Ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall and preparation method thereof

The ant hole-shaped super electrode carbon material prepared by high-temperature activation and high-pressure boiling method solves the problem of degradation of specific capacitance performance when the current density is high in the prior art, and achieves efficient electrochemical performance and rate performance, which is suitable for a variety of Application scenario.

CN114899014BActive Publication Date: 2024-12-03CHANGZHOU UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210384393.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-13
Publication Date
2024-12-03
Estimated Expiration
2042-04-13

AI Technical Summary

Technical Problem

The existing super electrode carbon materials have deteriorated specific capacitance performance when the current density is high, and lacks an optimized structure and easy-to-industrial preparation method, resulting in poor performance in practical applications.

Method used

The method of high-temperature activation combined with high-pressure boiling is used to prepare ant hole-like super electrode carbon material with graphene and microporous structures on the pore wall. Through the mixing, pre-decomposition, activation and high-pressure boiling, etc. of carbon source and phosphorus source, it is formed. Carbon material with special structure.

Benefits of technology

It significantly improves the electrolyte transfer rate and conductivity, improves the electrochemical performance and rate performance, and can maintain a high specific capacitance under high current density. It is suitable for supercapacitors, chemical energy storage batteries and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003594265300000081
    Figure BDA0003594265300000081
  • Figure HDA0003594265310000011
    Figure HDA0003594265310000011
  • Figure HDA0003594265310000012
    Figure HDA0003594265310000012
Patent Text Reader

Abstract

The present invention belongs to the field of electrode materials, and specifically relates to an ant-hole-shaped super electrode carbon material with graphene and microporous structure on the pore wall and a preparation method thereof. The material has a special ant-hole-shaped structure with graphene and microporous structure, and when used as electrode carbon, it can greatly promote the transfer rate of electrolyte inside the electrode and the conductivity of the body, and the walls of the ant-hole are covered with in-situ generated micropores and graphene structures, and its large surface specific surface area can be used to obtain high electrochemical performance. The specific surface area of ​​this carbon material is much lower than that of traditional electrode carbon materials, so the tap density is also higher, but the electrochemical performance is better, with excellent specific capacitance and excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrode materials, and in particular relates to an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall and a preparation method thereof. Background Art

[0002] At present, people generally use carbon materials with porous or multi-level pore structures as electrode materials. On the one hand, it is because the small pores in the carbon electrode material are needed to provide a large specific surface area. On the other hand, in order for the electrolyte solution to better penetrate into the pores to increase the effective surface area of ​​the electrode, the electrode also needs to have a strong surface hydrophilicity and a large and medium pore structure. However, there are many different opinions on the ratio between the multi-level pores, and the actual test data is also very complicated due to factors such as the structure of the carbon material. In fact, with the deepening of theoretical research, the main performance requirements of the electrode for porous carbon are not the ultra-large specific surface, but the effective penetration and distribution of the electrolyte in the electrode carbon and the relatively good conductivity of the carbon matrix. However, due to the affinity of the carbon surface and the surface tension of the electrolyte, it is difficult for the electrolyte to be distributed in some materials with ultra-large specific surfaces and deep pore structures. Therefore, in recent years, people have found that many carbon materials with low specific surface areas have higher specific capacitance than many high specific surface carbon materials. In addition, in order to obtain a higher specific capacitance, existing studies often dope carbon materials with elements such as boron, sulfur, nitrogen, and phosphorus or use polyaniline and other elements for surface modification, and use the pseudocapacitance of the redox reaction of these modified components to increase the capacitance.

[0003] CN113979433A discloses the preparation and application of lignin-based hierarchical porous carbon based on direct carbonization. In the case of introducing a small amount of KOH, the advantages of rich lignin functional groups are used to modify lignin by carboxylation and phenolic hydroxylation, and potassium atoms are grafted to carboxyl groups or phenolic hydroxyl groups. The effect of physical activation assisting chemical activation is achieved. In the absence of any template agent, the template salt KCl or carbonate formed during the pyrolysis carbonization process plays a role of self-template, and a carbon with a carbon content of up to 2500m 2 / g specific surface area and developed pore structure, and has excellent supercapacitor performance porous carbon. Although carbonization only takes one step, it is necessary to carry out grafting synthesis reaction on the precursor. The adsorption and desorption test of the prepared electrode carbon shows that it has a large specific surface but no obvious hysteresis loop, indicating that it is still a general activated carbon structure without macropores and mesoporous structures. This is also the reason why it uses a current density of 0.1A / g to obtain good specific capacitance data, but when the current density is greater than 20A / g, the specific capacitance drops to below 100. In fact, the specific capacitance data tested at such a low current density is meaningless for supercapacitors in practical applications.

