Method for epitaxial growth in deep trenches

The alternating deposition and etching cycles with controlled gas flow and pressure conditions address void defects in deep trenches, enhancing the quality and reliability of epitaxial layers in semiconductor devices.

CN114914191BActive Publication Date: 2024-12-03GEKKO SEMICON (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110173513.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-09
Publication Date
2024-12-03
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

Existing epitaxial growth processes in deep trenches with high aspect ratios suffer from void defects, which compromise the quality and reliability of semiconductor devices.

Method used

A method involving alternating low-pressure deposition and etching cycles, followed by high-pressure deposition if necessary, to fill deep trenches effectively, using hydrogen chloride gas with varying flow rates and pressures to manage deposition and etching rates.

Benefits of technology

This method enhances the filling of deep trenches, reduces void defects, and improves the quality and reliability of epitaxial layers in semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114914191B_ABST
    Figure CN114914191B_ABST
Patent Text Reader

Abstract

The present invention provides a method for epitaxial growth in a deep trench, comprising: S1: forming a deep trench in a semiconductor substrate; S2: depositing an epitaxial layer in the deep trench under a low pressure condition of less than 30 Torr; S3: etching the epitaxial layer to open the opening of the deep trench; repeating the above steps S2 and S3 until the epitaxial layer fills more than 2 / 3 of the depth of the deep trench. The present invention first repeats the low-pressure deposition-etching cycle to make the epitaxial layer fill more than 2 / 3 of the depth of the deep trench, and then continues to use the low-pressure deposition-etching cycle, or uses the high-pressure deposition of >30 Torr or the high-pressure deposition-etching cycle (if necessary) until the epitaxial layer completely fills the entire depth of the deep trench, thereby solving the hole defect problem of epitaxial growth in trenches with high aspect ratio (above 30:1), improving the quality of the epitaxial layer, and improving the reliability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for epitaxial growth in a deep trench. Background Art

[0002] In the field of integrated circuit manufacturing, it is often necessary to use a process of epitaxial growth in the grooves of a semiconductor substrate. In order to achieve a good filling effect, the existing technology has a method of controlling the deposition rate so that the epitaxial growth is fast at first and then slow. There is also a method of high-pressure deposition-etching-low-pressure deposition-etching (multiple cycles are set as needed) to achieve a conical epitaxial distribution during deposition, thereby avoiding premature sealing of the trench top and causing void defects.

[0003] In order to meet the needs of further miniaturization and multi-functionality of electronic products, for example, in the field of CMOS image sensors, as the demand for high pixels and small volume continues to increase, the opening of the trench structure that needs epitaxial growth in the pixel area of ​​the device is getting smaller and smaller, and the depth is getting deeper, with an aspect ratio of more than 30:1. The above-mentioned traditional epitaxial growth process is applied to deep trenches with such a high aspect ratio, and the problem of void defects will still occur. Summary of the invention

[0004] The purpose of the present invention is to provide a method for epitaxial growth in deep trenches, solve the hole defect problem of epitaxial growth in trenches with high aspect ratio, improve the quality of epitaxial layers, and improve device reliability.

[0005] Based on the above considerations, the present invention provides a method for epitaxial growth in a deep trench, comprising: S1: forming a deep trench in a semiconductor substrate; S2: depositing an epitaxial layer in the deep trench under a low pressure condition of less than 30 Torr; S3: etching the epitaxial layer to open the opening of the deep trench; repeating the above steps S2 and S3 until the epitaxial layer fills more than 2 / 3 of the depth of the deep trench.

[0006] Preferably, the above steps S2 and S3 are repeated until the epitaxial layer completely fills the entire depth of the deep trench.

[0007] Preferably, after the epitaxial layer fills more than 2 / 3 of the depth of the deep trench, the method further comprises: S4: depositing an epitaxial layer in the deep trench under a high pressure condition greater than 30 Torr; until the epitaxial layer completely fills the entire depth of the deep trench.

[0008] Preferably, after step S4, the method further comprises: S5: etching the epitaxial layer to open the opening of the deep trench; and repeating the above steps S4 and S5 until the epitaxial layer completely fills the entire depth of the deep trench.

[0009] Preferably, in step S2, the epitaxial gas includes hydrogen chloride, and the flow rate of the hydrogen chloride gradually decreases as the process time continues.

[0010] Preferably, in step S3, hydrogen chloride is used as the etching gas, and the flow rate of the hydrogen chloride gradually increases as the process time continues.

[0011] Preferably, in the step S3, the pressure of the etching process gradually increases as the process time continues.

[0012] Preferably, the aspect ratio of the deep trench is greater than 30:1.

