A method for enriching nickel and cobalt metals in fayalite slag
Through the method of combining oxidation roasting and reduction roasting, the fayalite-type slag is decomposed and the enrichment of nickel and cobalt in the metallic iron phase is avoided. Nickel and cobalt are separated by alkali leaching and magnetic separation, which solves the difficulty of separating nickel and cobalt in the existing technology. problem, achieving effective enrichment of nickel and cobalt and monomer dissociation of iron, improving the added value of fayalite slag.
Patent Information
- Application Number
- CN202210735625.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-27
AI Technical Summary
It is difficult to effectively enrich nickel and cobalt metal in fayalite-type slag with existing technology. In traditional methods, nickel and cobalt are easily enriched in the metallic iron phase, resulting in difficulty in separation and problems such as solution purification and equipment corrosion.
Using a method of combining oxidation roasting and reduction roasting, the fayalite-type slag is first roasted in an oxidizing atmosphere at 800~1000°C to decompose into hematite and silica, and then further roasted in a reducing atmosphere at 1000~1100°C to avoid nickel Cobalt is deeply reduced; then desiliconization reaction and magnetic separation are performed during the alkali leaching process to achieve directional enrichment of nickel and cobalt.
It effectively reduces the reduction and decomposition temperature, avoids the enrichment of nickel and cobalt in the metallic iron phase, realizes the selective enrichment of nickel and cobalt and the monomer dissociation of iron, increases the added value of fayalite slag, and reduces waste. emissions, significantly improving economic benefits.
Smart Images

Figure CN114934186B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral engineering, and more specifically, relates to a method for enriching nickel and cobalt metals in fayalite-type slag. Background Art
[0002] Fayalite slag (including copper slag, nickel slag, etc.) is a solid waste generated during the smelting process of non-ferrous metals. The main phase of fayalite slag is fayalite (Fe2SiO4), and the main chemical composition is Fe and SiO2, with contents of 35~50% and 30~40% respectively. The nickel and cobalt contents in some slags are as high as 0.2~0.5%, which has reached the boundary grade of nickel and cobalt mining. Since slag is a smelting product under high temperature, the occurrence state of nickel and cobalt in it is different from their enrichment in natural mineral resources. Therefore, it is difficult to achieve the selective enrichment of nickel and cobalt in slag using traditional flotation methods.
[0003] At present, most methods for recovering nickel and cobalt from slag use wet leaching process and high-temperature pyrometallurgical reduction process. The wet leaching process will cause some other metals such as iron to dissolve into the solution while leaching nickel and cobalt, making it difficult to purify the solution. In addition, there are problems such as difficulty in circulating the leaching solution and equipment corrosion.
[0004] In the high-temperature pyrometallurgical reduction process, the direct reduction decomposition temperature of the iron olivine type slag is above 1200 ° C. At this time, the nickel and cobalt in the slag will enter the metallic iron phase due to excessive reduction. In the patent document with publication number CN110551902B, iron olivine is directly reduced and decomposed. At this time, nickel and cobalt inevitably enter the metallic iron phase. Although the effective separation of iron and silicon in the reduction product is achieved by alkali leaching later, the nickel and cobalt in the metallic iron are difficult to be further separated. The patent document with publication number CN107227401A discloses a method for preparing copper-containing and nickel-iron powder by co-reduction of copper slag and laterite nickel ore. A high-temperature reduction process is used to reduce iron-containing and nickel-containing minerals to metals and form nickel-iron alloys. Nickel recovery is subsequently achieved through grinding and magnetic separation. However, nickel is enriched in metallic iron, and subsequent separation is difficult, so it can only be used as a raw material for steelmaking. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a method for enriching nickel and cobalt metals in fayalite slag, which can effectively reduce the reduction decomposition temperature of the fayalite slag while ensuring the complete decomposition of the fayalite slag, thereby avoiding the enrichment of nickel and cobalt in the metallic iron phase during the reduction process.
