Multifunctional vinyl aromatic copolymer and method for producing the same, conjugated diene copolymer and composition, crosslinked product, and tire component
By copolymerizing multifunctional vinyl aromatic copolymers with conjugated diene compounds using specific structural units, the problem of microgel formation in the preparation of conjugated diene rubber was solved, enabling the preparation of highly reactive and soluble copolymers and improving the processability and strength of the rubber.
Patent Information
- Application Number
- CN202210695039.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-09-26
AI Technical Summary
Existing technologies for preparing conjugated diene rubbers suffer from the problem of microgel formation and make it difficult to simultaneously achieve good processability, strength, and homogeneity.
Conjugated diene copolymers are prepared by copolymerization using multifunctional vinyl aromatic copolymers containing specific structural units. By utilizing a combination of monomers derived from divinyl aromatic compounds, monovinyl aromatic compounds, and cycloolefin monomers, copolymers with high reactivity and solubility are formed, avoiding gel formation.
It achieves high reactivity and solubility of conjugated diene copolymers, improves processability and strength, reduces gel formation, is suitable for molding materials and resin modifiers, and exhibits excellent filler dispersibility in rubber compositions.
Smart Images

Figure CN114933676B_ABST
Abstract
Description
[0001] The present invention is a divisional application of the invention patent application with application number 201980062619.6 (international application number PCT / JP2019 / 037953) filed on September 26, 2019, and invention name "Multifunctional vinyl aromatic copolymer and preparation method thereof, conjugated diene copolymer and composition thereof, cross-linked product, tire component". Technical Field
[0002] The present invention particularly relates to a multifunctional vinyl aromatic copolymer having excellent copolymerization reactivity with a conjugated diene compound (B) and an aromatic vinyl compound (C) in the presence of an anionic polymerization initiator and a method for producing the same, as well as a conjugated diene copolymer having excellent processability and excellent tensile strength and abrasion resistance, a conjugated diene copolymer composition containing the conjugated diene copolymer, and a cross-linked rubber product and tire component obtained by cross-linking the same. Background Art
[0003] Conjugated diene rubbers such as styrene-butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), and styrene-isoprene rubber have excellent wear resistance, elasticity, and water resistance, and are therefore used in various applications such as molding materials and resin modifiers.
[0004] One of the main uses of the conjugated diene rubber is automobile tires. The properties required in tires include mechanical strength, wear resistance, wet grip resistance, etc. (hereinafter also referred to as strength, etc.). Furthermore, in recent years, the development of tires with excellent energy-saving performance, i.e., low fuel consumption (so-called "eco tires") has become active. The eco tires are required not only to have strength, etc., but also to have low rolling resistance.
[0005] In order to ensure the strength of the tire, it is known to add fillers such as carbon black or silica (reinforcement fillers) in conjugated diene rubber, but as a material that further improves the strength of the tire and imparts excellent rolling resistance, end-modified solution polymerization type SBR (end-modified S-SBR) has attracted much attention. End-modified S-SBR has a functional group at the molecular end of SBR, and the functional group at the molecular end interacts with the filler. Through the interaction, the dispersibility of the filler in SBR is improved, and the molecular end of SBR is constrained, and mobility is reduced. As a result, the hysteresis loss (hysteresis loss) (internal friction) of the tire is reduced, and rolling resistance is reduced. Effectively utilizing the characteristics, the development of an eco-tire having both strength and low rolling resistance has been carried out.
[0006] For example, in Patent Document 1, a block copolymer including an α-methylstyrene block and a butadiene block is synthesized by living anionic polymerization using an organic lithium compound as an initiator in a non-polar solvent, and a multifunctional coupling agent is reacted as needed to obtain an S-SBR having both high temperature characteristics and rubber properties.
[0007] Patent document 2 discloses a star-block interpolymer having a random copolymer block of a conjugated diene and a monovinyl aromatic monomer, a polyconjugated diene block, and a functional group derived from a multifunctional lithium-based initiator, and discloses that the rubber can be widely used to make tire treads having excellent properties such as reduced rolling resistance and improved traction properties.
[0008] Patent Documents 1 and 2 suggest that the introduction of a branched structure into a rubber component has the effect of ensuring the processability of the rubber, but no special design is made for the interaction with the filler for ensuring strength, and the contribution to strength is insufficient.
[0009] Patent document 3 discloses a rubber composition, which is a rubber composition in which a predetermined amount of carbon black is blended into a mixed rubber containing a plurality of diene rubbers, and a polymer containing a low molecular weight functional group having a functional group that interacts with carbon black at the end of the molecular chain and a polymer structure similar to that of the rubber component of the diene rubber is blended. The rubber composition can control the amount of carbon black distributed to each diene rubber component by blending a low molecular weight compound that interacts with carbon black into the rubber. Therefore, the strengths of each rubber component can be effectively expressed, and a balance of rubber properties that are in an opposite relationship, such as rolling properties and wet properties, can be achieved. However, the technology blends low molecular weight compounds into the rubber, and therefore is not sufficient in terms of contribution to strength.
[0010] In patent document 4, a cross-linked rubber particle containing a conjugated diene monomer unit, an aromatic vinyl monomer unit and a monomer unit having at least two polymerizable unsaturated groups, and a rubber composition containing a conjugated diene / aromatic vinyl copolymer rubber containing a conjugated diene monomer unit having a specific bonding structure are disclosed, and it is disclosed that the cross-linked rubber particle may contain a monomer unit having a carboxylic acid group, a hydroxyl group and / or an epoxy group. The technology has a moderate interaction with inorganic fillers (fillers) such as silica, so the dispersibility and processability of the inorganic filler are excellent. However, the substances disclosed as monomer units having at least two polymerizable unsaturated groups or monomer units having carboxylic acid groups, hydroxyl groups and / or epoxy groups are all low molecular weight. Therefore, the reactivity is too high, and there is a risk of gelation in the cross-linked rubber particles and rubber compositions. In addition, the technology must be after the cross-linked rubber is synthesized independently from the conjugated diene / aromatic vinyl copolymer rubber, and the cross-linked rubber is blended with the conjugated diene / aromatic vinyl copolymer rubber, which needs to be improved from the perspective of the simplicity of the steps.
[0011] In view of the above problems, the present applicants have found that a copolymer rubber having both processability, strength and homogeneity can be provided by using a specific multifunctional vinyl aromatic copolymer compound having both a branched structure and an interactive function with a filler as a constituent unit of a conjugated diene rubber (Patent Document 5).
[0012] However, although the gelation of the polyfunctional vinyl aromatic copolymer compound is greatly improved, there is still a problem of incidentally generating a small amount of microgel.
[0013] Furthermore, the applicant has disclosed similar compounds to the polyfunctional vinyl aromatic copolymer compound disclosed in Patent Document 5 in Patent Document 6, Patent Document 7, etc. However, there is no teaching on using these similar compounds as constituent units of copolymer rubber.
[0014] Furthermore, the multifunctional vinyl aromatic copolymer disclosed in Patent Document 8 is a copolymer having a wide molecular weight distribution and including a large number of high molecular weight entities with significantly developed branched structures. Therefore, when used as a constituent unit of a copolymer rubber, there is a problem of incidentally generating a small amount of microgel.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application Publication No. 2003-73434
[0018] Patent Document 2: Japanese Patent Publication No. 2004-517202
[0019] Patent Document 3: Japanese Patent Application Publication No. 2005-213381
[0020] Patent Document 4: International Publication No. 2002 / 000779
[0021] Patent Document 5: International Publication No. 2018 / 084128
[0022] Patent Document 6: Japanese Patent Application Publication No. 2004-123873
[0023] Patent Document 7: Japanese Patent Application Publication No. 2018-39995
[0024] Patent Document 8: International Publication No. 2018 / 181842 Summary of the invention
[0025] The present invention aims to solve the above problems, to obtain a multifunctional vinyl aromatic copolymer which does not generate a small amount of microgel and has reactivity and solubility that can be used for the production of copolymer rubber, and to provide a copolymer rubber material having both processability, strength and homogeneity.
[0026] The present inventors have repeatedly conducted diligent studies and, as a result, have found that the multifunctional vinyl aromatic copolymer containing the structural unit (a) derived from a divinyl aromatic compound, the structural unit (b) derived from a monovinyl aromatic compound, and the structural unit (c) derived from a cycloolefin monomer containing an aromatic condensed ring structure, as the first invention, has high reactivity during the production of copolymer rubber, and have found that the above-mentioned problems can be solved by using the multifunctional vinyl aromatic copolymer as a structural unit of a conjugated diene rubber, thereby completing the present invention.
[0027] The first invention is a multifunctional vinyl aromatic copolymer, comprising: 5 mol% or more and 35 mol% or less of a structural unit (a) derived from a divinyl aromatic compound; 5 mol% or more and 25 mol% or less of a structural unit (b) derived from a monovinyl aromatic compound; and 40 mol% or more and 90 mol% or less of a structural unit (c) derived from a cycloolefin monomer containing an aromatic condensed ring structure, wherein at least a portion of the structural unit (a) is a vinyl-containing structural unit (a1) represented by the following formula (1),
[0028] [Chemistry 1]
[0029]
[0030] (Where R 1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms. )
[0031] The molar fraction of the vinyl group-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b), and the structural unit (c) is in the range of 0.01 to 0.30.
[0032] The multifunctional vinyl aromatic copolymer has a number average molecular weight Mn of 300 to 100,000, a molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn of 10.0 or less, and is soluble in toluene, xylene, tetrahydrofuran, dichloroethane or chloroform.
[0033] Examples of the cycloolefin monomer include one or more monomers selected from the group consisting of indene compounds, acenaphthene compounds, benzofuran compounds, and benzothiophene compounds.
[0034] In addition, the present invention is a method for producing the polyfunctional vinyl aromatic copolymer, comprising dissolving a polymerization raw material comprising a divinyl aromatic compound, a monovinyl aromatic compound and a cycloolefin monomer containing an aromatic fused ring structure in a uniform solvent having a dielectric constant of 2.0 to 15.0, and polymerizing at a temperature of 20° C. to 120° C. in the presence of a Lewis acid catalyst.
[0035] The present invention is also a conjugated diene-based copolymer obtained by copolymerizing the polyfunctional vinyl aromatic copolymer (A) and a conjugated diene compound (B), or a conjugated diene compound (B) and an aromatic vinyl compound (C).
[0036] The conjugated diene copolymer may contain 0.001 wt % to 6 wt % of a structural unit (A1) derived from a multifunctional vinyl aromatic copolymer, 29 wt % to 99.999 wt % of a structural unit (B1) derived from a conjugated diene compound, and 0 wt % to 70 wt % of a structural unit (C1) derived from an aromatic vinyl compound. In addition, the polymerization active end of the conjugated diene copolymer may be further reacted with a modifier to form the conjugated diene copolymer.
[0037] The present invention also provides a conjugated diene copolymer composition comprising 0.5 to 200 parts by weight of at least one reinforcing filler selected from the group consisting of silica-based inorganic fillers, metal oxides, metal hydroxides and carbon black, based on 100 parts by weight of the conjugated diene copolymer.
[0038] The conjugated diene-based copolymer composition may further contain a crosslinking agent.
[0039] The present invention also provides a cross-linked rubber obtained by cross-linking the conjugated diene copolymer composition containing a cross-linking agent.
[0040] The present invention also provides a tire member comprising the conjugated diene-based copolymer composition.
[0041] The present inventors have repeatedly conducted diligent studies and, as a result, have found that a multifunctional vinyl aromatic copolymer as the second invention, which contains structural units (a) derived from divinyl aromatic compounds and structural units (b) derived from monovinyl aromatic compounds and has a specific degree of crosslinking, molar fraction of vinyl-containing structural units and solubility, has high reactivity during the production of copolymer rubber. They have also found that the above-mentioned problems can be solved by using the multifunctional vinyl aromatic copolymer as a structural unit of a conjugated diene rubber, thereby completing the present invention.
[0042] The second invention is a multifunctional vinyl aromatic copolymer comprising: 0.5 mol% or more and 40 mol% or less of a structural unit (a) derived from a divinyl aromatic compound; and 60 mol% or more and 99.5 mol% or less of a structural unit (b) derived from a monovinyl aromatic compound, wherein at least a portion of the structural unit (a) is a crosslinking structural unit (a2) represented by the following formula (2), and a vinyl-containing structural unit (a1) represented by the following formula (1),
[0043] [Chemistry 2]
[0044]
[0045] (Where R 1 independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms.
[0046] The molar fraction of the cross-linked structural unit (a2) relative to the structural unit (a) is in the range of 0.05 to 0.50, the molar fraction of the vinyl-containing structural unit (a1) relative to the sum of the structural units (a) and the structural units (b) is in the range of 0.001 to 0.35, the number average molecular weight Mn of the multifunctional vinyl aromatic copolymer is 1,000 to 50,000, and the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is 8.0 or less.
[0047] A sample prepared by dissolving 0.5 g of the polyfunctional vinyl aromatic copolymer in 100 g of toluene is placed in a quartz cell. The haze value of the sample is measured using an integrating sphere light transmittance measuring device with toluene as the reference sample, and the haze value is 0.1 or less.
[0048] The monovinyl aromatic compound may include one or more monomers selected from the group consisting of styrene, vinylnaphthalene, vinylbiphenyl, m-methylstyrene, p-methylstyrene, o-p-dimethylstyrene, m-ethylvinylbenzene, and p-ethylvinylbenzene.
[0049] The present invention also provides a method for producing the polyfunctional vinyl aromatic copolymer, comprising performing polymerization at a temperature of 20°C to 120°C in a uniform solvent prepared by dissolving a polymerization raw material containing a divinyl aromatic compound and a monovinyl aromatic compound in a solvent having a dielectric constant of 2.0 to 15.0 in the presence of a Lewis acid catalyst.
[0050] The present invention is also a conjugated diene-based copolymer obtained by copolymerizing the polyfunctional vinyl aromatic copolymer (A) and a conjugated diene compound (B), or a conjugated diene compound (B) and an aromatic vinyl compound (C).
[0051] The conjugated diene copolymer may contain 0.001 wt % to 6 wt % of a structural unit (A1) derived from a multifunctional vinyl aromatic copolymer, 29 wt % to 99.999 wt % of a structural unit (B1) derived from a conjugated diene compound, and 0 wt % to 70 wt % of a structural unit (C1) derived from an aromatic vinyl compound. In addition, the polymerization active end of the conjugated diene copolymer may be further reacted with a modifier to form the conjugated diene copolymer.
[0052] The present invention also provides a conjugated diene copolymer composition comprising 0.5 to 200 parts by weight of at least one reinforcing filler selected from the group consisting of silica-based inorganic fillers, metal oxides, metal hydroxides and carbon black, based on 100 parts by weight of the conjugated diene copolymer.
[0053] The conjugated diene-based copolymer composition may further contain a crosslinking agent.
[0054] The present invention also provides a cross-linked rubber obtained by cross-linking the conjugated diene copolymer composition containing a cross-linking agent.
[0055] The present invention also provides a tire member comprising the conjugated diene-based copolymer composition.
[0056] The present inventors have repeatedly conducted diligent studies and, as a result, have found that a polyfunctional vinyl aromatic copolymer containing a structural unit (a) derived from a divinyl aromatic compound, a structural unit (b) derived from a monovinyl aromatic compound having no substituent at the α-position, and a structural unit (c) derived from an α,α-disubstituted olefin compound, as the third invention, has high reactivity during the production of a copolymer rubber. The inventors have also found that the above-mentioned problems can be solved by using the polyfunctional vinyl aromatic copolymer as a structural unit of a conjugated diene rubber, thereby completing the present invention.
[0057] The third invention is a multifunctional vinyl aromatic copolymer comprising: 0.5 mol% to 75 mol% of a structural unit (a) derived from a divinyl aromatic compound; 5.0 mol% to 75 mol% of a structural unit (b) derived from a monovinyl aromatic compound having no substituent at the α position; and 5.0 mol% to 75 mol% of a structural unit (c) derived from an α,α-disubstituted olefin compound, wherein at least a portion of the structural unit (a) is a crosslinking structural unit (a2) represented by the following formula (2), and a vinyl-containing structural unit (a1) represented by the following formula (1),
[0058] [Chemistry 3]
[0059]
[0060] (Where R 1 independently represents an aromatic hydrocarbon group having 6 to 30 carbon atoms.
[0061] The molar fraction of the crosslinking structural unit (a2) relative to the structural unit (a) is in the range of 0.05 to 0.60, and the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b) and the structural unit (c) is in the range of 0.001 to 0.60,
[0062] The number average molecular weight Mn of the polyfunctional vinyl aromatic copolymer is 300 to 50,000, and the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is 10.0 or less.
[0063] The α,α-disubstituted olefin compound may include one or more monomers selected from the group consisting of isobutylene, diisobutylene, 2-methyl-1-butene, 2-methyl-1-pentene, 1-methyl-1-cyclopentene, 2-methyl-1-hexene, 1-methyl-1-cyclohexene, 2-methyl-1-heptene, 2-methyl-1-octene, 2-methyl-1-nonene, 2-methyl-1-decene, 2-methyl-1-dodecene, 2-methyl-1-tetradecene, 2-methyl-1-hexadecene, 2-methyl-1-octadecene, 2-methyl-1-eicosene, 2-methyl-1-docosahexadecene, and 2-methyl-1-tetracosene.
[0064] The monovinyl aromatic compound having no substituent at the α position may be one or more monomers selected from the group consisting of styrene, vinylnaphthalene, vinylbiphenyl, m-methylstyrene, p-methylstyrene, o-p-dimethylstyrene, m-ethylvinylbenzene, and p-ethylvinylbenzene.
[0065] In addition, the present invention is a method for producing the polyfunctional vinyl aromatic copolymer, comprising dissolving a polymerization raw material comprising a divinyl aromatic compound, a monovinyl aromatic compound having no substituent at the α position, and an α,α-disubstituted olefin compound in a uniform solvent having a dielectric constant of 2.0 to 15.0, and polymerizing at a temperature of 0°C to 120°C in the presence of a Lewis acid catalyst.
[0066] The present invention is also a conjugated diene-based copolymer obtained by copolymerizing the polyfunctional vinyl aromatic copolymer (A) and a conjugated diene compound (B), or a conjugated diene compound (B) and an aromatic vinyl compound (C).
[0067] The conjugated diene copolymer may contain 0.001 wt % to 6 wt % of a structural unit (A1) derived from a multifunctional vinyl aromatic copolymer, 29 wt % to 99.999 wt % of a structural unit (B1) derived from a conjugated diene compound, and 0 wt % to 70 wt % of a structural unit (C1) derived from an aromatic vinyl compound. In addition, the polymerization active end of the conjugated diene copolymer may be further reacted with a modifier to form the conjugated diene copolymer.
[0068] The present invention is also a conjugated diene copolymer composition, which may contain 0.5 to 200 parts by weight of at least one reinforcing filler selected from the group consisting of silica-based inorganic fillers, metal oxides, metal hydroxides and carbon black, based on 100 parts by weight of the conjugated diene copolymer.
[0069] The conjugated diene-based copolymer composition may further contain a crosslinking agent.
[0070] The present invention also provides a cross-linked rubber obtained by cross-linking the conjugated diene copolymer composition containing a cross-linking agent.
[0071] The present invention also provides a tire member comprising the conjugated diene-based copolymer composition.
[0072] The multifunctional vinyl aromatic copolymer of the present invention has reactivity and solubility that can be used in the manufacture of copolymer rubber, and is therefore suitable as a raw material thereof. The conjugated diene copolymer of the present invention has a structural unit having both a branched structure and an interaction function with a filler, and is therefore excellent as a rubber having both processability and strength. Furthermore, it is not easy to form a gel-like substance and becomes homogeneous, and can be applied to molding materials, resin improvers, and the like.