[0004] CN114068201A discloses a supercapacitor electrode material prepared from a doped carbon material and a preparation method. Two doped carbon materials are prepared by five steps of first preparing a coordination solution, then doping the solution, adding alkali to dry, calcining and finally acid washing. However, from the actual measured data, it is still a traditional activated carbon structure, especially when the current density reaches 10A / g, the specific capacitance is less than half of that at 0.5A / g, and the rate performance is poor.

[0005] CN114084884A discloses a preparation method and application of a bio-based porous carbon material, which adopts a relatively simple process, and only involves mixing fresh plants with KOH, crushing, drying, grinding, calcining, crushing and washing to obtain the high-capacitance porous carbon material. The measured data shows that the material is still a traditional activated carbon structure material with almost no hysteresis loop, and the specific capacitance is only about 40F / g at a current density of 1A / g, and the electrochemical performance is poor.

[0006] CN113880085A discloses a method for preparing biomass activated carbon for supercapacitors and supercapacitor carbon, wherein the biomass carbonized material is pretreated with a sodium persulfate solution, a binder is added for room temperature granulation, and finally the granulated product is mixed with an activator for carbonization activation treatment, and spherical activated carbon is obtained by post-treatment. The biomass activated carbon prepared by the invention claims to have a high tap density, a good pore structure, and good electrochemical properties, but the measured data is still the traditional activated carbon structure material with almost no hysteresis loop, the main pores are concentrated below 5 nanometers, the specific capacitance is only about 200F / g at a current density of 1A / g, and no rate performance evaluation is performed.

[0007] In general, in the field of super electrode carbon materials, there is currently no method for preparing electrode carbon materials with truly optimized structure, truly easy industrialization and process controllable, and good comprehensive performance. Summary of the invention

[0008] In order to optimize the difficulties in the preparation and application of existing electrode carbon materials, the present invention aims to prepare ant nest-shaped super electrode carbon materials with graphene and microporous structures on the pore walls by a method of high-temperature activation combined with high-pressure water boiling. The prepared carbon material has a special ant nest-shaped structure, which can greatly promote the transfer rate of electrolytes inside the electrode and the conductive properties of the body when used as electrode carbon. The walls of the ant nest are covered with in-situ generated micropores and graphene structures, and their large surface specific area can be used to obtain high electrochemical performance.

[0009] The ant-hole-shaped super-electrode carbon material with graphene and microporous structure on the pore wall provided by the present invention comprises the following components in terms of mass percentage: carbon source: 30-70%, phosphorus source: 30-70%.

[0010] The carbon source is one or more of lignin, wood powder, petroleum coke powder, asphalt, charcoal powder, bamboo powder, polyacrylonitrile and polyphenylene ether.

[0011] The phosphorus source is one or more of phosphoric acid, polyphosphoric acid, ammonium polyphosphate, and ammonium polyphosphate cyanurate.

[0012] The present invention also provides a method for preparing an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall, which adopts a high-temperature activation combined with a high-pressure water boiling method to prepare the super electrode carbon material with graphene and microporous structure on the pore wall. The specific implementation steps are as follows:

[0013] (1) Mix the carbon source and phosphorus source thoroughly in a high-speed mixer, mortar or ball mill;

[0014] (2) Pre-decomposition at 300-400°C for 40-120 minutes in a high temperature furnace protected by nitrogen and oxygen-free environment;

[0015] (3) then continue to heat to 700-900° C. under nitrogen protection for activation for 40-180 minutes, and after cooling, ball-mill into a powdery phosphorus oxide composite carbon material;

[0016] (4) Finally, the prepared phosphorus oxide composite carbon material is subjected to high-pressure boiling in a high-pressure reactor using deionized water as the medium. The high-pressure boiling temperature is 110-200° C. and the boiling time is 8-72 hours. The water is changed every 4-24 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle.

[0017] (5) After boiling in water, the super electrode carbon material with graphene and microporous structure on the pore wall is obtained by filtering.