[0013] The method for epitaxial growth in a deep trench of the present invention can increase the free path of silicon source molecules by setting a low pressure condition of pressure <30 Torr, making it easier for them to reach the bottom of the deep trench, which is beneficial to improving the deposition rate at the bottom of the deep trench, so that the deposition rate at the bottom of the deep trench is greater than the deposition rate at the top. Therefore, compared with high-pressure deposition, low-pressure deposition can better form a conical epitaxial distribution, but it is still easy to form a sharp angle structure with two faces at the neck. In the subsequent growth process, the sharp angle position has two faces at the same time epitaxial growth, and the growth rate is higher than the bottom, which is easy to produce neck shrinkage. The neck opening can be eliminated by etching, so that the opening of the deep trench is reopened. Therefore, the present invention first repeats the low-pressure deposition-etching cycle to make the epitaxial layer fill more than 2 / 3 of the depth of the deep trench. Subsequently, the low-pressure deposition-etching cycle can be continued, or the high-pressure deposition of >30 Torr or the high-pressure deposition-etching cycle (if necessary) can be used until the epitaxial layer completely fills the entire depth of the deep trench, thereby solving the hole defect problem of epitaxial growth in trenches with high aspect ratio (above 30:1), improving the quality of the epitaxial layer, and improving the reliability of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Other features, objects and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings.

[0015] Figure 1 is a flow chart of a method for epitaxial growth in a deep trench of the present invention;

[0016] Figure 2-Figure 7 FIG. 4 is a schematic diagram of the process of the method for epitaxial growth in a deep trench according to the present invention.

[0017] In the drawings, the same or similar reference numerals denote the same or similar devices (modules) or steps throughout different drawings. DETAILED DESCRIPTION

[0018] To solve the above problems in the prior art, the present invention provides a method for epitaxial growth in deep trenches, which solves the hole defect problem of epitaxial growth in high aspect ratio trenches, improves the quality of the epitaxial layer, and improves device reliability.

[0019] In the following specific description of the preferred embodiments, reference will be made to the attached drawings which constitute a part of the present invention. The attached drawings show by way of example specific embodiments that can implement the present invention. The illustrative embodiments are not intended to be exhaustive of all embodiments according to the present invention. It will be appreciated that other embodiments may be utilized, and structural or logical modifications may also be made without departing from the scope of the present invention. Therefore, the following specific description is not restrictive, and the scope of the present invention is limited by the appended claims.

[0020] Figure 1 The method for epitaxial growth in a deep trench of the present invention is shown, comprising: S1: forming a deep trench in a semiconductor substrate; S2: depositing an epitaxial layer in the deep trench under a low pressure condition of less than 30 Torr; S3: etching the epitaxial layer to open the opening of the deep trench; repeating the above steps S2 and S3 until the epitaxial layer fills more than 2 / 3 of the depth of the deep trench.

[0021] In a preferred embodiment of the present invention, the above steps S2 and S3 may be repeated until the epitaxial layer completely fills the entire depth of the deep trench.

[0022] In another preferred embodiment of the present invention, the process may further include: S4: depositing an epitaxial layer in the deep trench under a high pressure condition greater than 30 Torr; until the epitaxial layer completely fills the entire depth of the deep trench.

[0023] In another preferred embodiment of the present invention, after step S4, the following may be further included: S5: etching the epitaxial layer to open the opening of the deep trench; repeating the above steps S4 and S5 until the epitaxial layer completely fills the entire depth of the deep trench.

[0024] The present invention is described in detail below with reference to specific embodiments.

[0025] See also Figure 2 , a semiconductor substrate 100 is provided, a patterned mask 101 is formed on the semiconductor substrate 100, and a deep trench 102 is formed in the semiconductor substrate 100 by an etching process. In advanced semiconductor processes, such as the field of high-end CMOS image sensors, the aspect ratio H:W of the deep trench 102 can reach more than 30:1.

[0026] See also Figure 3, under low pressure conditions of less than 30 Torr, an epitaxial layer 103 is deposited in the deep trench 102. The epitaxial growth temperature is between 700°C and 900°C, and the epitaxial gas includes hydrogen chloride, because under a certain hydrogen chloride flow rate condition, the epitaxial growth at the top of the deep trench 102 can be effectively suppressed, and the flow rate of the hydrogen chloride can be gradually reduced as the process time continues to ensure the deposition rate of the epitaxial growth.

[0027] Since the low pressure condition of pressure <30 Torr can increase the free path of silicon source molecules, making it easier for them to reach the bottom of the deep trench 102, it is beneficial to improve the deposition rate at the bottom of the deep trench 102, so that the deposition rate at the bottom of the deep trench 102 is greater than the deposition rate at the top. Therefore, compared with high-pressure deposition, low-pressure deposition can better form a conical epitaxial distribution, but it is still easy to form a sharp angle structure with two faces at the neck (A in the figure). In the subsequent growth process, the sharp angle position has two faces that grow epitaxially in the direction of the arrow at the same time, and the growth rate is higher than the bottom, which is easy to produce a neck closing, thereby causing a hole defect (see Figure 4 ).