[0073] Furthermore, the cross-linked rubber composition obtained by cross-linking the conjugated diene copolymer containing a filler has excellent dispersibility of the filler and thus has excellent mechanical strength and wear resistance. DETAILED DESCRIPTION
[0074] The polyfunctional vinyl aromatic copolymer according to the first invention will be described.
[0075] The polyfunctional vinyl aromatic copolymer of the present invention contains a structural unit (a) derived from a divinyl aromatic compound, a structural unit (b) derived from a monovinyl aromatic compound, and a structural unit (c) derived from a cycloolefin monomer containing an aromatic fused ring structure.
[0076] The number average molecular weight Mn may be 300 to 100,000, the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn may be 10.0 or less, and the polyol may be soluble in toluene, xylene, tetrahydrofuran, dichloroethane or chloroform.
[0077] The multifunctional vinyl aromatic copolymer of the present invention is preferably solvent-soluble, and therefore is also referred to as a soluble multifunctional vinyl aromatic copolymer, or simply a copolymer.
[0078] The structural unit described in this specification refers to a repeating unit present in the main chain of the copolymer.
[0079] The structural unit (a) derived from the divinyl aromatic compound may have several structural units with different structures, such as a structural unit in which only one vinyl group is reacted and a structural unit in which two vinyl groups are reacted, but includes structural units in which only one vinyl group is reacted in a molar fraction range of 0.01 to 0.30, i.e., vinyl-containing structural units (a1) represented by the above formula (1).
[0080] The preferred lower limit is 0.04, more preferably 0.05. In addition, the preferred upper limit is 0.25, more preferably 0.20. By setting it to the range, a copolymer rubber having excellent reactivity when copolymerized with a conjugated diene compound while maintaining solubility, excellent compatibility with diene rubber, and excellent processability, tensile strength, and wear resistance can be obtained. If the molar fraction is less than 0.01, there is a tendency for the copolymerization reactivity with a conjugated diene compound to decrease, and if it is greater than 0.30, there is a tendency to generate microgels during copolymerization.
[0081] Here, the molar fraction is the molar fraction of the vinyl group-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b), and the structural unit (c), and is calculated by the following formula (12).
[0082] (a1) / [(a)+(b)+(c)]…(12)
[0083] Here, (a), (b), (c) and (a1) represent the amounts (moles) of the structural unit (a), the structural unit (b), the structural unit (c) and the structural unit (a1), respectively.
[0084] The polyfunctional vinyl aromatic copolymer of the present invention preferably contains 5 mol % to 35 mol % of the structural unit (a) derived from the divinyl aromatic compound.
[0085] When the structural unit contains only structural unit (a), structural unit (b) and structural unit (c), the molar fraction of structural unit (a) is 0.05 to 0.35 relative to the sum of structural unit (a), structural unit (b) and structural unit (c). The molar fraction is calculated by the following formula (13).
[0086] (a) / [(a)+(b)+(c)]…(13)
[0087] (Here, (a), (b), and (c) have the same meanings as in formula (12).)
[0088] The preferred lower limit of the molar fraction is 0.06, and more preferably 0.07. The preferred upper limit is 0.30, and more preferably 0.25.
[0089] When structural units other than structural units (a), (b) and (c) are included, the preferred lower limit is 0.02, more preferably 0.05, and even more preferably 0.07. The preferred upper limit is 0.35, more preferably 0.30, and even more preferably 0.25.
[0090] On the other hand, the molar fraction of the structural unit (b) derived from the monovinyl aromatic compound is 0.05 to 0.25, and the preferred lower limit is 0.07. The preferred upper limit is 0.23, and more preferably 0.20.
[0091] The molar fraction of the structural unit (c) derived from the cycloolefin monomer is 0.40 to 0.90, with a preferred lower limit of 0.45, more preferably 0.50, and still more preferably 0.65. The preferred upper limit is 0.86, and more preferably 0.80.
[0092] When only the structural unit (a), the structural unit (b) and the structural unit (c) are included, the molar fraction of the structural unit (b) is calculated by the following formula (14), and the molar fraction of the structural unit (c) is calculated by the following formula (15).
[0093] (b) / [(a)+(b)+(c)]…(14)
[0094] (c) / [(a)+(b)+(c)]…(15)
[0095] (Here, (a), (b), and (c) have the same meanings as in formula (12).)
[0096] When a structural unit other than the structural unit (a), the structural unit (b), and the structural unit (c) is included, the preferred molar fraction of the structural unit (b) or the structural unit (c) is also within the above range.
[0097] The structural unit (a) derived from the divinyl aromatic compound includes a vinyl as a branch component for expressing copolymerization reactivity with a conjugated diene compound. On the other hand, the structural unit (b) derived from the monovinyl aromatic compound does not have a vinyl group participating in the curing reaction, so it is given formability or compatibility. In addition, the structural unit (c) derived from the cycloolefin monomer can affect the molecular weight and molecular weight distribution of the multifunctional vinyl aromatic copolymer due to its introduction amount, so it is given the ease of generation or compatibility of reactivity and gel. Therefore, if the molar fraction of the structural unit (a) is less than 0.05, the heat resistance of the cured product is insufficient, and if the molar fraction of the structural unit (a) exceeds 0.35, the forming processability is reduced. In addition, if the molar fraction of the structural unit (b) exceeds 0.25, the heat resistance is reduced, and if the molar fraction of the structural unit (b) is less than 0.05, the forming processability is reduced. On the other hand, when the molar fraction of the structural unit (c) exceeds 0.90, the heat resistance decreases, and when the molar fraction of the structural unit (c) is less than 0.40, the formability decreases.
[0098] The Mn (number average molecular weight in terms of standard polystyrene measured by gel permeation chromatography) of the multifunctional vinyl aromatic copolymer of the present invention is preferably 300 to 100,000, more preferably 400 to 50,000, and further preferably 500 to 10,000. If Mn is less than 300, the amount of monofunctional copolymer contained in the copolymer increases, so there is a tendency for the copolymerization reactivity with the conjugated diene compound to decrease. In addition, if Mn exceeds 100,000, gel is easily generated, and there is a tendency for the molding processability or tensile elongation at break to decrease. The value of the molecular weight distribution (Mw / Mn) is preferably 10.0 or less, more preferably 8.0 or less, and further preferably 1.0 to 7.0. Most preferably, it is 1.3 to 6.0. If Mw / Mn exceeds 10.0, there is a tendency for the processing characteristics of the copolymer rubber to deteriorate, and there is a tendency for gel to be generated.
[0099] The soluble multifunctional vinyl aromatic copolymer of the present invention can be dissolved in a solvent selected from toluene, xylene, tetrahydrofuran, dichloroethane or chloroform, but advantageously can be dissolved in any of the solvents. Since it is a multifunctional copolymer that can be dissolved in a solvent, a part of the vinyl groups of divinylbenzene must remain without crosslinking, and the branching degree must be appropriate. The copolymer or its production method is known from the patent literature, etc. Moreover, it can be a copolymer that dissolves more than 50 g in 100 g of solvent. More preferably, it dissolves more than 80 g.
[0100] The multifunctional vinyl aromatic copolymer of the second invention will be described.
[0101] The polyfunctional vinyl aromatic copolymer of the present invention contains a structural unit (a) derived from a divinyl aromatic compound and a structural unit (b) derived from a monovinyl aromatic compound.
[0102] Furthermore, at least a part of the structural unit (a) includes a crosslinking structural unit (a2) represented by the formula (2) and a vinyl group-containing structural unit (a1) represented by the formula (1).
[0103] The molar fraction (also referred to as the degree of crosslinking) of the crosslinked structural unit (a2) derived from the divinyl aromatic compound relative to the structural unit (a) is in the range of 0.05 to 0.50. In addition, the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a) and the structural units (b) is in the range of 0.001 to 0.35.
[0104] The crosslinking degree of the crosslinking structural unit (a2) is in the range of 0.05 to 0.50, with a preferred lower limit of 0.06 and more preferably 0.07. In addition, the preferred upper limit is 0.45, more preferably 0.40. Particularly preferably 0.35, most preferably 0.30. By setting the range, a copolymer rubber having excellent reactivity when copolymerized with a conjugated diene compound while maintaining solubility, excellent compatibility with a diene rubber, and excellent processability, tensile strength, and wear resistance can be obtained. By the method for preparing the multifunctional vinyl aromatic copolymer of the present invention, the crosslinking degree and the vinyl-containing structural unit (a1) represented by formula (1) described later are parameters that can be independently controlled and changed at will, but if the crosslinking degree is less than 0.05, the crosslinking degree of the multifunctional vinyl aromatic copolymer is small, so that the crosslinking reaction easily occurs in the molecule of the vinyl-containing structural unit (a1) represented by formula (1), and there is a tendency to generate microgels when copolymerized with conjugated diene compounds, etc. On the other hand, if the degree of crosslinking exceeds 0.50, the molecular weight of the polyfunctional vinyl aromatic copolymer itself increases, and the molecular weight distribution tends to become broad, so that the abrasion resistance tends to decrease.
[0105] The structural unit (a) derived from the divinyl aromatic compound may have several structural units with different structures, such as a structural unit in which only one vinyl group is reacted and a structural unit in which two vinyl groups are reacted, but includes a structural unit in which only one vinyl group is reacted within the range of 0.001 to 0.35 in terms of the molar fraction, i.e., a vinyl-containing structural unit (a1) represented by the formula (1).
[0106] The preferred lower limit is 0.005, more preferably 0.01. In addition, the preferred upper limit is 0.30, more preferably 0.20. By setting it to the range, a copolymer rubber having excellent reactivity when copolymerized with a conjugated diene compound while maintaining solubility, excellent compatibility with diene rubber, and excellent processability, tensile strength, and wear resistance can be obtained. If the molar fraction is less than 0.001, there is a tendency for the copolymerization reactivity with a conjugated diene compound to decrease, and if the molar fraction is greater than 0.35, there is a tendency to generate microgels during copolymerization.
[0107] Here, the molar fraction is the molar fraction of the vinyl group-containing structural unit (a1) relative to the total of the structural unit (a) and the structural unit (b), and is calculated by the following formula (23).
[0108] (a1) / [(a)+(b)] (23)
[0109] Here, (a), (b) and (a1) represent the amounts (moles) of the structural unit (a), the structural unit (b) and the structural unit (a1), respectively.
[0110] The multifunctional vinyl aromatic copolymer of the present invention contains 0.5 mol % to 40 mol % of the structural unit (a) derived from the divinyl aromatic compound.
[0111] When the structural unit contains only the structural unit (a) and the structural unit (b), the molar fraction of the structural unit (a) is 0.005 to 0.40 relative to the total of the structural unit (a) and the structural unit (b). The molar fraction is calculated by the following formula (24).
[0112] (a) / [(a)+(b)] (24)
[0113] (Here, (a) and (b) have the same meaning as in formula (23).)
[0114] The preferred lower limit of the molar fraction is 0.006, and more preferably 0.007. The preferred upper limit is 0.30, and more preferably 0.25.
[0115] Furthermore, when the structural units other than the structural units (a) and the structural units (b) are included, the preferred lower limit of the content is 0.2 mol%, more preferably 0.5 mol%, and further preferably 0.7 mol%. In addition, the preferred upper limit is 35 mol%, more preferably 30 mol%, and further preferably 25 mol%.
[0116] On the other hand, the molar fraction of the structural unit (b) derived from the monovinyl aromatic compound is 0.60 to 0.995. The preferred lower limit is 0.70. The more preferred lower limit is 0.75. The preferred upper limit is 0.994, and the more preferred upper limit is 0.993.
[0117] When only the structural unit (a) and the structural unit (b) are included, the molar fraction of the structural unit (b) is calculated by the following formula (25).
[0118] (b) / [(a)+(b)] (25)
[0119] (Here, (a) and (b) have the same meaning as in formula (23).)
[0120] In addition, when a structural unit other than the structural unit (a) and the structural unit (b) is contained, the preferred molar fraction of the structural unit (b) is also within the above range.
[0121] The structural unit (a) derived from the divinyl aromatic compound contains a vinyl group as a branch component for expressing copolymerization reactivity with the conjugated diene compound. On the other hand, the structural unit (b) derived from the monovinyl aromatic compound does not have a vinyl group that participates in the curing reaction, thereby imparting formability or compatibility. Therefore, if the molar fraction of the structural unit (a) is less than 0.005, the heat resistance of the cured product is insufficient, and if the molar fraction of the structural unit (a) exceeds 0.40, the formability is reduced. In addition, if the molar fraction of the structural unit (b) exceeds 0.995, the heat resistance is reduced, and if the molar fraction of the structural unit (b) is less than 0.60, the formability is reduced.
[0122] The polyfunctional vinyl aromatic copolymer of the present invention may contain not only the above-mentioned structural units but also other structural units. The details of other structural units can be understood from the description of the production method.
[0123] The Mn (number average molecular weight in terms of standard polystyrene measured by gel permeation chromatography) of the multifunctional vinyl aromatic copolymer of the present invention is 1,000 to 50,000, preferably 1,200 to 45,000, and more preferably 1,400 to 30,000. It is further preferably 1,600 to 20,000, and most preferably 2,000 to 10,000. If Mn is less than 1,000, the amount of monofunctional copolymer contained in the copolymer increases, so there is a tendency for the copolymerization reactivity with the conjugated diene compound to decrease. In addition, if Mn exceeds 50,000, not only is gel easily generated, but also there is a tendency for the molding processability or tensile elongation at break to decrease. The molecular weight distribution is 8.0 or less, preferably 7.0 or less, and more preferably 1.3 to 6.0. If Mw / Mn exceeds 8.0, there is a tendency not only for the processing characteristics of the copolymer rubber to deteriorate, but also for the formation of gel.
[0124] The polyfunctional vinyl aromatic copolymer of the present invention can be dissolved in a solvent selected from toluene, xylene, tetrahydrofuran, dichloroethane or chloroform, but advantageously can be dissolved in any of the above solvents. Since it is a polyfunctional copolymer that can be dissolved in a solvent, a part of the vinyl groups of divinylbenzene must remain without crosslinking, and the branching degree must be appropriate. The copolymer or its production method is known from the above patent documents, etc. Moreover, the copolymer can be dissolved in 100g of solvent in an amount of 50g or more. More preferably, it can be dissolved in an amount of 80g or more.
[0125] The polyfunctional vinyl aromatic copolymer of the present invention may have a haze value (turbidity) of a toluene solution of 0.1 or less. Here, the haze value refers to the haze value measured by using an integrating sphere light transmittance measuring device with toluene as the reference sample and placing a solution prepared by dissolving 0.5 g of the polyfunctional vinyl aromatic copolymer in 100 g of toluene in a quartz cell.
[0126] The haze value is also related to the evaluation of solubility in a solvent, and a low haze value means excellent solubility or less gel.
[0127] The polyfunctional vinyl aromatic copolymer of the third invention will be described.
[0128] The polyfunctional vinyl aromatic copolymer of the present invention contains a structural unit (a) derived from a divinyl aromatic compound, a structural unit (b) derived from a monovinyl aromatic compound having no substituent at the α-position, and a structural unit (c) derived from an α,α-disubstituted olefin compound.
[0129] Furthermore, at least a part of the structural unit (a) includes a crosslinking structural unit (a2) represented by the formula (2) and a vinyl group-containing structural unit (a1) represented by the formula (1).
[0130] The molar fraction (also referred to as the degree of crosslinking) of the crosslinked structural unit (a2) derived from the divinyl aromatic compound relative to the structural unit (a) is in the range of 0.05 to 0.60. In addition, the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b) and the structural unit (c) is in the range of 0.001 to 0.60.
[0131] The crosslinking degree of the crosslinking structural unit (a2) is in the range of 0.05 to 0.60, with a preferred lower limit of 0.06, and more preferably 0.07. In addition, the preferred upper limit is 0.55, and more preferably 0.50. It is particularly preferably 0.45, and most preferably 0.40. The most suitable range is 0.20 to 0.40. According to the method for preparing the multifunctional vinyl aromatic copolymer of the present invention, the crosslinking degree and the vinyl-containing structural unit (a1) represented by formula (1) are parameters that can be independently and arbitrarily controlled and changed, but if the crosslinking degree of the crosslinking structural unit (a2) is less than 0.05, the crosslinking degree of the multifunctional vinyl aromatic copolymer is small, and therefore the crosslinking reaction is easily generated in the molecule of the vinyl-containing structural unit (a1) represented by formula (1), and there is a tendency to generate microgels when copolymerized with conjugated diene compounds, etc. On the other hand, if the degree of crosslinking exceeds 0.60, the molecular weight of the polyfunctional vinyl aromatic copolymer itself increases, and the molecular weight distribution tends to become broad, so that the abrasion resistance tends to decrease.
[0132] The structural unit (a) derived from the divinyl aromatic compound may have several structural units with different structures, such as a structural unit in which only one vinyl group is reacted and a structural unit in which two vinyl groups are reacted, but includes a structural unit in which only one vinyl group is reacted within the range of 0.001 to 0.60 in terms of the molar fraction, i.e., a vinyl-containing structural unit (a1) represented by the formula (1).
[0133] The preferred lower limit is 0.005, more preferably 0.01. In addition, the preferred upper limit is 0.55, more preferably 0.50. The most suitable range is 0.10 to 0.50. By setting the range, a copolymer rubber having excellent reactivity when copolymerized with a conjugated diene compound while maintaining solubility, excellent compatibility with a diene rubber, and excellent processability, tensile strength, and wear resistance can be obtained. If the molar fraction is less than 0.001, there is a tendency for the copolymerization reactivity with a conjugated diene compound to decrease, and if the molar fraction is greater than 0.60, there is a tendency to generate microgels during copolymerization.
[0134] Here, the molar fraction is the molar fraction of the vinyl group-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b) and the structural unit (c), and is calculated by the following formula (33).
[0135] (a1) / [(a)+(b)+(c)] (33)
[0136] Here, (a), (b), (c) and (a1) represent the amounts (moles) of the structural unit (a), the structural unit (b), the structural unit (c) and the structural unit (a1), respectively.
[0137] The polyfunctional vinyl aromatic copolymer of the present invention contains 0.5 mol % to 60 mol % of the structural unit (a) derived from the divinyl aromatic compound.
[0138] When the structural unit contains only structural unit (a), structural unit (b) and structural unit (c), the molar fraction of structural unit (a) is 0.005 to 0.75 relative to the sum of structural unit (a), structural unit (b) and structural unit (c). The molar fraction is calculated by the following formula (34).
[0139] (a) / [(a)+(b)+(c)] (34)
[0140] (Here, (a), (b) and (c) have the same meanings as in formula (33).)
[0141] The preferred lower limit of the molar fraction is 0.006, more preferably 0.007. The preferred upper limit is 0.70, more preferably 0.60. The most suitable range is 0.10 to 0.55.
[0142] Furthermore, when the structural units other than the structural units (a), (b) and (c) are included, the lower limit of the content is preferably 0.2 mol%, more preferably 0.5 mol%, and further preferably 0.7 mol%. In addition, the upper limit is preferably 50 mol%, more preferably 45 mol%, and further preferably 40 mol%.
[0143] The multifunctional vinyl aromatic copolymer of the present invention contains 5.0 mol% to 75 mol% of structural units (b) derived from monovinyl aromatic compounds having no substituent at the α position. The molar fraction is 0.05 to 0.75. The preferred lower limit is 0.06. The more preferred lower limit is 0.07. In addition, the preferred upper limit is 0.70, and more preferably 0.65. The most suitable is 0.30 to 0.60.
[0144] When only the structural unit (a), the structural unit (b) and the structural unit (c) are included, the molar fraction of the structural unit (b) is calculated by the following formula (35).