[0006] To achieve the purpose of the present invention, the specific technical scheme is as follows:
[0007] A method for enriching nickel and cobalt metals in fayalite slag comprises the following steps:
[0008] (1) oxidatively roasting the ground fayalite slag at 800-1000° C. in an oxidative atmosphere to obtain an oxidatively roasted material;
[0009] (2) subjecting the oxidatively roasted material of step (1) to reduction roasting at 1000-1100° C. in a reducing atmosphere to obtain reduction roasted clinker;
[0010] (3) adding the reduction roasted clinker of step (2) into a sodium hydroxide solution or a sodium silicate solution to carry out an alkaline leaching desiliconization reaction, and after the reaction is completed, solid-liquid separation is performed to obtain a sodium silicate solution and desiliconized slag;
[0011] (4) The desiliconized slag of step (3) is subjected to magnetic separation to obtain iron concentrate and nickel-cobalt-rich tailings.
[0012] The present invention first decomposes the main iron-containing phase fayalite in the fayalite-type slag into hematite and silicon dioxide during the roasting process in an oxidizing atmosphere. After further reduction roasting of the oxidative roasted clinker, the hematite is directly reduced to metallic iron, while the silicon dioxide is converted into a quartz solid solution and a cristobalite solid solution. It can effectively avoid that nickel and cobalt are deeply reduced and enriched in the metallic iron during the reduction process. Subsequently, a low-temperature alkali leaching process is used to achieve the selective dissolution of silicon dioxide in the reduction roasting product, and metals such as nickel, cobalt, and iron are enriched in the leached slag because they do not react with alkali. At the same time, the alkali leaching and silicon dissolution process can achieve the monomer dissociation of metallic iron particles. Finally, the iron in the leached slag is effectively separated by weak magnetic separation, and at this time, nickel and cobalt are effectively enriched in the tailings because they are not in the iron particles.
[0013] Preferably, in step (1), the particle size of the ground fayalite slag is controlled to be below 200 mesh.
[0014] Preferably, in step (1), the oxidative roasting time is 20 to 120 minutes.
[0015] Preferably, in step (1), oxygen or air is introduced to form an oxidizing atmosphere.
[0016] Preferably, in step (2), the reduction roasting time is 20 to 120 minutes.
[0017] Preferably, in step (2), carbon monoxide or hydrogen is introduced to form a reducing atmosphere.
[0018] Preferably, in step (3), the reduction roasted clinker needs to be ground before the alkaline leaching desiliconization reaction to control the particle size to be below 325 mesh.
[0019] Preferably, in step (3), the concentration of the sodium hydroxide solution is in the range of 80 to 160 g / L, and the reaction liquid-to-solid ratio is in the range of 2:1 to 10:1.
[0020] Preferably, in step (3), the leaching temperature is 90-120° C., and the leaching time is 20-180 min.
[0021] Preferably, in step (4), the magnetic separation intensity is controlled at 500-2000 Gs.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] (1) The method of the present invention effectively reduces the reduction decomposition temperature of the fayalite slag while ensuring its complete decomposition, thereby avoiding the enrichment of nickel and cobalt in the metallic iron phase during the reduction process.
[0024] (2) In addition to comprehensive recovery of iron and silicon, the main chemical components of fayalite slag, the present invention realizes directional enrichment of valuable metals nickel and cobalt, thereby increasing the added value of fayalite slag, reducing waste emissions, and achieving significant economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0027] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0028] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0030] The fayalite slag used in the embodiment of the present invention is copper slag, and its chemical composition is shown in Table 1 below.