[0028] See also Figure 5 Hydrogen chloride is used as an etching gas to etch the epitaxial layer 103 to open the opening of the deep trench 102, wherein the flow rate of hydrogen chloride and the pressure of the etching process can be constant or gradually increased as the process time continues to ensure that the etching effect on the top of the deep trench 102 is greater than that on the bottom, thereby eliminating the neck closing problem.

[0029] See also Figure 6 , repeat the above low pressure deposition-etching cycle until the epitaxial layer 103 fills more than 2 / 3 of the depth H of the deep trench 102. After that, since the aspect ratio of the remaining part of the deep trench 102 is lower than that at the beginning, the possibility of generating void defects is greatly reduced. According to the actual situation, any one of the following three methods can be selected until the epitaxial layer 103 completely fills the entire depth of the deep trench 102 (see Figure 7 ):

[0030] Method 1: Continue to repeat the above low-pressure deposition-etching steps until the epitaxial layer 103 completely fills the entire depth of the deep trench 102;

[0031] Method 2: Depositing the epitaxial layer 103 in the deep trench 102 under a high pressure condition greater than 30 Torr until the epitaxial layer 103 completely fills the entire depth of the deep trench 102;

[0032] Method 3: After the high-pressure deposition step of more than 30 Torr, if the neck closing problem still exists and there is a tendency to produce void defects, the epitaxial layer 103 can be etched again with hydrogen chloride to open the opening of the deep trench 102, and the above high-pressure deposition-etching steps are repeated until the epitaxial layer 103 completely fills the entire depth of the deep trench 102.

[0033] In summary, the method for epitaxial growth in a deep trench of the present invention can increase the free path of the silicon source molecules by setting a low pressure condition of pressure <30 Torr, making it easier for them to reach the bottom of the deep trench, which is beneficial to improving the deposition rate at the bottom of the deep trench, so that the deposition rate at the bottom of the deep trench is greater than the deposition rate at the top. Therefore, compared with high-pressure deposition, low-pressure deposition can better form a conical epitaxial distribution, but it is still easy to form a sharp angle structure with two faces at the neck. In the subsequent growth process, the sharp angle position has two faces epitaxially growing at the same time, and the growth rate is higher than the bottom, which is easy to produce a neck. The neck closing can be eliminated by etching, so that the opening of the deep trench is reopened. Therefore, the present invention first repeats the low-pressure deposition-etching cycle to make the epitaxial layer fill more than 2 / 3 of the depth of the deep trench. Subsequently, the low-pressure deposition-etching cycle can be continued, or the high-pressure deposition of >30 Torr or the high-pressure deposition-etching cycle (if necessary) can be used until the epitaxial layer completely fills the entire depth of the deep trench, thereby solving the hole defect problem of epitaxial growth in trenches with high aspect ratio (above 30:1), improving the quality of the epitaxial layer, and improving the reliability of the device.

[0034] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, in any case, the embodiments should be considered exemplary and non-restrictive. Furthermore, it is apparent that the term "comprising" does not exclude other elements and steps, and the wording "a" does not exclude the plural. Multiple elements stated in a device claim may also be implemented by one element. The words first, second, etc. are used to indicate names and do not indicate any particular order.

Claims

1. A method for epitaxial growth in a deep trench, characterized in that: include: S1: forming a deep trench in a semiconductor substrate, wherein the aspect ratio of the deep trench is greater than 30:1; S2: depositing an epitaxial layer in the deep trench under a low pressure condition of less than 30 Torr; S3: etching the epitaxial layer to open the opening of the deep trench; Repeat the above steps S2 and S3 until the epitaxial layer fills more than 2 / 3 of the depth of the deep trench; S4: depositing an epitaxial layer in the deep trench under a high pressure condition greater than 30 Torr; Until the epitaxial layer completely fills the entire depth of the deep trench.

2. The method for epitaxial growth in a deep trench according to claim 1, characterized in that: After step S4, the method further comprises: S5: etching the epitaxial layer to open the opening of the deep trench; The above steps S4 and S5 are repeated until the epitaxial layer completely fills the entire depth of the deep trench.

3. The method for epitaxial growth in a deep trench according to claim 1, characterized in that: In the step S2, the epitaxial gas includes hydrogen chloride, and the flow rate of the hydrogen chloride gradually decreases as the process time continues.

4. The method for epitaxial growth in a deep trench according to claim 1, characterized in that: In the step S3, hydrogen chloride is used as the etching gas, and the flow rate of the hydrogen chloride gradually increases as the process time continues.

5. The method for epitaxial growth in a deep trench according to claim 1, characterized in that: In step S3, the pressure of the etching process gradually increases as the process time continues.