[0145] (b) / [(a)+(b)+(c)] (35)
[0146] (Here, (a), (b) and (c) have the same meanings as in formula (33).)
[0147] In addition, when a structural unit other than the structural unit (a), the structural unit (b) and the structural unit (c) is contained, the preferred molar fraction of the structural unit (b) is also within the above range.
[0148] The multifunctional vinyl aromatic copolymer of the present invention contains 5.0 mol% to 75 mol% of the structural unit (c) derived from the α,α-disubstituted olefin compound. The molar fraction is 0.05 to 0.75. The preferred lower limit is 0.06. The more preferred lower limit is 0.07. In addition, the preferred upper limit is 0.70, and the more preferred upper limit is 0.65. The most suitable is 0.10 to 0.40.
[0149] When only the structural unit (a), the structural unit (b) and the structural unit (c) are included, the molar fraction of the structural unit (c) is calculated by the following formula (36).
[0150] (c) / [(a)+(b)+(c)] (36)
[0151] (Here, (a), (b) and (c) have the same meanings as in formula (33).)
[0152] In addition, when a structural unit other than the structural unit (a), the structural unit (b) and the structural unit (c) is included, the preferred molar fraction of the structural unit (c) is also within the above range.
[0153] The structural unit (a) derived from the divinyl aromatic compound contains a vinyl group as a branch component for expressing copolymerization reactivity with the conjugated diene compound, while the structural unit (b) derived from the monovinyl aromatic compound having no substituent at the α position does not have a vinyl group that participates in the curing reaction, thereby imparting moldability or compatibility, etc. The structural unit (c) derived from the α,α-disubstituted olefin compound easily undergoes a chain transfer reaction, and thus has a function of controlling the molecular weight.
[0154] Furthermore, if the molar fraction of the structural unit (a) is less than 0.005, the heat resistance of the cured product is insufficient, and if the molar fraction of the structural unit (a) exceeds 0.75, the formability is reduced. In addition, if the molar fraction of the structural unit (b) exceeds 0.75, the heat resistance is reduced, and if the molar fraction of the structural unit (b) is less than 0.05, the formability is reduced. On the other hand, if the molar fraction of the structural unit (c) exceeds 0.75, the heat resistance is reduced, and if the molar fraction of the structural unit (c) is less than 0.05, the molecular weight increases, and the compatibility with other resins or the formability is reduced.
[0155] The polyfunctional vinyl aromatic copolymer of the present invention may contain not only the above-mentioned structural units but also other structural units. The details of other structural units can be understood from the description of the production method.
[0156] The Mn (number average molecular weight in terms of standard polystyrene measured by gel permeation chromatography) of the multifunctional vinyl aromatic copolymer of the present invention is 300 to 50,000, preferably 500 to 45,000, and more preferably 600 to 40,000. It is further preferably 700 to 35,000, and most preferably 800 to 30,000. The most suitable is 900 to 3,000. If Mn is less than 300, the amount of monofunctional copolymer contained in the copolymer increases, so there is a tendency for the copolymerization reactivity with the conjugated diene compound to decrease. In addition, if Mn exceeds 50,000, it is not only easy to generate gel, but also there is a tendency for the molding processability or tensile elongation at break to decrease. The molecular weight distribution is 10.0 or less, preferably 9.0 or less, and more preferably 1.3 to 8.0. The most suitable is 2.0 to 6.0. If Mw / Mn exceeds 10.0, not only will the processing properties of the copolymer rubber tend to deteriorate, but also gel will tend to be generated.
[0157] The polyfunctional vinyl aromatic copolymer of the present invention can be dissolved in a solvent selected from toluene, xylene, tetrahydrofuran, dichloroethane or chloroform, but advantageously can be dissolved in any of the above solvents. Since it is a polyfunctional copolymer that can be dissolved in a solvent, a part of the vinyl groups of divinylbenzene must remain without crosslinking, and the branching degree must be appropriate. The copolymer or its production method is known from the above patent documents, etc. Moreover, the copolymer can be dissolved in 100g of solvent in an amount of 50g or more. More preferably, it can be dissolved in an amount of 80g or more.
[0158] Next, the production method of the polyfunctional vinyl aromatic copolymer of the first invention, the second invention, and the third invention is described. The polyfunctional vinyl aromatic copolymer of the present invention can be advantageously produced by the production method.
[0159] In the production method of the present invention, polymerization can be carried out at a temperature of 20°C to 60°C in the presence of a Lewis acid catalyst in a uniform solvent prepared by dissolving a polymerization raw material containing essential components such as a divinyl aromatic compound and a monovinyl aromatic compound in a solvent having a dielectric constant of 2.0 to 15.0.
[0160] Divinyl aromatic compounds make copolymer branches and form multifunctional, and play an important role as a cross-linking component for making copolymers generate branches when copolymerized with conjugated diene compounds. As the example of divinyl aromatic compounds, divinylbenzene (including each isomer), divinylnaphthalene (including each isomer), divinylbiphenyl (including each isomer) are preferably used, but are not limited to these. In addition, these can be used alone or in combination of two or more. From the viewpoint of forming processability, divinylbenzene (inter-body, isomer or isomer mixture of these) is more preferably used.
[0161] The monovinyl aromatic compound improves the solvent solubility, compatibility, and processability of the copolymer.
[0162] As examples of monovinyl aromatic compounds, vinyl aromatic compounds such as styrene, vinyl naphthalene, and vinyl biphenyl can be cited; core alkyl substituted vinyl aromatic compounds such as o-methyl styrene, m-methyl styrene, p-methyl styrene, o-, p-dimethyl styrene, o-ethyl vinyl benzene, m-ethyl vinyl benzene, and p-ethyl vinyl benzene; etc., but are not limited to these. In order to prevent the gelation of the copolymer and improve the solubility, compatibility, and processability in the solvent, from the perspective of cost and ease of acquisition, styrene, ethyl vinyl benzene (including each isomer), ethyl vinyl biphenyl (including each isomer), and ethyl vinyl naphthalene (including each isomer) are particularly preferably used. From the perspective of compatibility and cost, styrene and ethyl vinyl benzene (inter-, para-, or isomer mixtures of these) are more preferred.
[0163] A compound having no substituent at the α-position is preferred.
[0164] In the first invention, the cycloolefin monomer contains an aromatic fused ring structure, but it also acts as a chain transfer agent to control the molecular weight and molecular weight distribution of the copolymer during polymerization, thereby improving solvent solubility and processability while maintaining the high dielectric properties of the hydrocarbon resin material.
[0165] As the cycloolefin monomer, any monomer containing an aromatic ring and a cycloolefin ring condensed therewith may be used, and the cycloolefin ring may contain an unsaturated bond capable of cation polymerization, and may contain heterogeneous atoms such as oxygen atoms or sulfur atoms as ring-constituting atoms. In addition, the aromatic ring or the cycloolefin ring may have a substituent such as an alkyl group, an alkoxy group, or an acyl group.
[0166] Preferred cycloolefin-based monomers include monomers selected from the group consisting of indene-based compounds, acenaphthene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds.
[0167] Examples of the indene compound include at least one compound selected from the group consisting of indene, alkyl indenes, halogenated indenes, aryl indenes, alkoxy indenes, alkoxycarbonyl indenes, acyloxy indenes, alkylsilyl indenes and alkylstannyl indenes.
[0168] Examples of the acenaphthene-based compound include at least one compound selected from the group consisting of acenaphthene, alkylacenaphthenes, halogenated acenaphthenes, arylacenaphthenes, alkoxyacenaphthenes, alkoxycarbonylacenaphthenes, acyloxyacenaphthenes, alkylsilylacenaphthenes, and alkylstannylacenaphthenes.
[0169] The benzofuran compounds and benzothiophene compounds may be not only benzofuran and benzothiophene, but also benzofurans and benzothiophenes modified with the same substituents as indene compounds and acenaphthene compounds. In addition, the benzofuran compounds may be 1-benzofuran or 2-benzofuran. The same is true for benzothiophene.
[0170] The cycloolefin monomers specifically exemplified above can be used alone or in combination of two or more. Among these cycloolefin monomers, indene compounds and acenaphthene compounds are preferably used from the viewpoints of industrial ease of acquisition, dielectric properties, and the molecular weight control effect of the copolymer of the present invention. Indene is most preferably used from the viewpoints of copolymerization reactivity and molecular weight control effect.
[0171] In the third invention, the α,α-disubstituted olefin compound has a function of controlling the molecular weight of the copolymer, thereby improving solvent solubility, compatibility and processability. Examples of the α,α-disubstituted olefin compound include one or more monomers selected from the group consisting of isobutylene, diisobutylene, 2-methyl-1-butene, 2-methyl-1-pentene, 1-methyl-1-cyclopentene, 2-methyl-1-hexene, 1-methyl-1-cyclohexene, 2-methyl-1-heptene, 2-methyl-1-octene, 2-methyl-1-decene, 2-methyl-1-dodecene, 2-methyl-1-tetradecene, 2-methyl-1-hexadecene, 2-methyl-1-octadecene, 2-methyl-1-eicosene, 2-methyl-1-eicosene, 2-methyl-1-eicosene, and α-methylstyrene, but are not limited thereto. In order to control the molecular weight and molecular weight distribution of the copolymer, prevent the formation of gel, and improve the solubility, compatibility, and processability in the solvent, it is preferred to use aliphatic-substituted α,α-disubstituted olefin compounds such as isobutylene, diisobutylene, 2-methyl-1-pentene, 2-methyl-1-hexene, and isoprene from the perspective of cost and availability, or α-methylstyrene if it is an aromatic-substituted α,α-disubstituted olefin compound. From the perspective of ease of production and cost, isobutylene, diisobutylene, and α-methylstyrene are more preferred.
[0172] In addition, in the method for producing the copolymer of the present invention, not only the essential components such as divinyl aromatic compounds and monovinyl aromatic compounds but also other monomers such as trivinyl aromatic compounds, trivinyl aliphatic compounds or divinyl aliphatic compounds and monovinyl aliphatic compounds may be used within a range not impairing the effects of the present invention, thereby introducing structural units (e) derived from other monomers into the copolymer.
[0173] As specific examples of the other monomers, 1,3,5-trivinylbenzene, 1,3,5-trivinylnaphthalene, 1,2,4-trivinylcyclohexane, ethylene glycol diacrylate, butadiene, etc. can be preferably cited, but are not limited thereto. These can be used alone or in combination of two or more. Other monomers can be used in the range of less than 30 mol% of all monomers. Thus, the structural unit (e) derived from other monomers is within the range of less than 30 mol% relative to the total amount of the structural units in the copolymer.
[0174] In the method for producing a copolymer of the present invention, a copolymer is produced by polymerizing monomers containing essential components such as a divinyl aromatic compound and a monovinyl aromatic compound and, if necessary, other monomers in the presence of a Lewis acid catalyst.
[0175] In the first invention, the usage ratio of each component as a monomer can be set to the following range with respect to 100 mol % of the total of the divinyl aromatic compound, the monovinyl aromatic compound and the cycloolefin-based monomer.
[0176] Divinyl aromatic compound: 5 mol% to 35 mol%, preferably 6 mol% to 30 mol%, more preferably 7 mol% to 25 mol%.
[0177] Monovinyl aromatic compound: 5 mol% to 25 mol%, preferably 6 mol% to 23 mol%, more preferably 7 mol% to 20 mol%.
[0178] Cycloolefin monomer: 40 mol% to 90 mol%, preferably 45 mol% to 86 mol%, more preferably 50 mol% to 80 mol%.
[0179] In the second invention, the usage ratio of each component as a monomer can be set to the following range with respect to 100 mol % of the total of the divinyl aromatic compound and the monovinyl aromatic compound.
[0180] Divinyl aromatic compound: 0.2 mol% to 45 mol%, preferably 0.3 mol% to 40 mol%, more preferably 0.4 mol% to 35 mol%.
[0181] Monovinyl aromatic compound: 55 mol% to 99.8 mol%, preferably 60 mol% to 99.7 mol%, more preferably 65 mol% to 99.6 mol%.
[0182] In the third invention, the usage ratio of each component as a monomer can be set to the following range with respect to 100 mol % of the total of the divinyl aromatic compound, the monovinyl aromatic compound having no substituent at the α-position, and the α,α-disubstituted olefin compound.
[0183] Divinyl aromatic compound: 0.2 mol% to 75 mol%, preferably 0.3 mol% to 65 mol%, more preferably 0.4 mol% to 55 mol%, most preferably 5 mol% to 50 mol%.
[0184] Monovinyl aromatic compound having no substituent at the α-position: 7 mol% to 99 mol%, preferably 10 mol% to 95 mol%, more preferably 15 mol% to 90 mol%.
[0185] α,α-disubstituted olefin compound: 5 mol% to 99 mol%, preferably 10 mol% to 95 mol%, more preferably 15 mol% to 90 mol%, and most preferably 20 mol% to 60 mol%.
[0186] As the Lewis acid catalyst (e) used herein, as long as it is a compound comprising a metal ion (acid) and a ligand (base) and can receive an electron pair, it can be used without particular limitation. Among the Lewis acid catalysts, from the viewpoint of the heat decomposition resistance of the obtained copolymer, preferably a metal fluoride or its complex, particularly preferably a divalent to hexavalent metal fluoride or its complex of B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Ti, W, Zn, Fe and V. These catalysts can be used alone or in combination of two or more. From the viewpoint of the control of the molecular weight and molecular weight distribution of the obtained copolymer and the polymerization activity, it is most preferred to use an ether complex of boron trifluoride. Here, as the ether of the ether complex, there are diethyl ether, dimethyl ether, etc.
[0187] Regarding the Lewis acid catalyst, relative to the total of 100 moles of all monomer components, the Lewis acid catalyst can be used in the range of 0.001 mole to 100 moles, more preferably 0.01 mole to 50 moles. Most preferably, it is 0.1 mole to 10 moles. If it exceeds 100 moles, the polymerization rate becomes too large, so it is difficult to control the molecular weight distribution. In addition, if it is less than 0.001 mole, the polymerization rate becomes too small, thus resulting in an increase in cost, which is not suitable for industrial implementation.
[0188] In the method for producing the copolymer of the present invention, one or more Lewis basic compounds may be used as a co-catalyst as desired.
[0189] Specific examples of the Lewis basic compound include the following compounds.
[0190] 1) Ester compounds such as ethyl acetate, butyl acetate, phenyl acetate, methyl propionate, etc.
[0191] 2) Thioester compounds such as methyl mercaptopropionate and ethyl mercaptopropionate;
[0192] 3) Ketone compounds such as methyl ethyl ketone, methyl isobutyl ketone, and benzophenone;
[0193] 4) Amine compounds such as methylamine, ethylamine, propylamine, butylamine, cyclohexylamine, methylethylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine;
[0194] 5) Ether compounds such as diethyl ether and tetrahydrofuran;
[0195] 6) Sulfide compounds such as diethyl sulfide and diphenyl sulfide; and
[0196] 7) Phosphine compounds such as tripropylphosphine, tributylphosphine, trihexylphosphine, tricyclohexylphosphine, trioctylphosphine, vinylphosphine, allylphosphine, cyclohexenylphosphine, dienylphosphine and trialenylphosphine.
[0197] Among these, ester compounds and ketone compounds are preferably used because they act synergistically with a Lewis acid catalyst and can easily control the polymerization rate and the molecular weight distribution of the polymer.
[0198] These Lewis basic compounds may be used alone or in combination of two or more.
[0199] The Lewis basic compound as a cocatalyst component controls the interaction between the carbon cation as an active species and the counter anion by coordinating with the Lewis acid catalyst as the counter anion during the polymerization reaction, thereby adjusting the relative reaction frequency between the cycloolefin compound, the divinyl aromatic compound and the monovinyl aromatic compound that function as a chain transfer agent. Generally, by adding the Lewis basic compound, the interaction between the carbon cation as an active species and the counter anion is enhanced, thereby suppressing the excessive insertion reaction of the divinyl aromatic compound and the monovinyl aromatic compound, facilitating the chain transfer reaction after the insertion reaction of the cycloolefin compound, and making it easy to control the molecular weight.
[0200] The amount of the Lewis basic compound as a cocatalyst is 0.005 mol to 500 mol, preferably 0.01 mol to 100 mol, and more preferably 0.1 mol to 50 mol, relative to 100 mol of the total of all monomers. If it is within the above range, the polymerization rate is appropriately maintained, and at the same time, the selectivity of the reaction between the monomers is improved, and a copolymer with excellent productivity, suppressed excessive increase or decrease in molecular weight, and excellent molding processability can be obtained.
[0201] The polymerization reaction is carried out by dissolving a polymerization raw material including the above-mentioned monomer mixture and a Lewis acid catalyst in a uniform solvent having a dielectric constant of 2.0 to 15.0, and performing cationic copolymerization at a temperature of 20°C to 120°C.
[0202] The solvent is a compound that does not substantially hinder cationic polymerization, and can be an organic solvent that dissolves the catalyst, polymerization additive, cocatalyst, monomer, and the generated vinyl aromatic copolymer to form a uniform solution, and has a dielectric constant in the range of 2.0 to 15.0, and can be used alone or in combination of two or more. If the dielectric constant of the solvent is less than 2.0, the molecular weight distribution becomes broad, which is not preferred, and if the dielectric constant of the solvent exceeds 15.0, the polymerization rate decreases.
[0203] As an organic solvent, toluene, xylene, n-hexane, cyclohexane, methylcyclohexane or ethylcyclohexane are particularly preferred from the viewpoint of the balance between polymerization activity and solubility. In addition, in consideration of the viscosity of the obtained polymerization solution or the ease of heat removal, the amount of the solvent is determined in such a way that the concentration of the copolymer in the polymerization solution becomes 1wt% to 90wt%, preferably 10wt% to 80wt%, and particularly preferably 20wt% to 70wt% at the end of the polymerization. When the concentration is less than 1wt%, the cost increases due to the low polymerization efficiency. If the concentration exceeds 90wt%, the molecular weight and molecular weight distribution increase, resulting in a decrease in molding processability.
[0204] When producing a soluble multifunctional vinyl aromatic polymer, the polymerization needs to be carried out at a temperature of 20° C. to 120° C., preferably 40° C. to 100° C. If the polymerization temperature exceeds 120° C., the selectivity of the reaction decreases, thereby causing problems such as an increase in molecular weight distribution or the generation of gels. If the polymerization is carried out at a temperature below 20° C., the catalyst activity decreases significantly, so a large amount of catalyst needs to be added.
[0205] The method for recovering the copolymer after the polymerization reaction is terminated is not particularly limited, and a commonly used method such as a heating concentration method, a steam stripping method, and precipitation in a poor solvent may be used.
[0206] The multifunctional vinyl aromatic copolymer obtained by the production method contains a structural unit (a) derived from a divinyl aromatic compound, a structural unit (b) derived from a monovinyl aromatic compound, and a structural unit (c) derived from a cycloolefin monomer containing an aromatic condensed ring structure, and at least a part of the structural unit (a) derived from the divinyl aromatic compound is present in the form of a vinyl-containing structural unit (a1) represented by the formula (1). Furthermore, the multifunctional vinyl aromatic copolymer is soluble in toluene, xylene, tetrahydrofuran, dichloroethane or chloroform.
[0207] The multifunctional vinyl aromatic copolymers of the first invention, the second invention, and the third invention have unreacted vinyl groups, and thus can be polymerized, cured, and molded alone, but can also be copolymerized with other polymerizable resins or monomers to form a second copolymer. In particular, the multifunctional vinyl aromatic copolymer of the present invention is excellent because it can be copolymerized with other monomers including conjugated dienes to obtain a conjugated diene-based copolymer (rubber).
