A TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material and its preparation method and application

By fixing TiO2 nanosheets inside the hydrophobic zeolite to form a core-shell hierarchical structure, the problem of existing TiO2 photocatalysts in degraded VOCs is solved, and high efficiency is achieved , stable toluene removal and long-term use reduce the cost of the air purification system.

CN114887651BActive Publication Date: 2024-11-19ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210544303.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-19
Publication Date
2024-11-19
Estimated Expiration
2042-05-19

AI Technical Summary

Technical Problem

Existing TiO2 photocatalysts are prone to inactivation during the degradation of volatile organic compounds (VOCs), resulting in low photocatalytic efficiency and short life, increasing the cost of air purification systems.

Method used

Using TiO2 nanosheets @ hydrophobic zeolite composite microsphere photocatalytic material, the core-shell hierarchical structure is formed by fixing TiO2 nanosheets inside hydrophobic zeolite nanoparticles, and the selective adsorption and enrichment of VOCs are used to prevent catalyst deactivation. and improve catalytic efficiency.

Benefits of technology

The removal rate of efficient toluene removal is greater than 95%, and the stability and life of the catalyst is significantly improved, reducing costs, and is suitable for long-term applications in the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114887651B_ABST
    Figure CN114887651B_ABST
Patent Text Reader

Abstract

The present invention discloses a TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material and a preparation method and application thereof. The photocatalytic material is based on a zeolite sheath synthesized by functionalizing an organic group on a faujasite zeolite skeleton during a crystallization process, and a titanium dioxide nanosheet prepared by a hydrothermal method is fixed inside the hydrophobic zeolite to obtain a titanium dioxide nanosheet@hydrophobic zeolite composite photocatalytic material. The photocatalytic material of the present invention has a core-shell hierarchical structure, a large specific surface area, the thickness and size of TiO2 can be regulated by synthetic conditions, the preparation process is simple and easy, the cost is low, and the yield is high. The core-shell structure anatase titanium dioxide zeolite assembled by the nanosheet has great application potential in the field of photocatalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalytic materials, and in particular to a TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material and a preparation method and application thereof. Background Art

[0002] With the rapid development of industry, volatile organic compounds (VOCs) have become one of the main air pollutants in urban areas of developing countries, with significant impacts on human health and atmospheric chemistry. Anthropogenic emission sources include chemical and petrochemical industries, automobile exhaust, gas stations, in-vehicle fuel delivery, etc. Toluene is a common and typical VOC that has been recognized as a strong carcinogen. VOCs can be treated by destructive methods (incineration, biofiltration and catalytic oxidation) and non-destructive methods (absorption, adsorption, condensation and membrane filtration) processes. In particular, photocatalytic oxidation is an attractive technology for the removal of air pollutants and has attracted great interest from the perspectives of materials science, physical chemistry and environmental engineering.

[0003] Photocatalyst is one of the key components in air purification technology for photocatalytic degradation of VOCs. So far, TiO2 has been widely used as an environmental photocatalyst due to its chemical stability and strong photooxidation ability. Under ultraviolet light, the photocatalyst can generate electrons and holes, which are further converted into hydroxyl radicals ( • OH), superoxide anion (O2 •- ) or other active substances that can oxidize VOCs into inorganic small molecules. However, the deactivation of TiO2 leads to low photocatalytic efficiency and shortened photocatalytic life, which will reduce the commercial value of photocatalysis as a practical air purification technology. From an economic point of view, the short life of the catalyst will lead to frequent replacement of the catalyst, thereby increasing the costs associated with the system.

