12.43 MPa, and the mass loss rate of the ceramic core was 10% after 6 hours in a water bath at 80°C. Compared with the ceramic core in Example 1 that was dissolved in a water bath at 80°C for 6 hours and completely collapsed, the ceramic core with fused corundum powder as the refractory aggregate had better water-soluble collapse performance.

[0066] Comparative Example 3

[0067] The effect of sintering temperature on the performance of the ceramic core was studied. The specific process was the same as in Example 1, except that the final sintering temperature of the ceramic core was 1200°C, and the bending strength of the ceramic core was 1.53 MPa. The mass loss rate of the ceramic core was 20.23% after sintering in an 80°C water bath for 6 hours. With the increase of sintering temperature, the burnout amount of potassium sulfate in the core increased during the sintering process, and the strength and mass loss of the core decreased.

Claims

1. A hot die casting water-soluble ceramic core for light alloy investment casting, characterized in that: The hot die casting water-soluble ceramic core comprises fused corundum powder, potassium sulfate, a plasticizer, a lubricant and a surfactant, and the weight ratio thereof is 60-80:7.7-30:10-15:1-2:1-2; the plasticizer comprises paraffin, beeswax, polyethylene, stearic acid and oleic acid, and the weight ratio thereof is 90-95:2-4:2-4:1-2:1-2; the lubricant is graphite powder or glycerol; and the surfactant is sodium lauryl sulfate or stearamide; The method for preparing a hot die casting water-soluble ceramic core for light alloy investment casting comprises the following steps: (1) Mixing fused corundum powder, potassium sulfate and surfactant, drying at 110-120 °C for 1-3 h, and ball milling at 250-350 r / min for 1.5-2 h to obtain a mixed ceramic powder; (2) Stir and mix the plasticizer and lubricant, and add the mixed ceramic powder in batches at 70-80 °C and 200-300 r / min, and continue stirring for 10-12 hours to obtain a slurry with a certain fluidity; (3) Preheat the mold to 40-50 °C, press the slurry into the mold, open the mold after the slurry solidifies, and obtain the green body. The hot die casting process parameters are: slurry temperature is 70-80 °C, pressure is 0.2-0.4 MPa, and holding time is 6-8 s; (4) Sintering the green body to obtain a hot die-cast water-soluble ceramic core. The sintering procedure includes slowly raising the temperature to 400 °C at a rate of 1 °C / min in an air atmosphere, keeping the temperature for 2 h, and then raising the temperature to 1000-1100 °C at a rate of 4 °C / min, and keeping the temperature for 0.5-1.0 h.

2. The method for preparing the hot die casting water-soluble ceramic core for light alloy investment casting according to claim 1, characterized in that: The following steps are involved: (1) Mixing fused corundum powder, potassium sulfate and surfactant, drying at 110-120 °C for 1-3 h, and ball milling at 250-350 r / min for 1.5-2 h to obtain a mixed ceramic powder; (2) Stir and mix the plasticizer and lubricant, and add the mixed ceramic powder in batches at 70-80 °C and 200-300 r / min, and continue stirring for 10-12 hours to obtain a slurry with a certain fluidity; (3) Preheat the mold to 40-50 °C, press the slurry into the mold, open the mold after the slurry solidifies, and obtain the green body. The hot die casting process parameters are: slurry temperature is 70-80 °C, pressure is 0.2-0.4 MPa, and holding time is 6-8 s; (4) Sintering the green body to obtain a hot die-cast water-soluble ceramic core. The sintering procedure includes slowly raising the temperature to 400 °C at a rate of 1 °C / min in an air atmosphere, keeping the temperature for 2 h, and then raising the temperature to 1000-1100 °C at a rate of 4 °C / min, and keeping the temperature for 0.5-1.0 h.

Citation Information

Patent Citations