[0018] Beneficial effects:

[0019] The process for preparing super electrode carbon materials of the present invention is relatively simple, does not require much manual intervention, and is easy to mass produce. The carbon material prepared by the present invention has a special ant hole-like structure, and the walls of the ant holes are covered with in-situ generated micropores and graphene structures. When used as electrode carbon, it can greatly promote the transfer rate of electrolytes inside the electrode and the conductive properties of the body, and can also utilize the large surface area of ​​the micropores and graphene on the ant hole walls to obtain very high electrochemical performance.

[0020] In addition, since the specific surface area of ​​this material is much lower than that of existing electrode carbon materials, its tap density is much higher than that of existing high specific surface electrode carbon materials, and the manufactured device can obtain a higher energy density. In particular, due to the excellent rate performance brought by the ant-hole structure of this material (current density increased by 100 times, specific capacitance can still be maintained at about 70%), it can meet the needs of rapid charging and discharging in various use environments, and can be widely used in the fields of supercapacitor electrodes, chemical energy storage battery electrodes, electrosorption water treatment and electrocatalysis, and carbon-loaded chemical catalysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is an electron microscope image of the electrode material made in Example 1 of the present invention.

[0022] Figure 2 This is a field emission scanning electron microscope image of the pore wall structure of the electrode material made in Example 1 of the present invention.

[0023] Figure 3 This is the adsorption-desorption curve of the electrode material prepared in Example 1 of the present invention.

[0024] Figure 4 This is the GCD curve of the electrode material prepared in Example 1 of the present invention.

[0025] Figure 5 It is an electron microscope image of the electrode material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The present invention uses the following embodiments to further illustrate the technical features of the present invention, but the protection scope of the present invention is not limited to the following embodiments.

[0027] Example 1

[0028] Formula: 30% lignin; 70% ammonium polyphosphate.

[0029] Preparation method: the carbon source and phosphorus source in the above formula are fully mixed in a mortar to form a mixture; the mixture is first pre-decomposed at 350°C for 60 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, and then the temperature is continuously raised to 850°C for activation for 60 minutes under nitrogen protection, and then ground into a powdered phosphorus oxide composite carbon material after cooling; finally, the prepared phosphorus oxide composite carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, the high-pressure boiling temperature is: 130°C, the boiling time is: 72 hours, and the water is changed every 24 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle. After boiling, filtering is performed to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall prepared by high-temperature activation and high-pressure boiling.

[0030] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0031] Example 2

[0032] Formula: Wood powder 35%; bamboo powder 35%; phosphoric acid 10%; polyphosphoric acid 20%.

[0033] Preparation method: the carbon source and phosphorus source in the above formula are fully mixed in a high-speed mixer to form a mixture; the mixture is first pre-decomposed at 300°C for 40 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, and then the temperature is continuously raised to 700°C for activation for 40 minutes under nitrogen protection, and then ground into a powdered phosphorus oxide composite carbon material after cooling; finally, the prepared phosphorus oxide composite carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, the high-pressure boiling temperature is: 110°C, the boiling time is: 60 hours, and the water is changed every 12 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle. After boiling, filtering is performed to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall prepared by high-temperature activation and high-pressure boiling.

[0034] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0035] Example 3

[0036] Formula: 25% petroleum coke powder; 25% asphalt; 25% ammonium polyphosphate cyanurate; 25% polyphosphoric acid.

[0037] Preparation method: the carbon source and phosphorus source in the above formula are fully mixed in a ball mill, first pre-decomposed at 400°C for 120 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, then continue to heat up to 900°C for activation for 180 minutes under nitrogen protection, and grind into powdered phosphorus oxide composite carbon material after cooling; finally, the prepared phosphorus oxide composite carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, the high-pressure boiling temperature is: 200°C, the boiling time is: 8 hours, and the water is changed every 4 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle. After boiling, filtering is performed to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall prepared by high-temperature activation and high-pressure boiling.

[0038] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0039] Example 4

[0040] Formula: 20% polyacrylonitrile; 40% polyphenylene ether; 10% ammonium polyphosphate; 30% polyphosphoric acid.

[0041] Preparation method: the carbon source and phosphorus source in the above formula are fully mixed in a ball mill, first pre-decomposed at 350°C for 60 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, then continue to heat up to 850°C for activation for 60 minutes under nitrogen protection, and grind into powdered phosphorus oxide composite carbon material after cooling; finally, the prepared phosphorus oxide composite carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, the high-pressure boiling temperature is: 130°C, the boiling time is: 72 hours, and the water is changed every 24 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle. After boiling, filtering is performed to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall prepared by high-temperature activation and high-pressure boiling.