[0208] The multifunctional vinyl aromatic copolymer (A) of the present invention as a raw material is copolymerized with 1) a conjugated diene compound (B), or 2) a conjugated diene compound (B) and an aromatic vinyl compound (C) to obtain the conjugated diene copolymer of the present invention. When the aromatic vinyl compound (C) is not used, a diene rubber such as butadiene rubber or isoprene rubber can be obtained, and when the aromatic vinyl compound (C) is used, a conjugated diene copolymer such as SBR can be obtained. The conjugated diene copolymer exhibits the properties of rubber and is therefore also called a copolymer rubber.
[0209] In the polymerization step of obtaining the conjugated diene copolymer, the following methods can be used: a method in which a polyfunctional anionic polymerization initiator is prepared in advance in a predetermined reactor by reacting the polyfunctional vinyl aromatic copolymer (A) of the present invention with an organic lithium compound, and the polyfunctional anionic polymerization initiator is supplied to a reactor for polymerization of the conjugated diene compound to carry out polymerization or copolymerization (method I); a method in which a raw material comprising the polyfunctional vinyl aromatic copolymer (A) and the conjugated diene compound (B), or the polyfunctional vinyl aromatic copolymer (A), the conjugated diene compound (B) and the aromatic vinyl compound (C) is reacted with the organic lithium compound (or the anionic polymerization initiator); ) are supplied in batches to a reactor for copolymerization to carry out copolymerization (method II); and a method for synthesizing a conjugated diene copolymer by supplying a conjugated diene compound (B), or a conjugated diene compound (B) and an aromatic vinyl compound (C) to a specified reactor to polymerize the conjugated diene compound, or to copolymerize the conjugated diene compound and the aromatic vinyl compound, and reacting the polymer of the conjugated diene compound having an active terminal generated in the reactor, or the copolymer of the conjugated diene compound and the aromatic vinyl compound, with the multifunctional vinyl aromatic copolymer (A) (method III), etc.
[0210] Among these polymerization methods, method I is preferred from the viewpoint of efficiency of the copolymerization reaction with the multifunctional vinyl aromatic copolymer (A) of the present invention.
[0211] Examples of the conjugated diene compound (B) include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-heptadiene, and 1,3-hexadiene. Among these, 1,3-butadiene and isoprene are preferred. These may be used alone or in combination of two or more.
[0212] As the aromatic vinyl compound (C), styrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, vinylxylene, 4-cyclohexylstyrene, 2,4,6-trimethylstyrene, tert-butoxydimethylsilylstyrene and isopropoxydimethylsilylstyrene can be used alone or in combination of two or more thereof. Among these, styrene is particularly preferred.
[0213] When 1,3-butadiene is used as the conjugated diene compound (B) and styrene is used as the aromatic vinyl compound, so-called styrene-butadiene rubber (SBR) is obtained. In addition, when styrene is not used as the aromatic vinyl compound, when 1,3-butadiene is used as the conjugated diene compound (B), so-called butadiene rubber (BR) is obtained. When isoprene is used as the conjugated diene compound (B) and there is no structural unit of the aromatic vinyl compound (C), it becomes isoprene rubber (IR). Among them, if it has a styrene-butadiene rubber (SBR) structure, it is particularly preferred because of its excellent wear resistance, heat resistance, and aging resistance.
[0214] The organolithium compound used as the initiator is not particularly limited, and examples thereof include: monoorganolithium compounds such as n-butyllithium, sec-butyllithium, tert-butyllithium, n-propyllithium, isopropyllithium, and benzyllithium; and polyfunctional organolithium compounds such as 1,4-dilithium butane, 1,5-dilithium pentane, 1,6-dilithium hexane, 1,10-dilithium decane, 1,1-dilithium diphenylene, dilithium polybutadiene, dilithium polyisoprene, 1,4-dilithium benzene, 1,2-dilithium-1,2-diphenylethane, 1,4-dilithium-2-ethylcyclohexane, 1,3,5-trilithium benzene, and 1,3,5-trilithium-2,4,6-triethylbenzene. Among these, monoorganolithium compounds such as n-butyllithium, sec-butyllithium, and tert-butyllithium are preferred.
[0215] When producing a conjugated diene copolymer, it is preferred to add the following polar compound as a vinylating agent for controlling the microstructure of the conjugated diene part and for improving the polymerization rate and the like.
[0216] Examples of polar compounds include ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-tetrahydrofuranyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidylethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butoxide, sodium tert-butoxide, and sodium amylate; phosphine compounds such as triphenylphosphine, etc. These polar compounds may be used alone or in combination of two or more.
[0217] The amount of the polar compound used is selected depending on the purpose and effect of the conjugated diene copolymer composition to be obtained, and is preferably 0.005 mol to 100 mol per 1 mol of the organolithium compound as an initiator.
[0218] The conjugated diene copolymer is preferably polymerized in a prescribed solvent. It is particularly preferred to polymerize in a solvent that satisfies the dielectric constant. The solvent is not particularly limited, and hydrocarbon solvents such as saturated hydrocarbons and aromatic hydrocarbons can be used. Specifically, hydrocarbon solvents including aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane; aromatic hydrocarbons such as benzene, toluene, and xylene, and mixtures thereof can be cited.
[0219] Preferably, the conjugated diene compound and the polymerization solvent are treated separately or in a mixed solution thereof using an organometallic compound in advance. Thus, the allenes or acetylenes contained in the conjugated diene compound or the polymerization solvent can be treated. As a result, a polymer having a high concentration of active terminals can be obtained, and a high modification rate can be achieved.
[0220] The polymerization active terminal of the conjugated diene copolymer of the present invention may be further reacted with a modifier. In the present specification, the conjugated diene copolymer obtained by the above reaction is also referred to as a modified conjugated diene copolymer.
[0221] The modifier (also referred to as "terminal modifier") used in the present embodiment uses a compound having a functional group that can react with the polymerization active end of the conjugated diene copolymer. The terminal modifier is not particularly limited. If a monofunctional compound is used, a linear two-end modified diene copolymer can be obtained, and if a polyfunctional compound is used, a branched two-end modified diene copolymer can be obtained. It is preferred to use a monofunctional or polyfunctional compound containing at least one element selected from the group consisting of nitrogen, silicon, tin, phosphorus, oxygen, sulfur, and halogen as the terminal modifier. In addition, a terminal modifier containing an onium generator can be added to react to introduce an onium structure into the modified conjugated diene copolymer. In addition, a terminal modifier containing multiple functional groups containing these elements in the molecule or a terminal modifier containing multiple functional groups containing these elements can also be used. By continuously adding these terminal modifiers, when a molded product such as a tire for a vehicle is produced, a vulcanized rubber composition tends to have lower rolling resistance, excellent wear resistance, and excellent tensile strength and tear strength.
[0222] Various terminal modification agents that can be used in the present invention are described below, but are not limited to the terminal modification agents exemplified above.
[0223] Examples of the nitrogen-containing compound as the terminal modification agent include isocyanate compounds, isothiocyanate compounds, isocyanuric acid derivatives, nitrogen group-containing carbonyl compounds, nitrogen group-containing vinyl compounds, nitrogen group-containing epoxy compounds, and the like.
[0224] Examples of the silicon-containing compound as the terminal modification agent include halogenated silicon compounds, epoxide silicon compounds, vinyl silicon compounds, alkoxy silicon compounds, and alkoxy silicon compounds containing a nitrogen-containing group.
[0225] Examples of tin-containing compounds as terminal modifiers include tin halide compounds, organic tin carboxylate compounds, etc. Examples of phosphorus-containing compounds as terminal modifiers include phosphite compounds, phosphine compounds, etc. Examples of oxygen-containing compounds as terminal modifiers include epoxy compounds, ether compounds, ester compounds, etc. Examples of sulfur-containing compounds as terminal modifiers include mercapto derivatives, thiocarbonyl compounds, isothiocyanates, etc. Examples of halogen-containing compounds as terminal modifiers include the above-mentioned silicon halide compounds, tin halide compounds, etc.
[0226] As the onium generator as the terminal modifier, for example, protected amine compounds (forming ammonium) that can form primary amines or secondary amines; protected phosphine compounds (forming phosphonium) that can form hydrophosphine; compounds that can form hydroxyl groups or thiols (forming onium and sulfonium), etc., it is preferred to use a terminal modifier having a functional group in the molecule for bonding the onium generator to the modified conjugated diene polymer. As the functional group for bonding the modified conjugated diene polymer, for example, carbonyl groups (ketones, esters, etc.), unsaturated groups such as vinyl groups, epoxy groups, halogenated silicon groups, alkoxy silicon groups, etc. can be listed.
[0227] Specific examples of the terminal modifier include isocyanate compounds such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane diisocyanate, polymeric type diphenylmethane diisocyanate (crude 4,4-diphenylmethane diisocyanate (CMDI)), phenyl isocyanate, isophorone diisocyanate, hexamethylene diisocyanate, butyl isocyanate, and 1,3,5-benzene triisocyanate. Examples of the isocyanuric acid derivatives include 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-tris(3-triethoxysilylpropyl)isocyanurate, 1,3,5-tris(oxirane-2-yl)-1,3,5-triazinane-2,4,6-trione, 1,3,5-tris(isothiocyanatomethyl)-1,3,5-triazinane-2,4,6-trione, and 1,3,5-trivinyl-1,3,5-triazinane-2,4,6-trione.
[0228] Specific examples of the nitrogen-containing carbonyl compound include 1,3-dimethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 1-methyl-3-(2-methoxyethyl)-2-imidazolidinone, N-methyl-2-pyrrolidone, N-methyl-2-piperidone, N-methyl-2-quinolone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, methyl-2-pyrrolidone, Pyridyl ketone, methyl-4-pyridyl ketone, propyl-2-pyridyl ketone, di-4-pyridyl ketone, 2-benzoylpyridine, N,N,N',N'-tetramethylurea, N,N-dimethyl-N',N'-diphenylurea, N,N-diethylcarbamic acid methyl ester, N,N-diethylacetamide, N,N-dimethyl-N',N'-dimethylaminoacetamide, N,N-dimethylpicolinic acid amide, N,N-dimethylisonicotinic acid amide, etc.
[0229] Specific examples of the nitrogen-containing vinyl compound include N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methylmaleimide, N-methylphthalimide, N,N-bistrimethylsilylacrylamide, morpholinoacrylamide, 3-(2-dimethylaminoethyl)styrene, (dimethylamino)dimethyl-4-vinylphenylsilane, 4,4'-vinylidenebis(N,N-dimethylaniline), 4,4'-vinylidenebis(N,N-diethylaniline), 1,1-bis(4-morpholinophenyl)ethylene, and 1-phenyl-1-(4-N,N-dimethylaminophenyl)ethylene.
[0230] Specific examples of the nitrogen-containing epoxy compound include N,N,N',N'-tetraglycidyl-1,3-bisaminomethylcyclohexane, N,N,N',N'-tetraglycidyl-m-xylene diamine, 4,4-methylene-bis(N,N-diglycidylaniline), 1,4-bis(N,N-diglycidylamino)cyclohexane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, 4,4'-bis(diglycidylamino)benzophenone, 4-(4-glycidylpiperidinium chloride, 4-(4-glycidylamino) ... oxazine)-(N,N-diglycidyl)aniline, 2-[2-(N,N-diglycidylamino)ethyl]-1-glycidylpyrrolidine, bis(glycidylmethylaniline), N,N'-diglycidyl-4-glycidyloxyaniline, 4,4'-diglycidyl-diphenylmethylamine, 4,4'-diglycidyl-dibenzylmethylamine, N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, N,N-diglycidylaminomethylcyclohexane, and the like.
[0231] Specific examples of the silicon halide compound include dibutyldichlorosilane, methyltrichlorosilane, dimethyldichlorosilane, methyldichlorosilane, trimethylchlorosilane, tetrachlorosilane, tris(trimethylsiloxy)chlorosilane, tris(dimethylamino)chlorosilane, hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,2-bis(methyldichlorosilyl)ethane, 1,4-bis(trichlorosilyl)butane, and 1,4-bis(methyldichlorosilyl)butane.
[0232] Specific examples of the silicon epoxide compound include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, and epoxy-modified silicone.
[0233] Specific examples of the alkoxysilicon compound include tetramethoxysilane, tetraethoxysilane, triphenoxymethylsilane, and methoxy-substituted polyorganosiloxane.
[0234] Specific examples of the alkoxysilicon compound containing a nitrogen-containing group include 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-diethylaminopropyltriethoxysilane, 3-morpholinopropyltrimethoxysilane, 3-piperidinylpropyltriethoxysilane, 3-hexamethyleneiminopropylmethyldiethoxysilane, 3-(4-methyl-1-piperazinyl)propyltriethoxysilane, 1-[3-(triethoxysilyl)-propyl]-3-methylhexahydropyrimidine, 3-(4-trimethylsilyl-1- piperazinyl)propyl triethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 3-dimethylamino-2-(dimethylaminomethyl)propyltrimethoxysilane, bis(3-dimethoxymethylsilylpropyl)-N-methylamine, bis(3-trimethoxysilylpropyl)-N-methylamine, bis(3-triethoxysilylpropyl)methylamine, tris(trimethoxysilyl)amine, tris(3-trimethoxysilylpropyl) )amine, N,N,N',N'-tetrakis(3-trimethoxysilylpropyl)ethylenediamine, 3-isothiocyanatopropyltrimethoxysilane, 3-cyanopropyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(3- dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-8-(4-methylpiperazinyl)methyl-1,6-dioxa-2-silacyclooctane, 2,2-dimethoxy-8-(N,N-diethylamino)methyl-1,6-dioxa-2-silacyclooctane, etc.
[0235] Specific examples of the protected amine compounds that can form primary or secondary amines and have an unsaturated bond and a protected amine in the molecule include: 4,4'-vinylidenebis[N,N-bis(trimethylsilyl)aniline], 4,4'-vinylidenebis[N,N-bis(triethylsilyl)aniline], 4,4'-vinylidenebis[N,N-bis(tert-butyldimethylsilyl)aniline], 4,4'-vinylidenebis[N-methyl-N-(trimethylsilyl)aniline], 4,4'-vinylidenebis[N-ethyl-N-(trimethylsilyl)aniline], 4,4'-vinylidenebis[N- methyl-N-(triethylsilyl)aniline〕, 4,4'-vinylidenebis〔N-ethyl-N-(triethylsilyl)aniline〕, 4,4'-vinylidenebis〔N-methyl-N-(tert-butyldimethylsilyl)aniline〕, 4,4'-vinylidenebis〔N-ethyl-N-(tert-butyldimethylsilyl)aniline〕, 1-〔4-N,N-bis(trimethylsilyl)aminophenyl〕-1-〔4-N-methyl-N-(trimethylsilyl)aminophenyl〕ethylene, 1-〔4-N,N-bis(trimethylsilyl)aminophenyl〕-1-〔4-N,N-dimethylaminophenyl〕ethylene, etc.
[0236] Among the protected amine compounds that can form primary or secondary amines, specific examples of compounds having an alkoxysilane and a protected amine in the molecule include N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane, N,N-bis(triethylsilyl)aminopropylmethyldiethoxysilane, 3-(4-trimethylsilyl-1-piperazinyl)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propyl methyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl) 2,2-Dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, and the like.
[0237] Specific examples of the tin halide compound include tin tetrachloride, tin tetrabromide, butyltin trichloride, octyltin trichloride, dimethyltin dibromide, dibutyltin dichloride, tributyltin chloride, trioctyltin chloride, triphenyltin chloride, 1,2-bis(trichlorostannyl)ethane, 1,2-bis(methyldichlorostannyl)ethane, 1,4-bis(trichlorostannyl)butane, and 1,4-bis(methyldichlorostannyl)butane.
[0238] Specific examples of the organic tin carboxylate compound include ethyltin tristearate, butyltin trioctanoate, butyltin tristearate, butyltin trilaurate, and dibutyltin dioctanoate.
[0239] Specific examples of the phosphite compound include trimethyl phosphite, tributyl phosphite, and triphenyl phosphite oxide.
[0240] Specific examples of the phosphine compound include protected phosphine compounds such as P,P-bis(trimethylsilyl)phosphinopropyltrimethoxysilane and P,P-bis(triethylsilyl)phosphinopropylmethylethoxysilane, 3-dimethylphosphinopropyltrimethoxysilane, and 3-diphenylphosphinopropyltrimethoxysilane.
[0241] Specific examples of oxygen-containing compounds include polyglycidyl ethers such as ethylene glycol diglycidyl ether and glycerol triglycidyl ether; polyepoxy compounds such as 1,4-diglycidyl benzene, 1,3,5-triglycidyl benzene, polyepoxidized liquid polybutadiene, epoxidized soybean oil, and epoxidized linseed oil; and ester compounds such as dimethyl adipate, diethyl adipate, dimethyl terephthalate, and diethyl terephthalate, which generate hydroxyl groups at the ends of the polymers.
[0242] Specific examples of the sulfur-containing compound include protected thiol compounds such as S-trimethylsilylthiopropyltrimethoxysilane, S-triethylsilylthiopropylmethyldiethylsilane, S-methylthiopropyltrimethoxysilane, S-ethylthiopropylmethyldiethoxysilane, N,N-diethyldithiocarbamate, phenyl isothiocyanate, phenyl-1,4-diisothiocyanate, hexamethylene diisothiocyanate, and butyl isothiocyanate.
[0243] The amount of the terminal modifier used is preferably more than 0.5 equivalent and less than 10 equivalents, more preferably more than 0.7 equivalent and less than 5 equivalents, and further preferably more than 1 equivalent and less than 4 equivalents relative to 1 equivalent of the active end of the conjugated diene copolymer. Furthermore, in this embodiment, the amount of the active end of the conjugated diene polymer can be calculated based on the amount of the organolithium compound used in the polymerization and the number of lithium atoms bonded to the organolithium compound, and can also be calculated based on the number average molecular weight of the obtained conjugated diene copolymer.
[0244] The terminal modifying agents may be used alone or in combination of two or more.
[0245] In consideration of processability and physical properties, the weight average molecular weight (in terms of polystyrene) of the conjugated diene copolymer of the present invention is preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,000,000. The weight average molecular weight can be determined by measuring a chromatogram using a gel permeation chromatograph (GPC) using a column filled with a polystyrene gel and by using a calibration curve using standard polystyrene.
[0246] Regarding the composition of the structural unit of the conjugated diene copolymer of the present invention, when no aromatic vinyl compound (C) is used, the ratio of the polyfunctional vinyl aromatic copolymer (A) to the conjugated diene compound (B) is preferably within the following range.
[0247] The content of the structural unit (A1) derived from the multifunctional vinyl aromatic copolymer (A) is 0.001% to 6% by weight, preferably 0.001% to 5% by weight, more preferably 0.005% to 5% by weight, and further preferably 0.01% to 5% by weight. The content of the structural unit (B1) derived from the conjugated diene compound (B) is 29% to 99.999% by weight, preferably 80% to 99.999% by weight, more preferably 90% to 99.995% by weight, and further preferably 95% to 99.99% by weight.
[0248] When an aromatic vinyl compound (C) is used, the ratio is preferably set to the following range. The structural unit (A1) is the same range as above, and the structural unit (B1) is 30% by weight to 97.999% by weight, preferably 45% by weight to 94.995% by weight, and more preferably 55% by weight to 89.99% by weight. The structural unit (C1) derived from the aromatic vinyl compound (C) is 2% by weight to 50% by weight, preferably 5% by weight to 45% by weight, and more preferably 10% by weight to 40% by weight.
[0249] In the case of a modified conjugated diene copolymer, the content of the structural unit (H1) derived from the terminal modifier may be 1 to 0 wt %. When the structural unit (H1) is included, the structural unit (H1) is regarded as an external number and is not included in the calculation of the above ratio.