[0004] In order to prevent the deactivation of photocatalysts during the long-term degradation of VOCs and improve the photocatalytic efficiency, the formation of stubborn intermediates or their accumulation on the surface should be highly prevented. Therefore, many strategies have been developed to prevent the deactivation of photocatalysts, including the formation of heterojunctions with other semiconductors, surface modification, and the synthesis of new photocatalytic materials. We chose to fix metal oxides in hydrophobic zeolites to achieve ideal wetting selectivity, selectively capture and enrich toluene in the micropores of hydrophobic zeolites, and then photodegrade them on titanium dioxide to achieve the purpose of anti-deactivation and improve efficiency. Summary of the invention

[0005] In view of the above-mentioned technical problems existing in the prior art, the object of the present invention is to provide a TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material and its preparation method and application. The present invention uses zeolite, a safe material that is pollution-free to the environment, and titanium dioxide to composite as a photocatalyst. In the process of photocatalytic degradation of organic pollutants, the deactivation of the catalyst in the degradation process is hindered, and the material is easy to recycle and is more conducive to application in the environment.

[0006] The technical solution adopted by the present invention is:

[0007] A TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material, which is a porous microsphere photocatalyst formed by a composite of TiO2 nanosheets and hydrophobic zeolite nanoparticles, and has a core-shell hierarchical structure, in which the TiO2 nanosheets are fixed inside the hydrophobic zeolite nanoparticles; wherein the mass percentage of TiO2 in the TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material is 43.5~85.5wt%.

[0008] Furthermore, the length of the TiO2 nanosheets is 40-60 nm and the thickness is 10-20 nm; and the average diameter of the photocatalytic material is 2.5-12 μm.

[0009] Furthermore, the TiO2 nanosheets are in anatase phase with (001) and (101) crystal planes exposed on the surface.

[0010] The method for preparing the TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material comprises the following steps:

[0011] 1) Disperse TiO2 nanosheets in a mixture of ammonia water, deionized water and ethanol with a mass fraction of 25-28%, stir well, add silicon source, and stir at room temperature for 5-10 hours; then remove water and ethanol by vacuum heating, dry at 90-110°C for 6-10 hours to obtain a composite of amorphous silicon and titanium dioxide; wherein the feed ratio of TiO2 nanosheets, ammonia water, deionized water, ethanol and silicon source is 0.5-4g:8-10mL:100-200mL:100-150mL:5-7g;

[0012] 2) Mixing the complex obtained in step 1) with sodium aluminate, sodium hydroxide and deionized water, stirring at room temperature for 10-15 hours to form a gel, transferring the gel to a stainless steel autoclave, heating and reacting at 90-120° C. for 20-30 hours, filtering, washing and drying after the reaction, and finally obtaining a TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material; wherein the feed ratio of the silicon source in step 1) to the sodium aluminate, sodium hydroxide and deionized water in step 2) is 5-7g: 0.6-0.7g: 0.9-1.0g: 8-10g.

[0013] Furthermore, in step 1), the silicon source is tetraethyl orthosilicate and dimethoxydiethoxysilane, and the feed mass ratio of tetraethyl orthosilicate to dimethoxydiethoxysilane is 6-10:1, preferably 8:1.

[0014] Furthermore, TiO2 nanosheets are synthesized by a hydrothermal method, which specifically includes the following steps: adding a morphology control agent to a titanium source, stirring at room temperature for 20 to 40 minutes for hydrolysis, then transferring to an autoclave with a polytetrafluoroethylene liner, continuing the hydrothermal reaction at 160 to 200°C for 20 to 30 hours, centrifuging, washing, drying, and grinding to finally obtain TiO2 nanosheet products.

[0015] Furthermore, the titanium source is tetrabutyl titanate, the morphology control agent is an aqueous solution of hydrofluoric acid with a mass fraction of 20-30%, and the volume ratio of the aqueous solution of tetrabutyl titanate to hydrofluoric acid is 6-10:1, preferably 8-8.5:1.

[0016] The invention discloses an application of a TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material in photocatalytic degradation of organic pollutants.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1) In the TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalytic material provided by the present invention, the TiO2 nanosheet is loaded on the zeolite, and the (001) crystal face of the TiO2 nanosheet with a high proportion of exposure is beneficial to the dissociation of H2O to produce hydroxyl groups, thereby improving the reaction activity and the catalytic efficiency. The removal efficiency of toluene under ultraviolet light source is greater than 95%.