[0031] Table 1
[0032]
[0033] Example 1
[0034] The copper slag was roasted in an oxidizing atmosphere (air) at 800°C for 60 minutes, and then transferred to a reducing atmosphere (carbon monoxide) at 1000°C for roasting for 120 minutes; the obtained reduction roasted clinker was finely ground to less than 74μm, and the roasted clinker was subjected to alkaline leaching and desiliconization reaction with a sodium hydroxide solution. The leaching temperature was 110°C, the liquid-solid ratio was 10:1, the concentration of the sodium hydroxide solution was 130g / L, and the leaching time was 100min. Under these conditions, the dissolution rate of silicon oxide was 88.95%. After the reaction was completed, the solid-liquid separation was performed to obtain a sodium silicate solution and desiliconized slag; the desiliconized slag was magnetically separated under a magnetic field intensity of 500Gs to obtain an iron concentrate and a nickel-cobalt-rich tailings.
[0035] After testing, the iron recovery rate in the obtained iron concentrate was 89.25%, the iron grade was 83.36%, and the nickel and cobalt contents in the nickel-cobalt-rich tailings were 0.46% and 1.86% respectively.
[0036] Example 2
[0037] The copper slag was roasted in an oxidizing atmosphere (air) at 1000°C for 60 minutes, and then roasted in a reducing atmosphere (carbon monoxide) at 1100°C for 120 minutes; the obtained roasted clinker was finely ground to less than 74μm, and the roasted clinker was subjected to alkaline leaching and desiliconization reaction with a sodium hydroxide solution. The leaching temperature was 110°C, the liquid-solid ratio was 10:1, the concentration of the sodium hydroxide solution was 160g / L, and the leaching time was 120min. Under these conditions, the dissolution rate of silicon oxide was 92.45%. After the reaction was completed, the solid-liquid separation was performed to obtain a sodium silicate solution and desiliconized slag; the desiliconized slag was magnetically separated under a magnetic field intensity of 500Gs to obtain an iron concentrate and a nickel-cobalt-rich tailings.
[0038] After testing, the iron recovery rate in the obtained iron concentrate was 92.56%, the iron grade was 88.56%, and the nickel and cobalt contents in the nickel-cobalt-rich tailings were 0.67% and 2.12% respectively.
[0039] Example 3
[0040] The copper slag was roasted in an oxidizing atmosphere (oxygen) at 1000°C for 60 minutes, and then roasted in a reducing atmosphere (carbon monoxide) at 1100°C for 120 minutes; the obtained roasted clinker was finely ground to less than 74μm, and the roasted clinker was subjected to alkaline leaching and desiliconization reaction with a sodium hydroxide solution. The leaching temperature was 120°C, the liquid-solid ratio was 10:1, the concentration of the sodium hydroxide solution was 160g / L, and the leaching time was 120min. Under these conditions, the dissolution rate of silicon oxide was 92.63%. After the reaction was completed, the solid-liquid separation was performed to obtain a sodium silicate solution and desiliconized slag; the desiliconized slag was magnetically separated under a magnetic field strength of 1000Gs to obtain an iron concentrate and a nickel-cobalt-rich tailings.
[0041] After testing, the iron recovery rate in the obtained iron concentrate was 93.68%, the iron grade was 91.05%, and the nickel and cobalt contents in the nickel-cobalt-rich tailings were 0.77% and 2.69% respectively.
[0042] Example 4
[0043] The copper slag was roasted in an oxidizing atmosphere (oxygen) at 900°C for 60 minutes, and then roasted in a reducing atmosphere (hydrogen) at 1000°C for 120 minutes; the obtained roasted clinker was finely ground to less than 74μm, and the roasted clinker was subjected to alkaline leaching and desiliconization reaction with a sodium hydroxide solution. The leaching temperature was 110°C, the liquid-solid ratio was 10:1, the concentration of the sodium hydroxide solution was 160g / L, and the leaching time was 120min. Under these conditions, the dissolution rate of silicon oxide was 91.61%. After the reaction was completed, the solid-liquid separation was performed to obtain a sodium silicate solution and desiliconized slag; the desiliconized slag was magnetically separated under a magnetic field strength of 500Gs to obtain an iron concentrate and a nickel-cobalt-rich tailings.