[0250] The structural unit (A1) imparts a branched structure to the conjugated diene copolymer to increase the molecular weight and / or increase the amount of terminal modifier introduced, thereby improving the physical properties of the conjugated diene copolymer and / or improving the dispersibility of the reinforcing filler.
[0251] The microstructure (cis bond, trans bond, vinyl bond amount) of the conjugated diene copolymer can be arbitrarily changed by using polar compounds, etc., but in the state before the terminal is modified, the content of vinyl bond (1,2-bond) in the conjugated diene unit is preferably 10 mol% to 80 mol%. When the conjugated diene copolymer of the present invention is made into the conjugated diene copolymer composition described later and further cross-linked and used as a tire for automobiles, in order to make the rolling resistance performance and the wear resistance highly balanced, the content is preferably 20 mol% to 75 mol%, more preferably 30 mol% to 75 mol%, and further preferably 40 mol% to 70 mol%. At this time, the mass ratio of cis bond to trans bond in the conjugated diene bond unit is preferably cis bond / trans bond=1 / 1.1 to 1.5.
[0252] A reaction terminator may be added to the polymer solution of the conjugated diene copolymer obtained by the polymerization method as required. Examples of the reaction terminator include alcohols such as methanol, ethanol, and propanol; organic acids such as stearic acid, lauric acid, and caprylic acid; and water.
[0253] After the polymerization reaction of the conjugated diene copolymer is carried out, the metals contained in the polymer may be deashed as needed. As a method for deashing, for example, a method of bringing water, an organic acid, an inorganic acid, an oxidizing agent such as hydrogen peroxide into contact with the polymer solution to extract the metals and then separating the water layer is used.
[0254] Furthermore, an antioxidant may be added to the polymer solution of the conjugated diene copolymer. Examples of the antioxidant include phenol stabilizers, phosphorus stabilizers, and sulfur stabilizers.
[0255] As a method for obtaining a conjugated diene copolymer from a polymer solution, conventional methods can be applied. For example, a method of separating the solvent by steam stripping, filtering and separating the polymer, and then dehydrating and drying the polymer to obtain the polymer; a method of concentrating the polymer by a flashing tank, and then devolatilizing the polymer by a gas extruder; a method of directly devolatilizing the polymer by a drum dryer, etc. can be applied.
[0256] The conjugated diene copolymer composition of the present invention preferably contains 0.5 to 200 parts by mass of at least one reinforcing filler selected from the group consisting of silica-based inorganic fillers, metal oxides, metal hydroxides and carbon black, based on 100 parts by mass of the conjugated diene copolymer.
[0257] As the silica-based inorganic filler contained in the conjugated diene copolymer composition, it is preferred to use solid particles having SiO2 or silicate as the main component of the constituent unit. Here, the so-called main component refers to a component accounting for 50% by mass or more of the whole, preferably a component accounting for 70% by mass or more, and more preferably a component accounting for 90% by mass or more.
[0258] As the specific example of silica-based inorganic filler, it is possible to enumerate inorganic fibrous materials such as silica, clay, talc, mica, diatomaceous earth, wollastonite, montmorillonite, zeolite, glass fiber, etc. The silica-based inorganic filler can be used alone or in combination of two or more. In addition, it is also possible to use a mixture of the silica-based inorganic filler, the silica-based inorganic filler and the inorganic filler other than the silica-based inorganic filler that has been hydrophobized on the surface. Among these, preferably silica and glass fiber, more preferably silica.
[0259] As silica, dry silica, wet silica, synthetic silicate silica and the like can be used. Among these, wet silica is preferred in terms of achieving both improved fracture characteristics and wet skid resistance.
[0260] From the viewpoint of obtaining good wear resistance and fracture characteristics, the nitrogen adsorption specific surface area of the silica-based inorganic filler determined by the Brunauer-Emmett-Teller (BET) adsorption method is preferably 170 m 2 / g~300m 2 / g, more preferably 200m 2 / g~300m 2 / g.
[0261] The amount of the silica-based inorganic filler in the conjugated diene copolymer composition is preferably 0.5 to 200 parts by mass relative to 100 parts by mass of the conjugated diene copolymer as a rubber component. The upper limit of the amount of the silica-based inorganic filler is preferably 100 parts by mass or less, more preferably 75 parts by mass or less. The lower limit is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, and particularly preferably 35 parts by mass or more. If the amount of the silica-based inorganic filler is within the range, the effect of adding the filler is exhibited, and in addition, the dispersibility of the silica-based inorganic filler becomes good, the processability of the obtained composition is improved, and the mechanical strength is improved.
[0262] Carbon black may be added to the conjugated diene copolymer composition as a reinforcing filler other than the silica-based inorganic filler.
[0263] As carbon black, various types of carbon black such as semi-reinforcing furnace (SRF), fast extrusion furnace (FEF), high abrasion furnace (HAF), intermediate super abrasion furnace (ISAF), and super abrasion furnace (SAF) can be used. From the viewpoint of excellent reinforcing effect, a carbon black having a nitrogen adsorption specific surface area of 50 m 2 / g or more, and carbon black having a dibutyl phthalate (DBP) oil absorption of 80mL / 100g.
[0264] The amount of carbon black added is 0.5 to 200 parts by mass, preferably 3 to 100 parts by mass, and more preferably 5 to 50 parts by mass, based on 100 parts by mass of the conjugated diene copolymer.
[0265] In the conjugated diene copolymer composition, not only a silica-based inorganic filler or carbon black but also a metal oxide or metal hydroxide as a reinforcing filler may be added. The metal oxide is preferably a solid particle having a chemical formula MxOy (M represents a metal atom, and x and y represent integers of 1 to 6, respectively) as the main component. Here, the so-called main component refers to a component accounting for 50% or more of the whole, preferably a component accounting for 70% or more of the mass, and more preferably a component accounting for 90% or more of the mass.
[0266] As the metal oxide, for example, aluminum oxide, titanium oxide, magnesium oxide, zinc oxide, etc. can be used. As the metal hydroxide, for example, aluminum hydroxide, magnesium hydroxide, zirconium hydroxide, etc. can be listed. The metal oxide and the metal hydroxide can be used alone or in combination of two or more. In addition, a mixture with an inorganic filler other than the metal oxide and the metal hydroxide can also be used.
[0267] The conjugated diene copolymer composition may contain a silane coupling agent. The silane coupling agent has a function of strengthening the interaction between the conjugated diene copolymer and the silica inorganic filler, and has a group having affinity or bonding properties with the conjugated diene copolymer and the silica inorganic filler, respectively.
[0268] Specific examples of the silane coupling agent include bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, and bis-[2-(triethoxysilyl)-ethyl]-tetrasulfide.
[0269] The amount of the silane coupling agent to be added is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, and still more preferably 1 to 15 parts by mass, relative to 100 parts by mass of the silica-based inorganic filler. By setting the amount of the silane coupling agent to be added within the above numerical range, a sufficient mixing effect can be obtained and economic efficiency can be improved.
[0270] The conjugated diene-based copolymer composition can be produced by mixing the above-mentioned components.
[0271] There is no particular limitation on the method of mixing the conjugated diene copolymer with at least one reinforcing filler selected from the group consisting of a silica-based inorganic filler, a metal oxide, a metal hydroxide and carbon black, and a desired silane coupling agent. For example, there can be cited: a melt kneading method using a general mixer such as an open roll, a Banbury mixer, a kneader, a single-axis screw extruder, a twin-axis screw extruder, and a multi-axis screw extruder; a method of melting and mixing each component and then heating to remove the solvent, etc. Among these, from the perspective of productivity and good kneading properties, a melt kneading method using a roll, a Banbury mixer, a kneader, and an extruder is preferred. In addition, any method of a method of kneading the rubber component with various formulations at one time or a method of mixing in multiple times can be applied.
[0272] In the present invention, the degree of polymer concentration ability on the filler surface can be represented by the bound rubber amount of the modified conjugated diene polymer at 25° C. From the viewpoint of improving wear resistance and breaking strength, the bound rubber amount in the conjugated diene copolymer composition (rubber composition) after kneading is preferably 15% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more.
[0273] The bound rubber amount can be measured by the method described in Examples below.
[0274] The conjugated diene copolymer composition can be formed into a vulcanized composition subjected to vulcanization treatment using a vulcanizing agent. As the vulcanizing agent, for example, free radical generators such as organic peroxides and azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, and sulfur compounds can be used. Sulfur compounds include sulfur monochloride, sulfur dichloride, disulfide compounds, high molecular weight polysulfide compounds, etc.
[0275] The amount of the vulcanizing agent used is not particularly limited, but is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the conjugated diene copolymer. As a vulcanization method, any existing method can be applied, and the vulcanization temperature is, for example, preferably 120°C to 200°C, more preferably 140°C to 180°C.
[0276] During vulcanization, a vulcanization accelerator may be used as necessary. As the vulcanization accelerator, conventional materials may be used, for example, sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, dithiocarbamate-based vulcanization accelerators may be mentioned. As the vulcanization aid, zinc white, stearic acid, etc. may be used.
[0277] The amount of the vulcanization accelerator used is not particularly limited, but is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, based on 100 parts by mass of the conjugated diene copolymer.
[0278] The conjugated diene copolymer composition of the present invention may contain a rubber softener in order to improve processability. The rubber softener is preferably a mineral oil, a liquid or a low molecular weight synthetic softener.
[0279] The mineral oil-based rubber softener called process oil or extender oil used to soften, increase volume, and improve processability of rubber is a mixture of aromatic rings, cycloalkane rings, and paraffin chains. The carbon number of the paraffin chain accounts for more than 50% of all carbons and is called a paraffin series, the carbon number of the cycloalkane ring is 30% to 45% and the aromatic carbon number is more than 30%. The rubber softener used in this embodiment is preferably a cycloalkane-based and / or paraffin-based rubber softener.
[0280] The amount of the rubber softener to be added is not particularly limited, but is preferably 10 to 80 parts by mass, more preferably 20 to 50 parts by mass, based on 100 parts by mass of the conjugated diene copolymer.
[0281] In the conjugated diene copolymer composition, various additives such as softeners or fillers other than those mentioned above, as well as heat stabilizers, antistatic agents, weather stabilizers, anti-aging agents, colorants, lubricants, etc. can be used within the scope that does not impair the purpose of the present embodiment. As fillers, specifically, calcium carbonate, magnesium carbonate, aluminum sulfate, barium sulfate, etc. can be cited.
[0282] As a softener which is mixed as needed to adjust the hardness or fluidity of the target product, for example, liquid paraffin, castor oil, linseed oil, etc. As a heat stabilizer, antistatic agent, weather stabilizer, anti-aging agent, colorant, lubricant, existing materials can be used.
[0283] The cross-linked rubber product of the present invention is obtained by cross-linking the rubber composition. For example, in the case of a tire, the rubber composition can be extruded and formed according to the shape of the tire (specifically, the shape of the tread), and heated and pressurized in a vulcanizer to manufacture the tread, and the target tire can be manufactured by assembling the tread with other parts.
[0284] The conjugated diene copolymer composition (rubber composition) of the present invention has excellent mechanical strength and wear resistance when it is made into the rubber cross-linked product. Therefore, as mentioned above, it can be suitably applied to tire components such as the tread or outer tire side member of tires such as low fuel consumption tires, large tires, and high-performance tires. In addition, it can be not only applicable to the tire components, but also suitably used in rubber belts, rubber hoses, materials for footwear, etc.
[0285] Example
[0286] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. In addition, parts in each example are parts by weight unless otherwise specified, and evaluation of various physical properties was performed by the methods shown below.
[0287] 1) Molecular weight and molecular weight distribution
[0288] The molecular weight and molecular weight distribution were measured using GPC (HLC-8220GPC manufactured by Tosoh Corporation) with tetrahydrofuran (THF) as a solvent, at a flow rate of 1.0 ml / min, a column temperature of 38° C., and a calibration curve obtained using monodisperse polystyrene.
[0289] 2) Structure of multifunctional vinyl aromatic copolymer
[0290] The JNM-LA600 nuclear magnetic resonance spectrometer manufactured by JEOL was used. 13 C-NMR (Nuclear Magnetic Resonance, NMR) and 1 The determination was made by H-NMR analysis using chloroform-d1 as a solvent and the resonance line of tetramethylsilane as an internal standard.
[0291] 3) Mooney viscosity (ML(1+4)100℃)
[0292] The value was determined in accordance with Japanese Industrial Standards (JIS) K6300-1, with an L-shaped rotor, 1 minute preheating, 4 minutes rotor operation time, and a temperature of 100°C.
[0293] 4) Confirmation of microgel (haze)
[0294] A sample prepared by dissolving 0.5 g of copolymer rubber in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) was measured using an integrating sphere light transmittance measuring device (SZ-Σ90 manufactured by Nippon Denshoku Co., Ltd.) with toluene as the reference sample.
[0295] When the haze value was less than 0.5, it was determined as no microgel: ○, and when the haze value exceeded 0.5, it was determined as the presence of microgel: ×.
[0296] 5) Glass transition temperature (Tg)
[0297] The solution obtained by dissolving the polyfunctional vinyl aromatic copolymer in toluene is uniformly coated on a glass substrate in such a manner that the thickness after drying becomes 20 μm, and a hot plate is used to heat at 90° C. for 30 minutes to be dried. The glass substrate is placed in a thermomechanical analyzer (TMA) (thermomechanical analysis device) together with the obtained resin film, and the temperature is increased to 220° C. at a heating rate of 10° C. / min under a nitrogen gas flow, and then heat-treated at 220° C. for 20 minutes to remove the residual solvent, and the polyfunctional vinyl aromatic copolymer is hardened. After the glass substrate is placed and cooled to room temperature, the analysis probe is contacted with the sample in the TMA measuring device, and the scanning measurement is performed from 30° C. to 360° C. at a heating rate of 10° C. / min under a nitrogen gas flow, and the softening temperature is obtained by the tangent method.
[0298] 6) Vinyl bond content of conjugated diene units
[0299] The sample was made into a carbon disulfide solution and the solution was heated at 600 cm -1 ~1000cm -1 The infrared spectrum was measured within a range of , and the amount of vinyl bonds was determined using the absorbance at a predetermined wave number according to the calculation formula of the Hampton (styrene-butadiene copolymer) method. The apparatus used was Spectrum 100 manufactured by Parkin Elmer.
[0300] 7) Combined rubber content (%)
[0301] Using a closed kneading apparatus with a kneading chamber volume of 2 liters, 100 parts by mass of the modified conjugated diene polymer and 60 parts by mass of wet silica (BET specific surface area: 205±10 m 2 / g, manufactured by Tosoh Silica Co., Ltd., trade name "Nipsil AQ") was kneaded, and when the maximum kneading temperature reached 160°C, the rubber kneaded product was discharged to obtain a rubber composition M for measuring the bound rubber amount.
[0302] 0.2 g of the rubber composition M was cut into 1 mm squares and the mass was measured, then added to 25 mL of toluene and allowed to stand at 25° C. for 48 hours. The mixture was filtered using a glass fiber filter manufactured by ADVANTEC to separate the toluene-insoluble components. The separated toluene-insoluble components were then vacuum dried at 25° C. and weighed, and the bound rubber amount was calculated using the following formula.
[0303] Bound rubber amount (%) = {(mass of toluene insoluble components - mass of wet silica in rubber composition M) / (mass of rubber composition M - mass of wet silica in rubber composition M)} × 100
[0304] The BET specific surface area of silica is measured in accordance with International Organization for Standardization (ISO) 5794 / 1.
[0305] 8) Tensile strength
[0306] The 300% modulus was measured by the tensile test method of JIS K6251.
[0307] In the first invention, the measured value of the cross-linked rubber obtained in Comparative Example 8A was set to 100 for indexing.
[0308] In the second invention, the measured value of the cross-linked rubber obtained in Example 20B was set to 100 for indexing.
[0309] In the third invention, the measured value of the cross-linked rubber obtained in Example 10C was set to 100 for indexing.
[0310] A larger index value indicates better tensile strength.
[0311] 9) Wear resistance
[0312] The wear amount at a slip ratio of 30% was measured by a method using a Lambourn type wear tester in accordance with JIS K6264.
[0313] In the first invention, the measured value of the cross-linked rubber obtained in Comparative Example 8A was set to 100 for indexing.
[0314] In the second invention, the measured value of the cross-linked rubber obtained in Example 20B was set to 100 for indexing.
[0315] In the third invention, the measured value of the cross-linked rubber obtained in Example 10C was set to 100 for indexing.
[0316] The larger the index value, the better the wear resistance.
[0317] 10) Solvent solubility
[0318] The copolymer was soluble in toluene, xylene, THF, dichloroethane, dichloromethane and chloroform, and the case where 100 g or more of the copolymer was dissolved in 100 g of each of the above solvents and no formation of gel was observed was regarded as solvent solubility (○).
[0319] The raw materials or their abbreviations used in the examples are as follows.
[0320] DVB-630: a mixture of divinylbenzene and ethylvinylbenzene; divinylbenzene content: 63.0 wt%, manufactured by NIPPON STEEL Chemical & Material
[0321] Indene: Manufactured by Wako Pure Chemical Industries, Ltd.
[0322] BHT (Butylated hydroxytoluene): 2,6-di-tert-butyl-p-cresol
[0323] BTESPA: Bis(3-trimethoxysilylpropyl)methylamine
[0324] <Example of the first invention>
[0325] Example 1A
[0326] 92.98 g of DVB-630 (divinylbenzene component 0.45 mol, ethylvinylbenzene component 0.26 mol), 276.58 g (2.29 mol) of indene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 60 mmol of boron trifluoride diethyl ether complex (7.5 mL) was added at 70° C., and the reaction was carried out for 2.5 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and it was confirmed that 221.7 g of copolymer 1A was obtained.
[0327] In the examples and comparative examples, the obtained copolymers are soluble multifunctional vinyl aromatic copolymers.
[0328] The obtained multifunctional vinyl aromatic copolymer 1A had an Mn of 828, an Mw of 2620, and an Mw / Mn of 3.17. 13 C-NMR and 1According to H-NMR analysis, the polyfunctional vinyl aromatic copolymer 1A contained 13.8 mol% (15.1 wt%) of structural units derived from divinylbenzene, 7.9 mol% (8.8 wt%) of structural units derived from ethylvinylbenzene, and 78.2 mol% (76.1 wt%) of structural units derived from indene. The structural units derived from divinylbenzene having residual vinyl groups contained in the polyfunctional vinyl aromatic copolymer 1A (corresponding to structural unit (a1)) accounted for 11.0 mol% (12.1 wt%).
[0329] The TMA measurement result of the cured product showed Tg: 182° C. and a softening temperature of 280° C. or higher. The thermogravimetric analysis (TGA) measurement result showed a weight loss of 1.52 wt % at 350° C. On the other hand, the compatibility with the epoxy resin was good (○).
[0330] The polyfunctional vinyl aromatic copolymer 1A is solvent-soluble (○).
[0331] Example 2A
[0332] 187.11 g of DVB-630 (divinylbenzene component 0.90 mol, ethylvinylbenzene component 0.53 mol), 182.37 g (1.57 mol) of indene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 40 mmol of boron trifluoride diethyl ether complex (5.0 mL) was added at 70° C., and the reaction was carried out for 3.5 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, degassing was performed under reduced pressure at 60° C., and reprecipitation was performed with 4,500 mL of methanol under strong stirring, filtration, and drying to recover the multifunctional vinyl aromatic copolymer. The obtained multifunctional vinyl aromatic copolymer was weighed, and 238.7 g of the multifunctional vinyl aromatic copolymer 2A was confirmed.