[0019] 2) The hydrophobic Y-type zeolite has an adsorption enhancement effect on the target pollutants and avoids competitive adsorption of water, and makes the overall composite structure extremely stable and will not be deactivated during long-term use.

[0020] 3) The TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalyst obtained by the present invention has good physical stability, is non-volatile, insoluble, has high heat resistance, and is non-toxic; when rinsed with deionized water, no titanium dioxide peeling is observed.

[0021] 4) The present invention uses Y-type zeolite as a carrier, and the raw material resources are abundant, the price is low, the preparation process is simple, and the output is large. In terms of environmental protection, it can be used to eliminate air pollution, treat sewage, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope (SEM) image of TiO2@Y-0.5 prepared in Example 1;

[0023] Figure 2This is the transmission electron microscope (TEM) image of TiO2@Y-0.5 prepared in Example 1.

[0024] Figure 3 This is the water contact angle diagram of TiO2@Y-0.5 prepared in Example 1.

[0025] Figure 4 This is the X-ray diffraction (XRD) pattern of TiO2@Y-0.5 prepared in Example 1.

[0026] Figure 5 This is the SEM image of TiO2 prepared in Comparative Example 1.

[0027] Figure 6 This is the SEM image of Y zeolite prepared in Comparative Example 2.

[0028] Figure 7 The degradation performance of the composite photocatalytic materials prepared in Examples 1, 2, 3, and 4, and TiO2 and P25 prepared in Comparative Example 1 on toluene under ultraviolet light.

[0029] FIG8 is a performance diagram of the TiO2 prepared in Example 3 and Comparative Example 1 for degrading toluene after continuous use for 5 times under ultraviolet light. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0031] Example 1

[0032] Preparation of TiO2 nanosheets: Synthesized by hydrothermal method, 6 mL of hydrofluoric acid solution (mass fraction 25%, the same as in the following examples) was added to 50 mL of tetrabutyl titanate at room temperature and stirred for 30 minutes for reaction and hydrolysis. Then transferred to a 200 mL autoclave with a white polytetrafluoroethylene liner and hydrothermally maintained at 180°C for 24 hours. Subsequently, the white precipitate was collected by centrifugation, washed with ethanol and distilled water, and finally transferred to a 60°C oven until dried and ground. The resulting sample was represented by F-TiO2.

[0033] Synthesis of TiO2@hydrophobic Y zeolite: 0.5 g of the titanium dioxide nanosheets prepared above were dispersed in a mixture of ammonia water (mass fraction 25%, 9 mL), water (150 mL) and ethanol (120 mL). After stirring for 0.5 h, 5.31 g of tetraethyl orthosilicate and 0.66 g of dimethoxydiethoxysilane were added and stirred for another 8 h. Water and ethanol were removed by heating under vacuum, and after drying at 100 ° C for 8 h, a composite material of amorphous silica and titanium dioxide was obtained, which was then mixed with sodium aluminate (0.624 g), sodium hydroxide (0.954 g) and water (9 g). After stirring at room temperature for 12 h, the gel was transferred to a polytetrafluoroethylene-calcified stainless steel autoclave and heated at 100 ° C for 24 h. After filtration, it was washed with a large amount of water and dried at 100°C for 12 h, and finally a hydrophobic Y zeolite-fixed titanium dioxide sample was obtained, which was recorded as TiO2@Y-0.5, and the mass proportion of TiO2 was 43.5%.

[0034] The TiO2@Y-0.5 sample obtained in Example 1 was characterized by SEM. Figure 1 . Figure 1 The results show that the prepared TiO2@Y-0.5 has a spherical structure with an average particle size of about 10 μm. Further observation shows that the microsphere is composed of countless stacked flaky particles.

[0035] The TiO2@Y-0.5 sample obtained in Example 1 was characterized by TEM. Figure 2 . Figure 2 The results show that the morphology of the prepared TiO2@Y-0.5 is spherical, and the microspheres are composed of TiO2 nanosheets and Y zeolite microspheres, which is consistent with the SEM results. Furthermore, the length of the TiO2 nanosheets is 40-60 nm, the thickness is 10-20 nm, and the interplanar spacing is 0.235 nm and 0.35 nm, respectively, corresponding to the (001) and (101) planes of anatase titanium dioxide.