[0042] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0043] Example 5

[0044] Formula: charcoal powder 70%; ammonium polyphosphate 30%.

[0045] Preparation method: the carbon source and phosphorus source in the above formula are fully mixed in a ball mill, first pre-decomposed at 400°C for 120 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, then continue to heat up to 900°C for activation for 120 minutes under nitrogen protection, and grind into powdered phosphorus oxide composite carbon material after cooling; finally, the prepared phosphorus oxide composite carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, the high-pressure boiling temperature is: 130°C, the boiling time is: 72 hours, and the water is changed once every 24 hours during the boiling period until the water used for boiling is neutral at the end of the next cycle. After boiling, filtering is performed to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall prepared by high-temperature activation and high-pressure boiling.

[0046] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0047] Comparative Example 1

[0048] Formula: 30% lignin; 70% potassium hydroxide.

[0049] Preparation method: The lignin and potassium hydroxide in the above formula are fully mixed in a mortar, and the mixture is first pre-decomposed at 350°C for 60 minutes in a high-temperature furnace in an oxygen-free environment under nitrogen protection, and then the temperature is continuously raised to 850°C for activation for 60 minutes under nitrogen protection, and then ground into powdered carbon material after cooling; since the activating agent is an alkali, the powdered carbon material prepared above needs to be acid-washed first, and then washed with water after acid washing; finally, the acid-washed carbon material is high-pressure boiled in a high-pressure reactor with deionized water as the medium, and the high-pressure boiling temperature is: 130°C, the boiling time is: 72 hours, and the water is changed every 24 hours during the boiling period. After boiling, filtering is performed to obtain a comparative electrode carbon material.

[0050] The prepared carbon material is directly ground into slurry in anhydrous ethanol according to the ratio of 8:1:1 with conductive carbon black and binder, and coated on conductive carbon paper to form an electrode sheet, which can be used after drying.

[0051] Comparative Example 2

[0052] Kuraray YP-80, the most commonly used supercapacitor on the market, was used as the electrode active material. It was ground into a slurry in anhydrous ethanol with conductive carbon black and a binder in a ratio of 8:1:1, and then coated on conductive carbon paper to make an electrode sheet for comparative testing.

[0053] The properties of the carbon materials prepared in the embodiments of the present invention and the comparative embodiments are shown in Table 1.

[0054] Table 1

[0055]

Claims

1. An ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall used as an electrode sheet, characterized in that: The electrode sheet is prepared by grinding anthill-shaped super electrode carbon material with graphene and microporous structure on the pore wall, conductive carbon black and binder in anhydrous ethanol in a ratio of 8:1:1 into slurry, and coating the slurry on conductive carbon paper to form the electrode sheet; The steps of preparing the super electrode carbon material are as follows: (1) Mix the carbon source and the phosphorus source in a high-speed mixer, mortar or ball mill according to the mass percentage of carbon source: 30-70%, phosphorus source: 30-70%; The carbon source is one or more of lignin, wood powder, petroleum coke powder, asphalt, charcoal powder, bamboo powder, polyacrylonitrile, and polyphenylene ether; The phosphorus source is one or more of phosphoric acid, polyphosphoric acid, ammonium polyphosphate, and ammonium polyphosphate cyanurate; (2) Pre-decomposing in a high temperature furnace at 300-400°C in a nitrogen-protected oxygen-free environment for 40-120 minutes; then heating to 700-900°C for activation for 40-180 minutes, and ball-milling into a powdery phosphorus oxide composite carbon material after cooling; (3) boiling the prepared phosphorus oxide composite carbon material in a high pressure reactor at 110-200° C. for 8-72 hours, filtering after boiling to obtain an ant nest-shaped super electrode carbon material with graphene and microporous structure on the pore wall; The medium for high pressure boiling is deionized water, and the water is changed every 4-24 hours during boiling until the water used for boiling is neutral at the end of the next cycle.

Citation Information

Patent Citations

  • Preparation method of biomass activated carbon for supercapacitor and super-capacity carbon

    CN113880085A

  • Preparation and application of lignin-based hierarchical porous carbon based on direct carbonization method

    CN113979433A

  • Super capacitor electrode material prepared by doping carbon material and preparation method thereof

    CN114068201A

  • Preparation method and application of bio-based porous carbon material

    CN114084884A

  • Method for manufacturing nitrogen / phosphorus codoped shrimp shell base porous carbon electrode material

    CN103824702A