[0333] The obtained multifunctional vinyl aromatic copolymer 2A had an Mn of 1240, an Mw of 3580, and an Mw / Mn of 2.89. Copolymer 2A contained 29.6 mol% (31.3 wt%) of structural units derived from divinylbenzene, a total of 17.9 mol% (19.2 wt%) of structural units derived from ethylvinylbenzene, and 52.5 mol% (49.5 wt%) of structural units derived from indene. The content of structural units derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer 2A was 19.5 mol% (20.6 wt%).
[0334] The Tg of the cured product was 205° C. and the softening temperature was 280° C. or higher. The weight loss at 350° C. was 0.96 wt % as measured by thermogravimetric analysis (TGA). On the other hand, the compatibility with the epoxy resin was ○.
[0335] The polyfunctional vinyl aromatic copolymer 2A is solvent-soluble (○).
[0336] Example 3A
[0337] 31.16 g of DVB-630 (divinylbenzene component 0.15 mol, ethylvinylbenzene component 0.09 mol), 320.83 g (2.76 mol) of indene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, and 80 mmol of boron trifluoride diethyl ether complex (10.0 mL) was added at 70° C., and the reaction was carried out for 3.0 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, degassing was carried out under reduced pressure at 60° C., and reprecipitation was carried out with 4,500 mL of methanol under strong stirring, filtration, and drying to recover the multifunctional vinyl aromatic copolymer. The obtained multifunctional vinyl aromatic copolymer was weighed, and it was confirmed that 256.3 g of multifunctional vinyl aromatic copolymer 3A was obtained.
[0338] The obtained multifunctional vinyl aromatic copolymer 3A had an Mn of 659, an Mw of 2560, and an Mw / Mn of 3.88. The copolymer 3A contained 5.1 mol% (5.8 wt%) of structural units derived from divinylbenzene, a total of 2.9 mol% (3.3 wt%) of structural units derived from ethylvinylbenzene, and 92.0 mol% (90.9 wt%) of structural units derived from indene. The content of structural units derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer 3A was 3.3 mol% (3.8 wt%).
[0339] The Tg of the cured product was 192° C. and the softening temperature was 280° C. or higher. The weight loss at 350° C. was 1.63 wt % as a result of TGA measurement. On the other hand, the compatibility with the epoxy resin was ○.
[0340] The multifunctional vinyl aromatic copolymer 3A is solvent-soluble (○).
[0341] Comparative Example 1A
[0342] 249.41 g of DVB-630 (1.20 mol of divinylbenzene component, 0.70 mol of ethylvinylbenzene component), 127.20 g (1.10 mol) of indene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 40 mmol of boron trifluoride diethyl ether complex (5.0 mL) was added at 70° C., and the reaction was carried out for 3.0 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, degassing was carried out under reduced pressure at 60° C., and reprecipitation was carried out with 4,500 mL of methanol under strong stirring, filtration, and drying to recover the multifunctional vinyl aromatic copolymer. The obtained multifunctional vinyl aromatic copolymer was weighed, and 253.6 g of the multifunctional vinyl aromatic copolymer C1A was confirmed to be obtained.
[0343] The obtained multifunctional vinyl aromatic copolymer C1A has an Mn of 1430, an Mw of 5030, and an Mw / Mn of 3.52. The copolymer C1A contains 40.2 mol% (41.6 wt%) of structural units derived from divinylbenzene, a total of 23.6 mol% (25.0 wt%) of structural units derived from ethylvinylbenzene, and 36.2 mol% (33.4 wt%) of structural units derived from indene. The content of structural units derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer C1A is 26.5 mol% (27.4 wt%).
[0344] The Tg of the cured product was 168° C. and the softening temperature was 280° C. or higher. The weight loss at 350° C. was 2.13 wt % as a result of TGA measurement. On the other hand, the compatibility with the epoxy resin was ○.
[0345] The polyfunctional vinyl aromatic copolymer C1A is solvent-soluble (○).
[0346] Comparative Example 2A
[0347] 12.46 g of DVB-630 (divinylbenzene component 0.06 mol, ethylvinylbenzene component 0.04 mol), 337.44 g (2.90 mol) of indene, 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 80 mmol of boron trifluoride diethyl ether complex (10.0 mL) was added at 70°C, and the reaction was carried out for 4.5 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, degassing was carried out under reduced pressure at 60°C, and reprecipitation was carried out with 4,500 mL of methanol under strong stirring, filtration, and drying to recover the multifunctional vinyl aromatic copolymer. The obtained multifunctional vinyl aromatic copolymer was weighed, and 212.6 g of the multifunctional vinyl aromatic copolymer C2A was confirmed to be obtained.
[0348] The obtained multifunctional vinyl aromatic copolymer C2A has an Mn of 596, an Mw of 1750, and an Mw / Mn of 2.93. The copolymer C2A contains 1.96 mol% (2.19 wt%) of structural units derived from divinylbenzene, a total of 1.16 mol% (1.32 wt%) of structural units derived from ethylvinylbenzene, and 96.88 mol% (96.49 wt%) of structural units derived from indene. The content of structural units derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer C2A is 1.30 mol% (1.45 wt%).
[0349] The results of TMA measurement of the cured product showed that Tg was 178° C. and the softening temperature was 201° C. The results of TGA measurement showed that the weight loss at 350° C. was 2.45 wt %. On the other hand, the compatibility with the epoxy resin was ○.
[0350] The multifunctional vinyl aromatic copolymer C2A is solvent-soluble (○).
[0351] Comparative Example 3A
[0352] 320.5 mL of DVB-810 (1.82 mol of divinylbenzene component, 0.43 mol of ethylvinylbenzene component), 0.28 mol (36.9 mL) of n-butyl acetate, and 140 mL of toluene were placed in a 1.0 L reactor, and a solution prepared by dissolving 40 mmol of methanesulfonic acid in 0.12 mol (15.7 mL) of n-butyl acetate was added at 70° C., and the reaction was carried out for 6 hours. After the polymerization was stopped by potassium hydroxide, activated alumina was used as a filter aid for filtration. Thereafter, the mixture was devolatilized under reduced pressure at 60° C. to obtain 22.6 g of a multifunctional vinyl aromatic copolymer C3A.
[0353] The obtained multifunctional vinyl aromatic copolymer C3A has an Mn of 1085, an Mw of 12400, and an Mw / Mn of 11.4. The multifunctional vinyl aromatic copolymer C3A contains 84.0 mol% (83.8 wt%) of structural units derived from divinylbenzene and a total of 16.0 mol% (16.2 wt%) of structural units derived from ethylvinylbenzene. The content of structural units derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer C3A is 53.8 mol% (53.6 wt%).
[0354] The Tg of the cured product was 82° C. and the softening temperature was 93° C. The weight loss at 350° C. as a result of TGA measurement was 8.25 wt %. On the other hand, the compatibility with the epoxy resin was ○.
[0355] The multifunctional vinyl aromatic copolymer C3A is solvent-soluble (○).
[0356] Example 4A
[0357] In a nitrogen-purged autoclave reactor with an internal volume of 0.5 liters, 245 g of cyclohexane, 2.5 g of THF, 10 g of styrene, 40 g of 1,3-butadiene, and 0.10 g of the copolymer 1A obtained in Example 1A were added. At 25° C., 5 g of a cyclohexane solution containing 50 mg of sec-butyl lithium was added to start polymerization. The temperature of the reaction solution rose due to the polymerization heat, and the maximum temperature reached 85° C.
[0358] After confirming that the polymerization conversion rate reached 99%, 50 mg of isopropanol was added to stop the polymerization, and 2,6-di-tert-butyl-p-cresol (BHT) was added to the reaction solution. Then, the solvent was removed by steam stripping to obtain conjugated diene copolymer 4A. The physical properties of the obtained conjugated diene copolymer 4A are shown in Table 1A.
[0359] Example 5A
[0360] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.10 g of the copolymer 1A obtained in Example 1A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 85°C.
[0361] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain conjugated diene copolymer 5A. The physical properties of the obtained conjugated diene copolymer 5A are shown in Table 1A.
[0362] Example 6A
[0363] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and 45 g of a cyclohexane solution containing 0.050 g of the copolymer 2A obtained in Example 2A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator can be dissolved in cyclohexane, and no gel is observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0364] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain conjugated diene copolymer 6A. The physical properties of the obtained conjugated diene copolymer 6A are shown in Table 1A.
[0365] Example 7A
[0366] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.30 g of the copolymer 3A obtained in Example 3A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0367] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 7A. The physical properties of the obtained conjugated diene copolymer 7A are shown in Table 1A.
[0368] Comparative Example 4A
[0369] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.0375 g of the copolymer C1A obtained in Comparative Example 1A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was generally soluble in cyclohexane, but the formation of gel was also observed visually. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 82°C.
[0370] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C4A. The physical properties of the obtained conjugated diene copolymer C4A are shown in Table 1A.
[0371] Comparative Example 5A
[0372] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.75 g of the copolymer C2A obtained in Comparative Example 2A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 78°C.
[0373] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C5A. The physical properties of the obtained conjugated diene copolymer C5A are shown in Table 1A.
[0374] Comparative Example 6A
[0375] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.020 g of the copolymer C3A obtained in Comparative Example 3A was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the generation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0376] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C6A. The physical properties of the obtained conjugated diene copolymer C6A are shown in Table 1A.
[0377] In Table 1A, the diene copolymer means a conjugated diene copolymer. The same is true in other tables.
[0378] [Table 1A]
[0379]
[0380] Example 8A
[0381] The conjugated diene copolymer 4A, process oil, carbon black, zinc oxide, stearic acid and antioxidant were kneaded using a Labo Plastomill at 155° C. and 60 rpm for 4 minutes.
[0382] Sulfur and a vulcanization accelerator were added to the kneaded product obtained by the kneading, and the mixture was kneaded at 70° C. and 60 rpm for 1 minute for vulcanization to obtain a crosslinked rubber 8A.
[0383] The blending ratio of each additive is shown in Table 2A. In addition, the physical properties of the crosslinked rubber 8A are shown in Table 3A.
[0384] Example 9A to Example 11A, Comparative Example 7A to Comparative Example 9A
[0385] Cross-linked rubbers 9A to 11A and cross-linked rubbers C7A to C9A were obtained by the same method as in Example 8A, except that the conjugated diene copolymers 5A, 6A, 7A, C4A, C5A and C6A synthesized in the examples or comparative examples were used instead of the conjugated diene copolymer 4A.
[0386] The types of the conjugated diene copolymers used and the physical properties of the obtained cross-linked rubbers 9A to 11A and C7A to C9A are shown in Table 3A.
[0387] [Table 2A]
[0388] Copolymer rubber 100.0 Process oil 37.5 Zinc Oxide 3.0 sulfur 1.8 Stearic acid 1.0 Silicon dioxide 65.0 Carbon Black 5.0 Vulcanization accelerator 1.5 Anti-aging agents 1.0
[0389] In addition, in Table 2A, the additives used are as follows.
[0390] Process oil: Diana process oil AC-12 manufactured by Idemitsu Kosan
[0391] Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry
[0392] Zinc oxide: Zinc White No. 1 manufactured by Mitsui Mining and Smelting
[0393] Stearic acid: Made in NOF Corporation
[0394] Silicon dioxide: Degussa, ULTRASIL VN3
[0395] Carbon black: Nitrotron #300 manufactured by NIPPON STEEL Carbon
[0396] Vulcanization accelerator: N-tert-butylbenzothiazole-2-sulfenamide
[0397] Anti-aging agent: Nocceler-NS manufactured by Ouchi Shinko Chemical Industry
[0398] [Table 3A]
[0399] Conjugated diene copolymer Cross-linked rubber Tensile strength index Wear resistance index Example 8A 4A 8A 107 106 Example 9A 5A 9A 109 108 Example 10A 6A 10A 116 117 Example 11A 7A 11A 115 118 Comparative Example 7A C4A C7A 102 91 Comparative Example 8A C5A C8A 100 100 Comparative Example 9A C6A C9A 101 87
[0400] In Table 3A, the tensile strength index and the abrasion resistance index are obtained by setting the values of the cross-linked rubber of Comparative Example 8A to 100. As can be seen from Table 3A, the cross-linked rubber of the present invention using the multifunctional vinyl aromatic copolymer of the present invention imparts processability equal to or better than that of the case using divinylbenzene as a conventional branching agent, and in the vulcanized rubber blended with carbon black, the tensile strength and abrasion resistance are excellent.
[0401] <Example of the second invention>
[0402] Example 1B
[0403] 9.30 g of DVB-630 (divinylbenzene component 0.045 mol, ethylvinylbenzene component 0.026 mol), 148.79 g (1.43 mol) of styrene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, and 200 mmol of boron trifluoride diethyl ether complex (25.1 mL) was added at 50° C., and the reaction was carried out for 2.5 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 90.1 g of a multifunctional vinyl aromatic copolymer 1B.
[0404] The obtained multifunctional vinyl aromatic copolymer 1B had an Mn of 4140, an Mw of 9550, and an Mw / Mn of 2.31. 13 C-NMR and 1 H-NMR analysis showed that the multifunctional vinyl aromatic copolymer 1B contained 3.0 mol% (3.7 wt%) of structural units derived from divinylbenzene, 1.4 mol% (1.8 wt%) of structural units derived from ethylvinylbenzene, and 95.5 mol% (94.5 wt%) of structural units derived from styrene. The crosslinking structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) was 0.24 mol% (0.30 wt%), so the degree of crosslinking was 0.08. In addition, the structural unit (a1) derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer 1B was 2.76 mol% (3.40 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a) and (b) was 0.028.
[0405] The result of TMA measurement of the cured product was Tg: 105°C and the softening temperature was 128°C.
[0406] The result of TGA measurement was 1.36 wt % at 350° C. A sample prepared by dissolving 0.5 g of the polyfunctional vinyl aromatic copolymer 1B in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.00.
[0407] Example 2B
[0408] 18.60 g of DVB-630 (divinylbenzene component 0.090 mol, ethylvinylbenzene component 0.053 mol), 141.34 g (1.36 mol) of styrene, and 1.00 mol (115.0 mL) of n-propyl acetate were placed in a 1.0 L reactor, 50 mmol of boron trifluoride diethyl ether complex (6.1 mL) was added at 60° C., and the reaction was carried out for 3.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 95.8 g of a multifunctional vinyl aromatic copolymer 2B.
[0409] The multifunctional vinyl aromatic copolymer 2B has an Mn of 2620, an Mw of 11800, and an Mw / Mn of 4.51, and contains 7.37 mol% (8.97 wt%) of structural units derived from divinylbenzene, 3.34 mol% (4.12 wt%) of structural units derived from ethylvinylbenzene, and 89.3 mol% (86.9 wt%) of structural units derived from styrene. The crosslinking structural unit (a2) is 1.55 mol% (1.82 wt%), the crosslinking degree is 0.21, the vinyl-containing structural unit (a1) is 5.82 mol% (7.15 wt%), and the molar fraction of the structural unit (a1) is 0.058.
[0410] The Tg of the cured product was 158° C. and the softening temperature was 265° C. The weight loss at 350° C. was 1.28 wt %.
[0411] The haze value of the multifunctional vinyl aromatic copolymer 2B was 0.01.
[0412] Example 3B
[0413] 31.00 g of DVB-630 (divinylbenzene component 0.150 mol, ethylvinylbenzene component 0.088 mol), 131.43 g (1.262 mol) of styrene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 60 mmol of boron trifluoride diethyl ether complex (7.5 mL) was added at 55° C., and the reaction was carried out for 5.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 96.3 g of a multifunctional vinyl aromatic copolymer 3B.
[0414] The multifunctional vinyl aromatic copolymer 3B has an Mn of 2950, an Mw of 13400, and an Mw / Mn of 4.54. It contains 11.63 mol% (13.91 wt%) of structural units derived from divinylbenzene, a total of 5.87 mol% (7.13 wt%) of structural units derived from ethylvinylbenzene, and 82.50 mol% (78.96 wt%) of structural units derived from styrene. The crosslinked structural unit (a2) is 3.14 mol% (3.76 wt%), and the degree of crosslinking is 0.27. In addition, the structural unit (a1) is 8.49 mol% (10.16 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.085.
[0415] The Tg of the cured product was 165°C, the softening temperature was 280°C or higher, and the weight loss at 350°C was 1.46 wt%.
[0416] The haze value of the multifunctional vinyl aromatic copolymer 3B was 0.04.
[0417] Example 4B
[0418] 46.49 g of DVB-630 (divinylbenzene component 0.225 mol, ethylvinylbenzene component 0.132 mol), 119.03 g (1.143 mol) of styrene, and 1.50 mol (172.5 mL) of n-propyl acetate were placed in a 1.0 L reactor, 60 mmol of boron trifluoride diethyl ether complex (7.54 mL) was added at 50° C., and the reaction was carried out for 3.5 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 96.10 g of a multifunctional vinyl aromatic copolymer 4B.
[0419] The multifunctional vinyl aromatic copolymer 4B has an Mn of 3870, an Mw of 23600, and an Mw / Mn of 6.10. It contains 20.64 mol% (23.98 wt%) of structural units derived from divinylbenzene, 9.09 mol% (10.72 wt%) of structural units derived from ethylvinylbenzene, and 70.27 mol% (65.30 wt%) of structural units derived from styrene. The crosslinking structural unit (a2) is 6.61 mol% (7.67 wt%), the degree of crosslinking is 0.32, the vinyl-containing structural unit (a1) is 14.04 mol% (16.31 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.140.
[0420] The Tg of the cured product was 178°C, the softening temperature was 280°C or higher, and the weight loss at 350°C was 1.53 wt%.
[0421] The haze value of the multifunctional vinyl aromatic copolymer 4B was 0.07.
[0422] Example 5B
[0423] 77.49 g of DVB-630 (divinylbenzene component 0.375 mol, ethylvinylbenzene component 0.220 mol), 94.23 g (0.905 mol) of styrene, and 1.57 mol (180.2 mL) of n-propyl acetate were placed in a 1.0 L reactor, and 23.3 mmol of boron trifluoride diethyl ether complex (2.93 mL) was added at 50° C., and the reaction was carried out for 5.25 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 76.19 g of a multifunctional vinyl aromatic copolymer 5B.
[0424] The multifunctional vinyl aromatic copolymer 5B had an Mn of 4230, an Mw of 26200, and an Mw / Mn of 6.19, and contained 39.29 mol% (43.12 wt%) of structural units derived from divinylbenzene, 15.08 mol% (16.81 wt%) of structural units derived from ethylvinylbenzene, and 45.63 mol% (40.07 wt%) of structural units derived from styrene.
[0425] The cross-linked structural unit (a2) is 16.89 mol% (18.54 wt%), the cross-linking degree is 0.43, the vinyl-containing structural unit (a1) is 22.39 mol% (24.58 wt%), and the molar fraction of the structural unit (a1) is 0.224.
[0426] The cured product had no Tg, had a softening temperature of 280°C or higher, and had a weight loss of 1.61 wt% at 350°C.
[0427] The haze value of the multifunctional vinyl aromatic copolymer 5B was 0.09.
[0428] Comparative Example 1B
[0429] 320.5 mL of DVB-810 (1.82 mol of divinylbenzene component, 0.43 mol of ethylvinylbenzene component), 0.28 mol (36.9 mL) of n-butyl acetate, and 140 mL of toluene were placed in a 1.0 L reactor, and a solution prepared by dissolving 40 mmol of methanesulfonic acid in 0.12 mol (15.7 mL) of n-butyl acetate was added at 70° C., and the reaction was carried out for 6 hours. After the polymerization was stopped by potassium hydroxide, activated alumina was used as a filter aid for filtration. Thereafter, the mixture was devolatilized under reduced pressure at 60° C. to obtain 22.6 g of a multifunctional vinyl aromatic copolymer C1B.