[0036] The TiO2@Y-0.5 sample obtained in Example 1 was tested for water contact angle. Figure 3 . Figure 3 The water contact angle of TiO2@Y-0.5 is 110.1 o , the surface is hydrophobic.

[0037] The TiO2@Y-0.5 sample obtained in Example 1 was subjected to XRD test, and the results are shown in Figure 4 . Figure 4 The prepared TiO2@Y-0.5 contains obvious diffraction peaks of TiO2 and Y zeolite, indicating that the catalyst is composed of TiO2 and Y zeolite.

[0038] Example 2

[0039] The preparation process of TiO2 nanosheets was repeated in Example 1.

[0040] Synthesis of TiO2@hydrophobic Y zeolite: 1 g of the titanium dioxide nanosheets prepared above was dispersed in a mixture of ammonia water (mass fraction 25%, 9 mL), water (150 mL) and ethanol (120 mL). After stirring for 0.5 h, 5.31 g of tetraethyl orthosilicate and 0.66 g of dimethoxydiethoxysilane were added and stirred for another 8 h. Water and ethanol were removed by heating under vacuum, and after drying at 100 ° C for 8 h, a composite material of amorphous silica and titanium dioxide was obtained, which was then mixed with sodium aluminate (0.624 g), sodium hydroxide (0.954 g) and water (9 g). After stirring at room temperature for 12 h, the gel was transferred to a polytetrafluoroethylene-calcified stainless steel autoclave and heated at 100 ° C for 24 h. After filtration, it was washed with a large amount of water and dried at 100°C for 12 h. Finally, a hydrophobic Y zeolite-fixed titanium dioxide sample was obtained, which was recorded as TiO2@Y-1, and the mass proportion of TiO2 was 65.1%.

[0041] Example 3

[0042] The preparation process of TiO2 nanosheets was repeated in Example 1.

[0043] Synthesis of TiO2@hydrophobic Y zeolite: 2 g of the prepared titanium dioxide nanosheets were dispersed in a mixture of ammonia water (mass fraction 25%, 9 mL), water (150 mL) and ethanol (120 mL). After stirring for 0.5 h, 5.31 g of tetraethyl orthosilicate and 0.66 g of dimethoxydiethoxysilane were added and stirred for another 8 h. Water and ethanol were removed by heating under vacuum, and after drying at 100 ° C for 8 h, a composite material of amorphous silica and titanium dioxide was obtained, which was then mixed with sodium aluminate (0.624 g), sodium hydroxide (0.954 g) and water (9 g). After stirring at room temperature for 12 h, the gel was transferred to a polytetrafluoroethylene-calcified stainless steel autoclave and heated at 100 ° C for 24 h. After filtration, it was washed with a large amount of water and dried at 100°C for 12 h, and finally a hydrophobic Y zeolite-fixed titanium dioxide sample was obtained, which was recorded as TiO2@Y-2, and the mass proportion of TiO2 was 72.7%.

[0044] Example 4

[0045] The preparation process of TiO2 nanosheets was repeated in Example 1.

[0046] Synthesis of TiO2@hydrophobic Y zeolite: 4 g of the titanium dioxide nanosheets prepared above were dispersed in a mixture of ammonia water (mass fraction 25%, 9 mL), water (150 mL) and ethanol (120 mL). After stirring for 0.5 h, 5.31 g of tetraethyl orthosilicate and 0.66 g of dimethoxydiethoxysilane were added and stirred for another 8 h. Water and ethanol were removed by heating under vacuum, and after drying at 100 ° C for 8 h, a composite material of amorphous silica and titanium dioxide was obtained, which was then mixed with sodium aluminate (0.624 g), sodium hydroxide (0.954 g) and water (9 g). After stirring at room temperature for 12 h, the gel was transferred to a polytetrafluoroethylene-calcified stainless steel autoclave and heated at 100 ° C for 24 h. After filtration, it was washed with a large amount of water and dried at 100°C for 12 h, and finally a hydrophobic Y zeolite-fixed titanium dioxide sample was obtained, which was recorded as TiO2@Y-4, and the mass proportion of TiO2 was 85.5%.