[0044] After testing, the iron recovery rate in the obtained iron concentrate was 90.11%, the iron grade was 86.59%, and the nickel and cobalt contents in the nickel-cobalt-rich tailings were 0.41% and 1.91% respectively.
[0045] Example 5
[0046] The copper slag was roasted in an oxidizing atmosphere (oxygen) at 1000°C for 60 minutes, and then roasted in a reducing atmosphere (hydrogen) at 1200°C for 120 minutes; the obtained roasted clinker was finely ground to less than 74μm, and the roasted clinker was subjected to alkaline leaching and desiliconization reaction with a sodium hydroxide solution. The leaching temperature was 120°C, the liquid-solid ratio was 10:1, the concentration of the sodium hydroxide solution was 160g / L, and the leaching time was 120min. Under these conditions, the dissolution rate of silicon oxide was 92.43%. After the reaction was completed, the solid-liquid separation was performed to obtain a sodium silicate solution and desiliconized slag; the desiliconized slag was magnetically separated under a magnetic field strength of 1000Gs to obtain an iron concentrate and a nickel-cobalt-rich tailings.
[0047] After testing, the iron recovery rate in the obtained iron concentrate was 93.12%, the iron grade was 90.86%, and the nickel and cobalt contents in the nickel-cobalt-rich tailings were 0.76% and 2.89% respectively.
[0048] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the present invention.
Claims
1. A method for enriching nickel and cobalt metals in fayalite slag, characterized in that: The steps include: (1) oxidatively roasting the ground fayalite slag at 800-1000° C. in an oxidative atmosphere to obtain an oxidatively roasted material; (2) subjecting the oxidatively roasted material of step (1) to reduction roasting at 1000° C. in a reducing atmosphere to obtain reduction roasted clinker; (3) adding the reduction roasted clinker of step (2) into a sodium hydroxide solution or a sodium silicate solution to carry out an alkaline leaching desiliconization reaction, and after the reaction is completed, solid-liquid separation is performed to obtain a sodium silicate solution and desiliconized slag; (4) The desiliconized slag of step (3) is subjected to magnetic separation to obtain iron concentrate and nickel-cobalt-rich tailings.
2. The method according to claim 1, characterized in that In step (1), the particle size of the ground fayalite slag is controlled to be below 200 mesh.
3. The method according to claim 1, characterized in that In step (1), the oxidation roasting time is 20 to 120 minutes.
4. The method according to claim 1, characterized in that In step (1), oxygen or air is introduced to form an oxidizing atmosphere.
5. The method according to claim 1, characterized in that In step (2), the reduction roasting time is 20 to 120 minutes.
6. The method according to claim 1, characterized in that In step (2), carbon monoxide or hydrogen is introduced to form a reducing atmosphere.
7. The method according to claim 1, characterized in that In step (3), the reduction roasted clinker needs to be ground before the alkaline leaching desiliconization reaction to control the particle size to be below 325 mesh.
8. The method according to claim 1, characterized in that In step (3), the concentration of the sodium hydroxide solution is 80-160 g / L, and the reaction liquid-solid ratio is 2:1-10:
1.
9. The method according to claim 1, characterized in that In step (3), the leaching temperature is 90-120°C, and the leaching time is 20-180 min.
10. The method according to claim 1, characterized in that In step (4), the magnetic separation intensity is controlled at 500-2000 Gs.
Citation Information
Patent Citations
Method for preparing iron powder containing copper and nickel by coreduction of copper slag and nickel laterite ores
CN107227401A
A method for resource recovery of olivine-type slag
CN110551902B
Method for separating iron, aluminum and silicon from diasporic bauxite
CN103614547A
Method for separating and gathering ferro-nickel from laterite-nickel ore
CN103757200A
Roasting-ammonia leaching processing method for brown iron type laterite nickel ore
CN105039683A