[0430] The multifunctional vinyl aromatic copolymer C1B has an Mn of 1085, an Mw of 12400, and an Mw / Mn of 11.4, and contains 84.0 mol% (83.8 wt%) of structural units derived from divinylbenzene and a total of 16.0 mol% (16.2 wt%) of structural units derived from ethylvinylbenzene. The crosslinking structural unit (a2) is 2.60 mol% (2.59 wt%), the degree of crosslinking is 0.031, the vinyl-containing structural unit (a1) is 11.40 mol% (11.37 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.114.
[0431] The Tg of the cured product was 82° C., the softening temperature was 93° C., and the weight loss at 350° C. was 8.25 wt %. On the other hand, the compatibility with the epoxy resin was ○.
[0432] The haze value of the multifunctional vinyl aromatic copolymer C1B was 0.02.
[0433] Comparative Example 2B
[0434] 1.5 mol (195.3 g) of divinylbenzene, 0.88 mol (114.7 g) of ethylvinylbenzene, 12.6 mol (1314.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were placed in a 5.0 L reactor, 600 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 820.8 g of copolymer C2B was confirmed.
[0435] The Mn of copolymer C2B is 1490, the Mw is 12600, and the Mw / Mn is 8.44. Copolymer C2B contains 11.3 mol% (13.5 wt%) of structural units derived from divinylbenzene, 5.79 mol% (7.04 wt%) of structural units derived from ethylvinylbenzene, and 82.9 mol% (79.4 wt%) of structural units derived from styrene.
[0436] The cross-linked structural unit (a2) is 5.86 mol% (7.02 wt%), the cross-linking degree is 0.52, the vinyl-containing structural unit (a1) is 5.41 mol% (6.48 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.054.
[0437] The cured product had a Tg of 162°C, a softening temperature of 280°C or higher, and a weight loss of 1.86 wt% at 350°C.
[0438] The haze value of the multifunctional vinyl aromatic copolymer C2B was 0.14.
[0439] Comparative Example 3B
[0440] 2.25 mol (292.9 g) of divinylbenzene, 1.32 mol (172.0 g) of ethylvinylbenzene, 11.4 mol (1190.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were placed in a 5.0 L reactor, and 600 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 860.8 g of copolymer C3B was confirmed.
[0441] The Mn of copolymer C3B is 2060, the Mw is 30700, and the Mw / Mn is 14.9. Copolymer C3B contains 20.92 mol% (24.29 wt%) of structural units derived from divinylbenzene, 9.06 mol% (10.68 wt%) of structural units derived from ethylvinylbenzene, and 70.02 mol% (65.03 wt%) of structural units derived from styrene.
[0442] The cross-linked structural unit (a2) is 11.30 mol% (13.12 wt%), the cross-linking degree is 0.54, the vinyl-containing structural unit (a1) is 9.62 mol% (11.17 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.096.
[0443] The cured product had no Tg, had a softening temperature of 280°C or higher, and had a weight loss of 2.11 wt% at 350°C.
[0444] The haze value of the multifunctional vinyl aromatic copolymer C3B was 0.17.
[0445] Comparative Example 4B
[0446] 3.1 mol (404.5 g) of divinylbenzene, 1.8 mol (237.6 g) of ethylvinylbenzene, 7.5 mol (780.7 g) of styrene, and 13.0 mol (1325.7 g) of n-propyl acetate were placed in a 5.0 L reactor, 193 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 689.2 g of copolymer C4B was confirmed.
[0447] The Mn of copolymer C4B is 2940, the Mw is 39500, and the Mw / Mn is 13.4. Copolymer C4B contains 36.8 mol% (40.7 wt%) of structural units derived from divinylbenzene, 14.5 mol% (16.3 wt%) of structural units derived from ethylvinylbenzene, and 48.6 mol% (43.0 wt%) of structural units derived from styrene.
[0448] The cross-linked structural unit (a2) is 20.99 mol% (23.20 wt%), the cross-linking degree is 0.57, the vinyl-containing structural unit (a1) is 15.84 mol% (17.50 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.158.
[0449] The cured product had no Tg, had a softening temperature of 280°C or higher, and had a weight loss of 2.23 wt% at 350°C.
[0450] The haze value of the multifunctional vinyl aromatic copolymer C4B was 0.21.
[0451] Example 6B
[0452] In a nitrogen-purged autoclave reactor with an internal volume of 0.5 liters, 245 g of cyclohexane, 2.5 g of THF, 10 g of styrene, 40 g of 1,3-butadiene, and 0.50 g of the multifunctional vinyl aromatic copolymer 1B obtained in Example 1B were added. At 25° C., 5 g of a cyclohexane solution containing 50 mg of sec-butyl lithium was added to start polymerization. The temperature of the reaction solution rose due to the polymerization heat, and the maximum temperature reached 85° C.
[0453] After confirming that the polymerization conversion rate reached 99%, 50 mg of isopropanol was added to stop the polymerization, and 2,6-di-tert-butyl-p-cresol (BHT) was added to the reaction solution. Then, the solvent was removed by steam stripping to obtain conjugated diene copolymer 6B. The physical properties of the obtained conjugated diene copolymer 6B are shown in Table 1B.
[0454] Example 7B
[0455] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.50 g of the multifunctional vinyl aromatic copolymer 1B obtained in Example 1B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 85°C.
[0456] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 7B. The physical properties of the obtained conjugated diene copolymer 7B are shown in Table 1B.
[0457] Example 8B
[0458] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.30 g of the multifunctional vinyl aromatic copolymer 2B obtained in Example 2B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 85°C.
[0459] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain conjugated diene copolymer 8B. The physical properties of the obtained conjugated diene copolymer 8B are shown in Table 1B.
[0460] Example 9B
[0461] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.50 g of the multifunctional vinyl aromatic copolymer 1B obtained in Example 1B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0462] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain conjugated diene copolymer 9B. The physical properties of the obtained conjugated diene copolymer 9B are shown in Table 1B.
[0463] Example 10B
[0464] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.35 g of the multifunctional vinyl aromatic copolymer 2B obtained in Example 2B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0465] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 10B. The physical properties of the obtained conjugated diene copolymer 10B are shown in Table 1B.
[0466] Example 11B
[0467] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.030 g of the multifunctional vinyl aromatic copolymer 3B obtained in Example 3B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was generally soluble in cyclohexane, but the formation of gel was also observed visually. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 82°C.
[0468] After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80° C. for 5 minutes to obtain a polymer solution. After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 11B. The physical properties of the obtained conjugated diene copolymer 11B are shown in Table 1B.
[0469] Example 12B
[0470] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.25 g of the multifunctional vinyl aromatic copolymer 4B obtained in Example 4B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C.
[0471] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 12B. The physical properties of the obtained conjugated diene copolymer 12B are shown in Table 1B.
[0472] Example 13B
[0473] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.15 g of the multifunctional vinyl aromatic copolymer 5B obtained in Example 5B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C.
[0474] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to terminate the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 13B. The physical properties of the obtained conjugated diene copolymer 13B are shown in Table 1B.
[0475] Comparative Example 5B
[0476] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.5 g of the multifunctional vinyl aromatic copolymer C1B obtained in Comparative Example 1B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 84°C.
[0477] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Then, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C5B. The physical properties of the obtained conjugated diene copolymer C5B are shown in Table 1B.
[0478] Comparative Example 6B
[0479] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50 ° C. Then, 45 g of a cyclohexane solution containing 0.030 g of the multifunctional vinyl aromatic copolymer C2B obtained in Comparative Example 2B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator is generally soluble in cyclohexane, but the formation of gel was also observed visually. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83 ° C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80 ° C for 5 minutes to obtain a polymer solution.
[0480] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C6B. The physical properties of the obtained conjugated diene copolymer C6B are shown in Table 1B.
[0481] Comparative Example 7B
[0482] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.25 g of the multifunctional vinyl aromatic copolymer C3B obtained in Comparative Example 3B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0483] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C7B. The physical properties of the obtained conjugated diene copolymer C7B are shown in Table 1B.
[0484] Comparative Example 8B
[0485] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 2.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 50 mg (0.78 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.15 g of the multifunctional vinyl aromatic copolymer C4B obtained in Comparative Example 4B was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0486] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Then, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C8B. The physical properties of the obtained conjugated diene copolymer C8B are shown in Table 1B.
[0487] [Table 1B]
[0488]
[0489] Example 14B
[0490] The conjugated diene copolymer 6B, process oil, carbon black, zinc oxide, stearic acid and antioxidant were kneaded at 155° C. and 60 rpm for 4 minutes using a Labo Plastomill.
[0491] Sulfur and a vulcanization accelerator were added to the kneaded product obtained by the kneading, and the mixture was kneaded at 70° C. and 60 rpm for 1 minute for vulcanization to obtain a crosslinked rubber 14B.
[0492] Each additive and the blending ratio are the same as those in Table 2A. In addition, the physical properties of the crosslinked rubber 14B are shown in Table 3B.
[0493] Example 15B to Example 21B, Comparative Example 9B to Comparative Example 12B
[0494] Cross-linked rubbers 15B to 21B and cross-linked rubbers C9B to C12B were obtained by the same method as in Example 14B, except that the conjugated diene copolymers 7B to 13B and the conjugated diene copolymers C5B to C8B synthesized in the examples or comparative examples were used instead of the conjugated diene copolymer 6B.
[0495] The types of the conjugated diene copolymers used and the physical properties of the obtained cross-linked rubbers 14B to 21B and cross-linked rubbers C9B to C12B are shown in Table 3B.
[0496] [Table 3B]
[0497]
[0498] As can be seen from Table 3B, the cross-linked rubber of the present invention using the multifunctional vinyl aromatic copolymer of the present invention imparts processability equal to or better than that of the case using divinylbenzene as a conventional branching agent, and in the vulcanized rubber blended with carbon black, has excellent tensile strength and abrasion resistance.
[0499] <Examples of the third invention>
[0500] Example 1C
[0501] 31.00 g of DVB-630 (divinylbenzene component 0.150 mol, ethylvinylbenzene (mixture of metamer and paramer) component 0.088 mol), 65.72 g (0.631 mol) of styrene, 70.80 g (0.631 mol) of diisobutylene, 60 mmol (6.90 mL) of n-propyl acetate, and 48.55 g (0.527 mol) of toluene were placed in a 500 mL reactor, 15.2 mmol of boron trifluoride diethyl ether complex (1.91 mL) was added at 70° C., and the reaction was carried out for 2.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 60.6 g of a multifunctional vinyl aromatic copolymer 1C.
[0502] The obtained multifunctional vinyl aromatic copolymer 1C had an Mn of 941, an Mw of 2850, and an Mw / Mn of 3.03. 13 C-NMR and 1According to H-NMR analysis, the polyfunctional vinyl aromatic copolymer 1C contains 19.0 mol% (21.8 wt%) of structural units derived from divinylbenzene, 8.3 mol% (9.6 wt%) of structural units derived from ethylvinylbenzene, 48.6 mol% (44.6 wt%) of structural units derived from styrene, and 24.2 mol% (24.0 wt%) of structural units derived from diisobutylene. The crosslinking structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) is 4.6 mol% (5.2 wt%), so the crosslinking degree (a2 / a) is 0.24. In addition, the structural unit (a1) derived from divinylbenzene having a residual vinyl group contained in the polyfunctional vinyl aromatic copolymer 1C is 14.4 mol% (16.5 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a), (b) and (c) is 0.144.
[0503] The result of TMA measurement of the cured product was Tg: 167°C, and the softening temperature was 280°C or higher.
[0504] The result of TGA measurement was a weight loss of 1.41 wt % at 350° C. A sample prepared by dissolving 0.5 g of the multifunctional vinyl aromatic copolymer 1C in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.02.
[0505] Example 2C
[0506] 46.49 g of DVB-630 (divinylbenzene component 0.225 mol, ethylvinylbenzene component 0.132 mol), 53.33 g (0.512 mol) of styrene, 70.80 g (0.631 mol) of diisobutylene, 60 mmol (6.90 mL) of n-propyl acetate, and 48.55 g (0.527 mol) of toluene were placed in a 500 mL reactor, 10.0 mmol of boron trifluoride diethyl ether complex (1.26 mL) was added at 70° C., and the reaction was carried out for 2.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 66.4 g of a multifunctional vinyl aromatic copolymer 2C.
[0507] The obtained multifunctional vinyl aromatic copolymer 2C had an Mn of 1240, an Mw of 4980, and an Mw / Mn of 4.02. 13 C-NMR and 1According to H-NMR analysis, the multifunctional vinyl aromatic copolymer 2C contains 28.2 mol% (31.5 wt%) of structural units derived from divinylbenzene, 12.2 mol% (13.8 wt%) of structural units derived from ethylvinylbenzene, 37.6 mol% (33.6 wt%) of structural units derived from styrene, and 22.0 mol% (21.1 wt%) of structural units derived from diisobutylene. The crosslinking structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) is 7.6 mol% (8.5 wt%), so the degree of crosslinking is 0.27. In addition, the structural unit (a1) derived from divinylbenzene having a residual vinyl group contained in the multifunctional vinyl aromatic copolymer 2C is 20.6 mol% (23.0 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a), (b) and (c) is 0.206.
[0508] The result of TMA measurement of the cured product was Tg: 176°C, and the softening temperature was 280°C or higher.
[0509] The result of TGA measurement was a weight loss of 1.32 wt % at 350° C. A sample prepared by dissolving 0.5 g of the multifunctional vinyl aromatic copolymer 2C in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.03.
[0510] Example 3C
[0511] 62.00 g of DVB-630 (divinylbenzene component 0.300 mol, ethylvinylbenzene component 0.176 mol), 40.92 g (0.393 mol) of styrene, 70.80 g (0.631 mol) of diisobutylene, 60 mmol (6.90 mL) of n-propyl acetate, and 48.55 g (0.527 mol) of toluene were placed in a 500 mL reactor, 8.2 mmol of boron trifluoride diethyl ether complex (1.03 mL) was added at 70° C., and the reaction was carried out for 1.5 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 56.3 g of a multifunctional vinyl aromatic copolymer 3C.
[0512] The obtained multifunctional vinyl aromatic copolymer 3C had an Mn of 1430, an Mw of 5490, and an Mw / Mn of 3.84. 13 C-NMR and 1According to H-NMR analysis, the multifunctional vinyl aromatic copolymer 3C contained 39.4 mol% (42.6 wt%) of structural units derived from divinylbenzene, 15.9 mol% (17.4 wt%) of structural units derived from ethylvinylbenzene, 25.7 mol% (22.2 wt%) of structural units derived from styrene, and 19.1 mol% (17.8 wt%) of structural units derived from diisobutylene. The crosslinking structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) was 11.4 mol% (12.3 wt%), so the degree of crosslinking was 0.29. In addition, the structural unit (a1) derived from divinylbenzene having a residual vinyl group contained in the multifunctional vinyl aromatic copolymer 3C was 28.0 mol% (30.2 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a), (b), and (c) was 0.280.
[0513] The result of TMA measurement of the cured product was Tg: 183°C, and the softening temperature was 280°C or higher.
[0514] The result of TGA measurement was that the weight loss at 350° C. was 1.28 wt %. A sample prepared by dissolving 0.5 g of the polyfunctional vinyl aromatic copolymer 3C in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.05.
[0515] Comparative Example 1C
[0516] 320.5 mL of DVB-810 (1.82 mol of divinylbenzene component, 0.43 mol of ethylvinylbenzene component), 0.28 mol (36.9 mL) of n-butyl acetate, and 140 mL of toluene were placed in a 1.0 L reactor, and a solution of 40 mmol of methanesulfonic acid dissolved in 0.12 mol (15.7 mL) of n-butyl acetate was added at 70° C., and the reaction was carried out for 6 hours. After the polymerization was stopped by potassium hydroxide, activated alumina was used as a filter aid for filtration. Thereafter, the mixture was devolatilized under reduced pressure at 60° C. to obtain 22.6 g of a multifunctional vinyl aromatic copolymer C1C.
[0517] The multifunctional vinyl aromatic copolymer C1C has an Mn of 1085, an Mw of 12400, and an Mw / Mn of 11.4, and contains 84.0 mol% (83.8 wt%) of structural units derived from divinylbenzene and a total of 16.0 mol% (16.2 wt%) of structural units derived from ethylvinylbenzene. The crosslinking structural unit (a2) is 2.60 mol% (2.59 wt%), the degree of crosslinking is 0.031, the vinyl-containing structural unit (a1) is 11.40 mol% (11.37 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.114.
[0518] The Tg of the cured product was 82° C., the softening temperature was 93° C., and the weight loss at 350° C. was 8.25 wt %. On the other hand, the compatibility with the epoxy resin was ○.
[0519] The haze value of the multifunctional vinyl aromatic copolymer C1C was 0.02.
[0520] Comparative Example 2C
[0521] 1.5 mol (195.3 g) of divinylbenzene, 0.88 mol (114.7 g) of ethylvinylbenzene, 12.6 mol (1314.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were placed in a 5.0 L reactor, 600 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 820.8 g of copolymer C2C was obtained.
[0522] The Mn of copolymer C2C is 1490, the Mw is 12600, and the Mw / Mn is 8.44. Copolymer C2C contains 11.3 mol% (13.5 wt%) of structural units derived from divinylbenzene, 5.79 mol% (7.04 wt%) of structural units derived from ethylvinylbenzene, and 82.9 mol% (79.4 wt%) of structural units derived from styrene.
[0523] The cross-linked structural unit (a2) is 5.86 mol% (7.02 wt%), the cross-linking degree is 0.52, the vinyl-containing structural unit (a1) is 5.41 mol% (6.48 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.054.
[0524] The cured product had a Tg of 162°C, a softening temperature of 280°C or higher, and a weight loss of 1.86 wt% at 350°C.
[0525] The haze value of the multifunctional vinyl aromatic copolymer C2C was 0.14.
[0526] Comparative Example 3C
[0527] 2.25 mol (292.9 g) of divinylbenzene, 1.32 mol (172.0 g) of ethylvinylbenzene, 11.4 mol (1190.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were placed in a 5.0 L reactor, and 600 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 860.8 g of copolymer C3C was confirmed.
[0528] The Mn of copolymer C3C is 2060, the Mw is 30700, and the Mw / Mn is 14.9. Copolymer C3C contains 20.92 mol% (24.29 wt%) of structural units derived from divinylbenzene, 9.06 mol% (10.68 wt%) of structural units derived from ethylvinylbenzene, and 70.02 mol% (65.03 wt%) of structural units derived from styrene.
[0529] The cross-linked structural unit (a2) is 11.30 mol% (13.12 wt%), the cross-linking degree is 0.54, the vinyl-containing structural unit (a1) is 9.62 mol% (11.17 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.096.
[0530] The cured product had no Tg, had a softening temperature of 280°C or higher, and had a weight loss of 2.11 wt% at 350°C.
[0531] The haze value of the multifunctional vinyl aromatic copolymer C3C was 0.17.
[0532] Comparative Example 4C
[0533] 3.1 mol (404.5 g) of divinylbenzene, 1.8 mol (237.6 g) of ethylvinylbenzene, 7.5 mol (780.7 g) of styrene, and 13.0 mol (1325.7 g) of n-propyl acetate were placed in a 5.0 L reactor, 193 mmol of diethyl ether complex of boron trifluoride was added at 70° C., and the reaction was carried out for 4 hours. After the polymerization was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. The obtained copolymer was weighed, and 689.2 g of copolymer C4C was confirmed.
[0534] The Mn of copolymer C4C is 2940, the Mw is 39500, and the Mw / Mn is 13.4. Copolymer C4C contains 36.8 mol% (40.7 wt%) of structural units derived from divinylbenzene, 14.5 mol% (16.3 wt%) of structural units derived from ethylvinylbenzene, and 48.6 mol% (43.0 wt%) of structural units derived from styrene.