[0047] Comparative Example 1

[0048] Synthesis of TiO2 nanosheets: The preparation process of TiO2 nanosheets was repeated in Example 1.

[0049] The TiO2 nanosheet sample obtained in Comparative Example 1 was characterized by SEM. Figure 5 . Figure 5 The results show that the nanosheets present decahedral blocks with a high proportion of (001) crystal planes exposed.

[0050] Comparative Example 2

[0051] Synthesis of hydrophobic Y zeolite: After stirring a mixture of ammonia (mass fraction 25%, 9 mL), water (150 mL) and ethanol (120 mL) for 0.5 h, 5.31 g of tetraethyl orthosilicate and 0.66 g of dimethoxydiethoxysilane were added and stirred for another 8 h. After heating under vacuum to remove water and ethanol, the amorphous silica material was obtained after drying at 100 ° C for 8 h, and then mixed with sodium aluminate (0.624 g), sodium hydroxide (0.954 g) and water (9 g). After stirring at room temperature for 12 h, the gel was transferred to a polytetrafluoroethylene-calcified stainless steel autoclave and heated at 100 ° C for 24 h. After filtration, it was washed with a large amount of water and dried at 100 ° C for 12 h to finally obtain hydrophobic Y zeolite.

[0052] The hydrophobic Y zeolite sample obtained in Example 2 was characterized by SEM. Figure 6 . Figure 6 It shows that zeolite is a scaly irregular sphere with small holes in some parts of the particle surface. These blocky scales and small holes not only facilitate the catalyst to adsorb pollutants, but also enhance the catalyst's ability to selectively adsorb pollutants.

[0053] Comparative Example 3

[0054] The catalytic performance of the conventional commercial titanium dioxide Degussa P25 commercial photocatalyst (P25 for short) and the photocatalyst prepared by the present invention was compared. The P25 was purchased from Guangzhou Heqian Trading Co., Ltd., Germany Degussa brand, with an average particle size of 25 nm.

[0055] Application Example 1:

[0056] The performance of the TiO2 nanosheets@hydrophobic zeolite composite microsphere photocatalysts prepared in Examples 1 to 4 and the TiO2 nanosheets prepared in Comparative Example 1 in photocatalytic degradation of toluene was studied, and the specific steps were as follows:

[0057] First, take 0.1g of the catalyst sample and spread it evenly on a round quartz glass dish with a diameter of 4cm with ethanol and dry it. Then fix the round quartz glass dish containing the catalyst on a tray rack, and fix the tray rack in the middle of the dried reactor. Set a stirrer at the bottom of the reactor (the function of the stirrer is to make the gas in the reactor flow through rotation, and the gas is evenly dispersed in the reactor). Seal the reactor. The volume of the reactor is about 270cm 3 . 1ul of toluene and 3ul of water were injected into the reactor, and then placed in an oven for 30 minutes to allow the toluene and water to completely vaporize to form a gaseous environment. The toluene-water was in contact with the catalyst in the form of gas. Then the reactor was taken out and first placed in a water bath at 25°C to simulate a normal temperature environment for 30 minutes, which was recorded as the initial time. The mercury lamp was turned on to carry out a catalytic reaction under ultraviolet light irradiation for 2 hours (the irradiation power of the mercury lamp was 300W and the light intensity was 450uw / cm 2 ), sampling was performed regularly and VOC detection was performed using an Agilent gas chromatograph.

[0058] Figure 7The degradation performance diagram of toluene under ultraviolet light for the composite photocatalytic materials prepared in Examples 1, 2, 3, and 4 and the TiO2 and P25 catalysts prepared in Comparative Example 1. When the hydrophobic Y zeolite is not compounded, the removal rate of toluene in Comparative Example 1 is 94.6% in 45 min; when compounded with the hydrophobic Y zeolite, the removal rate of toluene by the TiO2@Y-0.5 photocatalyst of Example 1 is 37.8% in 120 min; the removal rate of toluene by the TiO2@Y-1 photocatalyst of Example 2 is 92.7% in 120 min; the removal rate of toluene by the TiO2@Y-2 photocatalyst of Example 3 is 97.0% in 120 min; the removal rate of toluene by the TiO2@Y-4 photocatalyst of Example 4 is 56.3% in 120 min. The removal effect of TiO2@Yx on toluene is affected by the degree of encapsulation, and the order of its photocatalytic removal efficiency on toluene is:

[001] TIO2> P25> TiO2@Y-2> TiO2@Y-1>> TiO2@Y-0.5. By comparing with the conventional commercial photocatalyst P25 in Comparative Example 3, it can be seen that the photocatalytic degradation performance of the TiO2@Y-2 catalyst prepared in Example 3 on toluene is not better than that of P25 in a short reaction time, but because P25 is quickly poisoned (p25 is an ordinary mixed crystal TiO2, its catalytic degradation effect is relatively similar to that of the pure TiO2 in Comparative Example 1, from this point of view Figure 7 It can also be seen in the figure. Figure 8a It has been proved that the rapid deactivation occurs in the samples prepared by the present invention. The actual mineralization rate of the samples prepared by the present invention is higher and the oxidation effect is better, indicating that the TiO2 nanosheet@hydrophobic zeolite composite microsphere photocatalyst of the present invention has very good application prospects.

[0059] The present invention first prepares titanium dioxide nanosheets by a hydrothermal method, and then fixes the titanium dioxide nanosheets inside the hydrophobic zeolite in the process of preparing hydrophobic zeolite nanoparticles to obtain a catalyst with a core-shell hierarchical structure, which has good catalytic activity and high stability after experimental verification. Compared with the conventional preparation method of the existing catalyst, it has a better catalytic effect. For example, the document Efficient removal of toluene and benzene in gas phase by the TiO2 / Y-zeolite hybrid photocatalyst directly uses USY zeolite as a carrier, impregnates the aqueous solution of ammonium titanyl oxalate, and then converts the ammonium titanyl oxalate into TiO2 to finally form a catalyst. Compared with this, the catalyst of the present invention has a better catalytic effect.

[0060] Application Example 2:

[0061] The stability of the TiO2@Y-2 prepared in Example 3 and the TiO2 nanosheets prepared in Comparative Example 1 in photocatalytic degradation of toluene was studied, and the specific steps were as follows:

[0062] First, take 0.1g of the catalyst sample and spread it evenly on a round quartz glass dish with a diameter of 4cm with ethanol and dry it. Then fix the round quartz glass dish containing the catalyst on a tray rack, and fix the tray rack in the middle of the dried reactor. Set a stirrer at the bottom of the reactor (the function of the stirrer is to make the gas in the reactor flow through rotation, and the gas is evenly dispersed in the reactor). Seal the reactor. The volume of the reactor is about 270cm 3 . 1ul of toluene and 3ul of water were injected into the reactor, and then placed in an oven for 30 minutes to allow the toluene and water to completely vaporize to form a gaseous environment. The toluene-water was in contact with the catalyst in the form of gas. Then the reactor was taken out and first placed in a water bath at 25°C to simulate a normal temperature environment for 30 minutes, which was recorded as the initial time. The mercury lamp was turned on to carry out a catalytic reaction under ultraviolet light irradiation for 2 hours (the irradiation power of the mercury lamp was 300W and the light intensity was 450uw / cm 2 ), sampling was performed regularly and VOC detection was performed using an Agilent gas phase analyzer. The catalyst was reused for five consecutive experiments.

[0063] Figure 8a This is a performance diagram of the TiO2@Y-2 prepared in Example 3 for degrading toluene after being continuously recycled for 5 times under ultraviolet light, and the catalyst TiO2@Y-2 basically does not change color after being recycled for 5 times. Figure 8b This is a performance diagram of the TiO2 prepared in Comparative Example 1 for degrading toluene after being continuously recycled for 5 times under ultraviolet light. The catalyst TiO2 has turned into brown after being recycled once, and the color change is serious.