[0535] The cross-linked structural unit (a2) is 20.99 mol% (23.20 wt%), the cross-linking degree is 0.57, the vinyl-containing structural unit (a1) is 15.84 mol% (17.50 wt%), and the molar fraction of the vinyl-containing structural unit (a1) is 0.158.
[0536] The cured product had no Tg, had a softening temperature of 280°C or higher, and had a weight loss of 2.23 wt% at 350°C.
[0537] The haze value of the multifunctional vinyl aromatic copolymer C4C was 0.21.
[0538] Example 4C
[0539] In a nitrogen-purged autoclave reactor with an internal volume of 0.5 liters, 245 g of cyclohexane, 0.5 g of THF, 10 g of styrene, 40 g of 1,3-butadiene, and 0.10 g of the multifunctional vinyl aromatic copolymer 1C obtained in Example 1C were added. At 25° C., 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of sec-butyl lithium was added to start polymerization. The temperature of the reaction solution rose due to the polymerization heat, and the maximum temperature reached 81° C.
[0540] After confirming that the polymerization conversion rate reached 99%, 50 mg of isopropanol was added to stop the polymerization, and 2,6-di-tert-butyl-p-cresol (BHT) was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 4C. 0.5 g of the obtained conjugated diene copolymer 4C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added for coloring, and filtered using a 0.2 μm polytetrafluoroethylene (PTFE) membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 4C are shown in Table 1C.
[0541] Example 5C
[0542] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.10 g of the multifunctional vinyl aromatic copolymer 1C obtained in Example 1C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 80°C.
[0543] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 5C. 0.5 g of the obtained conjugated diene copolymer 5C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 5C are shown in Table 1C.
[0544] Example 6C
[0545] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.085 g of the multifunctional vinyl aromatic copolymer 2C obtained in Example 2C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added, and polymerization was started. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0546] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 6C. 0.5 g of the obtained conjugated diene copolymer 6C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 6C are shown in Table 1C.
[0547] Example 7C
[0548] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.10 g of the multifunctional vinyl aromatic copolymer 1C obtained in Example 1C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 81°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0549] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 7C. 0.5 g of the obtained conjugated diene copolymer 7C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 7C are shown in Table 1C.
[0550] Example 8C
[0551] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.085 g of the multifunctional vinyl aromatic copolymer 2C obtained in Example 2C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 82°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0552] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 8C. 0.5 g of the obtained conjugated diene copolymer 8C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 8C are shown in Table 1C.
[0553] Example 9C
[0554] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.070 g of the multifunctional vinyl aromatic copolymer 3C obtained in Example 3C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 78°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0555] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 9C. 0.5 g of the obtained conjugated diene copolymer 9C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added for coloring, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 9C are shown in Table 1C.
[0556] Comparative Example 5C
[0557] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.1 g of the multifunctional vinyl aromatic copolymer C1C obtained in Comparative Example 1C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 84°C.
[0558] After confirming that the polymerization conversion rate reaches 99%, 50 mg (0.83 mmol) of isopropanol is added to stop the polymerization, and BHT is added to the reaction solution. Subsequently, the solvent is removed by steam stripping to obtain a conjugated diene copolymer C5C. 0.5 g of the obtained conjugated diene copolymer C5C is dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution is added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration is observed using a real-time dynamic microscope, and the formation of microgels is confirmed. The physical properties of the conjugated diene copolymer C5C are shown in Table 1C.
[0559] Comparative Example 6C
[0560] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium was added at 50 ° C. Then, 45 g of a cyclohexane solution containing 0.08 g of the multifunctional vinyl aromatic copolymer C2C obtained in Comparative Example 2C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator is generally soluble in cyclohexane, but the formation of gel was also observed visually. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83 ° C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out for 5 minutes at a temperature of 80 ° C to obtain a polymer solution.
[0561] After confirming that the polymerization conversion rate reaches 99%, 50 mg (0.83 mmol) of isopropanol is added to stop the polymerization, and BHT is added to the reaction solution. Subsequently, the solvent is removed by steam stripping to obtain a conjugated diene copolymer C6C. 0.5 g of the obtained conjugated diene copolymer C6C is dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution is added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration is observed using a real-time dynamic microscope, and the formation of microgels is confirmed. The physical properties of the conjugated diene copolymer C6C are shown in Table 1C.
[0562] Comparative Example 7C
[0563] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.10 g of the multifunctional vinyl aromatic copolymer C3C obtained in Comparative Example 3C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, but the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0564] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer C7C. 0.5 g of the obtained conjugated diene copolymer C7C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and the formation of microgels was confirmed. The physical properties of the conjugated diene copolymer C7C are shown in Table 1C.
[0565] Comparative Example 8C
[0566] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium was added at 50°C, and then 45 g of a cyclohexane solution containing 0.08 g of the multifunctional vinyl aromatic copolymer C4C obtained in Comparative Example 4C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was partially soluble in cyclohexane, and the formation of gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 83°C.
[0567] After confirming that the polymerization conversion rate reaches 99%, 50 mg (0.83 mmol) of isopropanol is added to stop the polymerization, and BHT is added to the reaction solution. Subsequently, the solvent is removed by steam stripping to obtain a conjugated diene copolymer C8C. 0.5 g of the obtained conjugated diene copolymer C8C is dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution is added to color it, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration is observed using a real-time dynamic microscope, and the formation of microgels is confirmed. The physical properties of the conjugated diene copolymer C8C are shown in Table 1C.
[0568] [Table 1C]
[0569]
[0570] Example 10C
[0571] The conjugated diene copolymer 4C (copolymer rubber) synthesized in Example 4C, process oil, carbon black, zinc oxide, stearic acid and an antioxidant were mixed and kneaded at 155° C. and 60 rpm for 4 minutes using a Labo Plastomill.
[0572] Sulfur and a vulcanization accelerator were added to the kneaded product obtained by the kneading, and the mixture was kneaded at 70° C. and 60 rpm for 1 minute for vulcanization to obtain a crosslinked rubber 10C.
[0573] The blending ratio of each additive is shown in Table 2C. In addition, the physical properties of the crosslinked rubber 10C are shown in Table 3C.
[0574] [Table 2C]
[0575] Copolymer rubber 100.0 Process oil 37.5 Silicon dioxide 65.0 Carbon Black 5.0 Zinc Oxide 3.0 Stearic acid 1.0 Anti-aging agents 1.0 sulfur 1.8 Vulcanization accelerator 1.5
[0576] In addition, the additives used were as follows.
[0577] Process oil: Diana process oil AC-12 manufactured by Idemitsu Kosan
[0578] Silicon dioxide: Degussa, ULTRASIL VN3
[0579] Carbon black: Nitrotron #300 manufactured by NIPPON STEEL Carbon
[0580] Zinc oxide: Zinc White No. 1 manufactured by Mitsui Mining and Smelting
[0581] Stearic acid: Made in NOF Corporation
[0582] Anti-aging agent: Nocceler-NS manufactured by Ouchi Shinko Chemical Industry
[0583] Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry
[0584] Vulcanization accelerator: N-tert-butylbenzothiazole-2-sulfenamide
[0585] Example 11C to Example 15C, Comparative Example 9C to Comparative Example 12C
[0586] Cross-linked rubbers 11C to 15C and cross-linked rubbers C9C to C12C were obtained by the same method as Example 10C, except that conjugated diene copolymers 5C to 9C and conjugated diene copolymers C5C to C8C synthesized in the above-mentioned examples or comparative examples were used instead of conjugated diene copolymer 4C.
[0587] The types of the conjugated diene copolymers used and the physical properties of the obtained cross-linked rubbers 11C to 15C and C9C to C12C are shown in Table 3C.
[0588] [Table 3C]
[0589]
[0590] As can be seen from Table 3C, the cross-linked rubber of the present invention using the multifunctional vinyl aromatic copolymer of the present invention imparts silica dispersibility and interface adhesion equal to or higher than that of the case using divinylbenzene as a conventional branching agent, and therefore, in the vulcanized rubber, has excellent tensile strength and abrasion resistance.
[0591] Example 16C
[0592] 46.49 g of DVB-630 (divinylbenzene component 0.225 mol, ethylvinylbenzene component 0.132 mol), 53.33 g (0.512 mol) of styrene, 61.95 g (0.631 mol) of 2-methyl-1-hexene, 60 mmol (6.90 mL) of n-propyl acetate, and 48.55 g (0.527 mol) of toluene were placed in a 500 mL reactor, 10.0 mmol of boron trifluoride diethyl ether complex (1.26 mL) was added at 70° C., and the reaction was carried out for 2.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered by decompression devolatilization at 60° C. to obtain 64.8 g of a multifunctional vinyl aromatic copolymer 16C.
[0593] The obtained multifunctional vinyl aromatic copolymer 16C had an Mn of 1310, an Mw of 5070, and an Mw / Mn of 3.87. 13 C-NMR and 1 H-NMR analysis showed that the multifunctional vinyl aromatic copolymer 16C contained 28.0 mol % (32.2 wt %) of structural units derived from divinylbenzene, 12.2 mol % (14.2 wt %) of structural units derived from ethylvinylbenzene, 32.5 mol % (35.3 wt %) of structural units derived from styrene, and 24.5 mol % (21.2 wt %) of structural units derived from 2-methyl-1-hexene.
[0594] The crosslinked structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) is 8.1 mol% (9.3 wt%), so the degree of crosslinking is 0.29. In addition, the structural unit (a1) derived from divinylbenzene having a residual vinyl group contained in the multifunctional vinyl aromatic copolymer 16C is 19.9 mol% (22.8 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a), (b) and (c) is 0.199.
[0595] The result of TMA measurement of the cured product was Tg: 168°C, and the softening temperature was 280°C or higher.
[0596] The result of TGA measurement was a weight loss of 1.41 wt % at 350° C. A sample prepared by dissolving 0.5 g of the multifunctional vinyl aromatic copolymer 16C in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.04.
[0597] Example 17C
[0598] 46.49 g of DVB-630 (divinylbenzene component 0.225 mol, ethylvinylbenzene component 0.132 mol), 53.33 g (0.512 mol) of styrene, 53.10 g (0.631 mol) of 2-methyl-1-pentene, 60 mmol (6.90 mL) of n-propyl acetate, and 48.55 g (0.527 mol) of toluene were placed in a 500 mL reactor, 10.0 mmol of boron trifluoride diethyl ether complex (1.26 mL) was added at 70° C., and the reaction was carried out for 2.0 hours. After the polymerization was stopped with a sodium bicarbonate aqueous solution, the oil layer was washed three times with pure water, and the copolymer was recovered under reduced pressure at 60° C. to obtain 61.5 g of a multifunctional vinyl aromatic copolymer 17C.
[0599] The obtained multifunctional vinyl aromatic copolymer 17C had an Mn of 1280, an Mw of 5260, and an Mw / Mn of 4.11. 13 C-NMR and 1 H-NMR analysis showed that the multifunctional vinyl aromatic copolymer 17C contained 26.5 mol % (31.7 wt %) of structural units derived from divinylbenzene, 11.3 mol % (13.8 wt %) of structural units derived from ethylvinylbenzene, 35.3 mol % (33.8 wt %) of structural units derived from styrene, and 26.8 mol % (20.8 wt %) of structural units derived from 2-methyl-1-pentene.
[0600] The crosslinked structural unit (a2) derived from the divinyl aromatic compound represented by the formula (2) is 7.2 mol% (8.6 wt%), so the degree of crosslinking is 0.27. In addition, the structural unit (a1) derived from divinylbenzene having residual vinyl groups contained in the multifunctional vinyl aromatic copolymer 17C is 19.3 mol% (23.1 wt%), so the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural units (a), (b) and (c) is 0.193.
[0601] The result of TMA measurement of the cured product was Tg: 171°C, and the softening temperature was 280°C or higher.
[0602] The result of TGA measurement was a weight loss of 1.38 wt % at 350° C. A sample prepared by dissolving 0.5 g of the multifunctional vinyl aromatic copolymer 17C in 100 g of toluene was placed in a quartz cell, and the haze (turbidity) thereof was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.03.
[0603] Example 18C
[0604] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.085 g of the multifunctional vinyl aromatic copolymer 16C obtained in Example 16C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 82°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out the modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0605] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 18C. 0.5 g of the obtained conjugated diene copolymer 18C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added for coloring, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 18C are shown in Table 4C.
[0606] Example 19C
[0607] In a nitrogen-substituted autoclave reactor, 200 g of cyclohexane and 0.5 g of THF were loaded, and 5 g of a cyclohexane solution containing 10 mg (0.16 mmol) of n-butyl lithium in purity was added at 50°C, and then 45 g of a cyclohexane solution containing 0.085 g of the multifunctional vinyl aromatic copolymer 17C obtained in Example 17C was added over 30 minutes to prepare a multifunctional anionic polymerization initiator. The prepared multifunctional anionic polymerization initiator was soluble in cyclohexane, and no gel was observed. 10 g of styrene and 40 g of 1,3-butadiene from which impurities had been removed in advance were added to start polymerization. The temperature of the reaction solution rose due to the heat of polymerization, and the maximum temperature reached 82°C. After the polymerization reaction was completed, 21 mmol of BTESPA was added to the reactor as a modifier to carry out a modification reaction, and the modification reaction was carried out at a temperature of 80°C for 5 minutes to obtain a polymer solution.
[0608] After confirming that the polymerization conversion rate reached 99%, 50 mg (0.83 mmol) of isopropanol was added to stop the polymerization, and BHT was added to the reaction solution. Subsequently, the solvent was removed by steam stripping to obtain a conjugated diene copolymer 19C. 0.5 g of the obtained conjugated diene copolymer 19C was dissolved in 100 mL of toluene, and 1.0 g of a 0.2 wt % Sudan III toluene solution was added for coloring, and filtered using a 0.2 μm PTFE membrane filter. The membrane filter after filtration was observed using a real-time dynamic microscope, and it was confirmed that no microgel was generated. The physical properties of the conjugated diene copolymer 19C are shown in Table 4C.
[0609] [Table 4C]
[0610]
[0611] [Industrial Applicability]
[0612] The multifunctional vinyl aromatic copolymer of the present invention can be used as a raw material for a conjugated diene copolymer. Furthermore, a crosslinked rubber composition obtained by crosslinking a filler in the conjugated diene copolymer has excellent dispersibility of the filler, excellent mechanical strength and wear resistance, and can therefore be effectively used as an elastomeric material such as a tire (especially a tire tread), a shock-absorbing rubber, a rubber hose, a rubber roller, and a shoe material.
[0613] In addition, it can be applied to the improver of molding materials, resins, etc. In the fields of electrical and electronic industry, aerospace industry, etc., it can be provided as dielectric materials, insulating materials, heat-resistant materials, structural materials, etc. In addition, the film and sheet formed by coating the curable resin composition containing the multifunctional vinyl aromatic copolymer of the present invention can be suitably used for plastic optical parts, touch screens, flat panel displays, film liquid crystal elements, etc. The multifunctional vinyl aromatic copolymer of the present invention can also be used as a improver for improving the heat resistance, dielectric properties and optical properties of the thermoplastic resin or curable resin composition used as the main material of the film, sheet and prepreg. In addition, the curable resin composition containing the multifunctional vinyl aromatic copolymer of the present invention as the main material can also be processed into a film, sheet and prepreg for use. And then, the curable resin composition containing the multifunctional vinyl aromatic copolymer of the present invention can also be used as various optical elements headed by optical waveguides or optical lenses.
Claims
1. A multifunctional vinyl aromatic copolymer comprising: 0.5 mol% to 75 mol% of a structural unit (a) derived from a divinyl aromatic compound; 5.0 mol% to 75 mol% of a structural unit (b) derived from a monovinyl aromatic compound having no substituent at the α position; and 5.0 mol% to 75 mol% of a structural unit (c) derived from an α,α-disubstituted olefin compound, characterized in that: At least a part of the structural unit (a) is a crosslinking structural unit (a2) represented by the following formula (2) and a vinyl group-containing structural unit (a1) represented by the following formula (1), wherein the α,α-disubstituted olefin compound is one or more monomers selected from the group consisting of isobutylene, diisobutylene, 2-methyl-1-butene, 2-methyl-1-pentene, 1-methyl-1-cyclopentene, 2-methyl-1-hexene, 1-methyl-1-cyclohexene, 2-methyl-1-heptene, 2-methyl-1-octene, 2-methyl-1-nonene, 2-methyl-1-decene, 2-methyl-1-dodecene, 2-methyl-1-tetradecene, 2-methyl-1-hexadecene, 2-methyl-1-octadecene, 2-methyl-1-eicosene, 2-methyl-1-docosahexadecene, and 2-methyl-1-tetracosene, In the formula, R 1 independently represent an aromatic hydrocarbon group having 6 to 30 carbon atoms, The molar fraction of the crosslinking structural unit (a2) relative to the structural unit (a) is in the range of 0.05 to 0.60, and the molar fraction of the vinyl-containing structural unit (a1) relative to the total of the structural unit (a), the structural unit (b) and the structural unit (c) is in the range of 0.001 to 0.60, The number average molecular weight Mn of the polyfunctional vinyl aromatic copolymer is 300 to 50,000, and the molecular weight distribution represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is 10.0 or less.
2. The multifunctional vinyl aromatic copolymer according to claim 1, wherein the monovinyl aromatic compound having no substituent at the α position is one or more monomers selected from the group consisting of styrene, vinyl naphthalene, vinyl biphenyl, m-methylstyrene, p-methylstyrene, o-,p-dimethylstyrene, m-ethylvinylbenzene, and p-ethylvinylbenzene.
3. A method for producing a multifunctional vinyl aromatic copolymer, characterized in that: The multifunctional vinyl aromatic copolymer is the multifunctional vinyl aromatic copolymer as claimed in claim 1, and the production method is to dissolve a polymerization raw material comprising a divinyl aromatic compound, a monovinyl aromatic compound having no substituent at the α position, and an α,α-disubstituted olefin compound in a uniform solvent having a dielectric constant of 2.0 to 15.0, and polymerize at a temperature of 0°C to 120°C in the presence of a Lewis acid catalyst.
4. A conjugated diene copolymer, characterized in that: The polyfunctional vinyl aromatic copolymer (A) according to claim 1 is obtained by copolymerizing a conjugated diene compound (B) or a conjugated diene compound (B) and an aromatic vinyl compound (C).
5. The conjugated diene copolymer according to claim 4, characterized in that: The polyfunctional vinyl aromatic copolymer contains 0.001 to 6 wt % of a structural unit (A1) derived from the polyfunctional vinyl aromatic copolymer, 29 to 99.999 wt % of a structural unit (B1) derived from a conjugated diene compound, and 0 to 70 wt % of a structural unit (C1) derived from an aromatic vinyl compound. 6 . The conjugated diene copolymer according to claim 4 , wherein the polymerization active end of the conjugated diene copolymer is further reacted with a modifier to be modified.
7. A conjugated diene copolymer composition, characterized in that: The conjugated diene copolymer according to claim 4 contains 0.5 to 200 parts by weight of at least one reinforcing filler selected from the group consisting of silica-based inorganic fillers, metal oxides, metal hydroxides and carbon black, based on 100 parts by weight of the conjugated diene copolymer. 8 . The conjugated diene copolymer composition according to claim 7 , further comprising a crosslinking agent.
9. A cross-linked rubber product, characterized in that: The conjugated diene copolymer composition according to claim 8 is cross-linked.
10. A tire component comprising the rubber cross-linked product according to claim 9.
Citation Information
Patent Citations
Method for producing block copolymer
JP2003073434A
Star-block interpolymers and their manufacture
JP2004517202A
Rubber composition
JP2005213381A
Soluble polyfunctional vinyl aromatic copolymer, method for producing the same, curable resin composition, and cured product of the same