[0064] As shown in Figure 8, the removal efficiency of toluene by the TiO2@Y-2 photocatalyst prepared in Example 3 did not decrease significantly during the five cycles, while the removal efficiency of toluene by the TiO2 nanosheets prepared in Comparative Example 1 after the third cycle was only 50% of that in the first experiment. This result shows that the TiO2@Y-2 prepared in Example 3 has a high reaction stability, and the presence of the hydrophobic Y zeolite can prevent the deactivation of TiO2 during the reaction.

[0065] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.

Claims

1. A method for preparing a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material, characterized in that The photocatalytic material is a porous microsphere photocatalyst formed by a composite of TiO2 nanosheets and hydrophobic Y zeolite nanoparticles, which has a core-shell hierarchical structure, and the TiO2 nanosheets are fixed inside the hydrophobic Y zeolite nanoparticles; wherein the mass percentage of TiO2 in the TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material is 65.1wt%; The length of the TiO2 nanosheet is 40-60 nm and the thickness is 10-20 nm; the average diameter of the photocatalytic material is 2.5-12 μm, and the TiO2 nanosheet is anatase phase with (001) and (101) crystal planes exposed on the surface; The preparation method comprises the following steps: 1) Disperse TiO2 nanosheets in a mixture of ammonia water, deionized water and ethanol with a mass fraction of 25-28%, stir well, add silicon source, and stir at room temperature for 5-10 hours; then remove water and ethanol by vacuum heating, dry at 90-110°C for 6-10 hours to obtain a composite of amorphous silicon and titanium dioxide; wherein the feed ratio of TiO2 nanosheets, ammonia water, deionized water, ethanol and silicon source is 0.5-4g:8-10mL:100-200mL:100-150mL:5-7g; 2) Mixing the complex obtained in step 1) with sodium aluminate, sodium hydroxide and deionized water, stirring at room temperature for 10-15 hours to form a gel, transferring the gel to a stainless steel autoclave, heating and reacting at 90-120° C. for 20-30 hours, filtering, washing and drying after the reaction, and finally obtaining a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material; wherein the feed ratio of the silicon source in step 1) to the sodium aluminate, sodium hydroxide and deionized water in step 2) is 5-7 g: 0.6-0.7 g: 0.9-1.0 g: 8-10 g; In step 1), the silicon sources are tetraethyl orthosilicate and dimethoxydiethoxysilane, and the feed mass ratio of tetraethyl orthosilicate to dimethoxydiethoxysilane is 6-10:

1.

2. The method for preparing a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material as claimed in claim 1, characterized in that In step 1), the silicon sources are tetraethyl orthosilicate and dimethoxydiethoxysilane, and the mass ratio of tetraethyl orthosilicate to dimethoxydiethoxysilane is 8:

1.

3. The method for preparing a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material as claimed in claim 1, characterized in that TiO2 nanosheets are synthesized by a hydrothermal method, which specifically includes the following steps: adding a morphology control agent to a titanium source, stirring at room temperature for 20 to 40 minutes for hydrolysis, then transferring to an autoclave with a polytetrafluoroethylene liner, continuing the hydrothermal reaction at 160 to 200°C for 20 to 30 hours, centrifuging, washing, drying, and grinding to finally obtain TiO2 nanosheet products.

4. The method for preparing a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material as claimed in claim 3, characterized in that The titanium source is tetrabutyl titanate, the morphology control agent is a hydrofluoric acid aqueous solution with a mass fraction of 20-30%, and the volume ratio of the tetrabutyl titanate to the hydrofluoric acid aqueous solution is 6-10:

1.

5. The method for preparing a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material as claimed in claim 4, characterized in that The volume ratio of tetrabutyl titanate to hydrofluoric acid aqueous solution is 8-8.5:

1.

6. Use of a TiO2 nanosheet@hydrophobic Y zeolite composite microsphere photocatalytic material prepared by the method of claim 1 in photocatalytic degradation of organic pollutants.