A standard substance for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer and its preparation method
By preparing polymer standard materials containing specific elements and particle size ranges, the problems of easy deliquescence and unevenness of samples in the existing technology are solved, a more stable energy-dispersive X-ray fluorescence spectrometer standard material is achieved, and the stability and stability of the test are improved. Accuracy.
Patent Information
- Application Number
- CN202210489363.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-05-06
AI Technical Summary
In existing energy dispersive X-ray fluorescence spectrometers, metal oxide samples have problems such as easy deliquescence, unevenness and poor performance stability, which affects test accuracy.
Standard materials prepared from aluminum oxide, manganese oxide, copper oxide, yttrium trioxide, silver oxide, polyethylene wax, polypropylene and polyethylene are used to granulate through vacuum oven drying and twin-screw extruder granulator. Combined with the injection molding preparation method of the injection molding machine, the content and particle size range of each element are controlled to ensure the deliquescence resistance, uniformity and stability of the standard material.
The obtained standard material has no deliquescence in a humidity environment of 30°C and 75% RH. The relative standard deviation of 5 pieces of the standard material is within 1%, and the nonlinear energy change within 6 months is within 0.05%. It is resistant to deliquescence, has good uniformity and It has good stability and is suitable for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer.
Smart Images

Figure CN114935580B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metrological standard substances, and in particular relates to a standard substance for energy nonlinear evaluation of an energy dispersion X-ray fluorescence spectrometer and a preparation method thereof. Background Art
[0002] Energy dispersive X-ray fluorescence spectrometer (EDXRF for short) is an instrument that can rapidly, non-destructively and over a wide range measure multiple elements in various samples. It is widely used in minerals, medicine, metals, petroleum and other fields.
[0003] The principle of EDXRF's ability to detect multiple elements in a sample is that different elements in the sample will emit characteristic responses of different energies after being irradiated by X-rays, such as the Ka1 characteristic response of the Ti element at 4.512Kev, the Ka1 characteristic response of the Cr element at 5.414Kev, etc. By detecting these characteristic responses, EDXRF can achieve qualitative and quantitative analysis of multiple elements in the sample. The characteristic response of each element is a natural constant, and its theoretical characteristic response is a fixed value. However, due to various factors such as the detection capability of the EDXRF detector, signal transmission, and software algorithms, there will be a certain deviation between the characteristic response actually detected by EDXRF and the theoretical characteristic response of each element, thus affecting the test accuracy.
[0004] The current mainstream method for evaluating the degree of deviation is to calculate the energy nonlinearity of EDXRF. The specific steps are as follows: (1) Mix metal oxides of multiple different elements (usually no less than 4 elements) and press them into samples through boric acid; (2) Measure the characteristic response of each element in the sample respectively; (3) Eliminate one element from the multiple elements (usually the element with the characteristic response in the middle position), establish a linear working curve between the measured characteristic response of the remaining elements and the theoretical characteristic response to obtain a linear equation; (4) Calculate the characteristic response of the eliminated element through this linear equation; (5) Subtract the measured characteristic response from the calculated characteristic response, take the absolute value and divide it by the maximum energy value, which is the energy nonlinearity.
[0005] The above-mentioned samples are made by pressing metal oxides and boric acid into tablets, and have problems such as easy deliquesce, unevenness, and poor performance stability.
[0006] Therefore, how to overcome the above-mentioned problems of samples and obtain more stable and uniform standard substances has become one of the problems to be solved urgently in this field. Summary of the invention
[0007] The present invention aims at the blank of the prior art and provides a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer and a preparation method thereof. The standard substance is prepared from aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene and polyethylene. The standard substance has a wide concentration range, covers a wide range of element contents, has the characteristics of deliquescence resistance, good uniformity and good stability, etc., and can be used as a standard substance for an energy dispersive X-ray fluorescence spectrometer to evaluate the energy nonlinearity of the instrument.
[0008] The specific technical solution of the present invention is:
[0009] A standard substance for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer, the component contents of which are calculated by weight percentage:
[0010] Aluminum oxide 1.89% to 9.44%, manganese dioxide 1.58% to 7.91%, copper oxide 1.25% to 6.26%, yttrium oxide 1.27% to 6.35%, silver oxide 1.07% to 5.37%, polyethylene wax 2% to 4%, polypropylene 3% to 8%, and the balance polyethylene;
[0011] The aluminum oxide content corresponds to the Al element content of 1% to 5%;
[0012] The manganese dioxide content corresponds to the Mn element content of 1% to 5%;
[0013] The copper oxide content corresponds to the Cu element content of 1% to 5%;
[0014] The Y content of yttrium trioxide corresponds to 1% to 5% of the Y element content;
[0015] The silver oxide content corresponds to the Ag element content of 1% to 5%;
[0016] Furthermore, the particle sizes of various metal oxides are:
[0017] The particle size of aluminum oxide is 400-500 mesh;
[0018] The particle size of manganese dioxide is 500-600 mesh;
[0019] The particle size of copper oxide is 200-300 mesh;
[0020] The particle size of yttrium trioxide is 2000 mesh to 2500 mesh;
[0021] The particle size of silver oxide is 400-600 mesh.
[0022] Too fine or too coarse particles will affect their dispersion in polyethylene, resulting in poor uniformity. The above range is the optimal particle size range.
[0023] In addition to this, the melt index of polypropylene is 70-80 g / 10 min;
[0024] The polyethylene has a melt index of 25-30 g / 10 min, and can be specifically selected from high-density polyethylene (HDPE);
[0025] The molecular weight of polyethylene wax is 4000-5000.
[0026] The more preferred amount of polyethylene wax is 3%-4%; the more preferred amount of polypropylene is 5%-6%.
[0027] The use of polyethylene as the base material in combination with the above-mentioned auxiliary materials can stabilize the final standard substance, improve its dispersibility, and make it more evenly dispersed.
[0028] The method for preparing the above-mentioned standard material for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer comprises the following steps:
[0029] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0030] (2) Extruding all raw materials through a twin-screw extruder for granulation for 3 times, the granulation temperature is 170-180° C., the screw aspect ratio is 48-64, and the screw speed is 500-600 r / min;
[0031] (3) The sample was injected into the injection molding machine. The injection molding temperature was divided into 4 zones: zone 1 160-170°C, zone 2 170-180°C, zone 3 180-190°C, and nozzle zone 200°C. Screw speed: 80-90r / min, injection pressure 12Mpa, and molding cycle 180s.
[0032] The target standard substance can be obtained through the above steps and can be directly used as a standard substance for energy dispersive X-ray fluorescence spectrometer.
[0033] The types, proportions, mesh sizes and other parameters of the above-mentioned raw materials, as well as the preparation methods and processing parameters are screened by the inventors from a variety of raw materials, processing methods and parameters through a large number of experiments, in order to ensure that the prepared standard substances can be used for the evaluation of energy nonlinearity of energy dispersive X-ray fluorescence spectroscopy, and at the same time have the advantages of deliquescence resistance, good uniformity and good stability.
[0034] In summary, the standard material for energy nonlinearity evaluation of energy dispersive X-ray fluorescence spectrometer provided in the present application is stored in a humidity box at 30°C and 75% RH for 24 hours without deliquescence or breakage; the relative standard deviation of 5 pieces of standard material is within 1%; the energy nonlinearity change in 6 months is within 0.05%; it has the advantages of deliquescence resistance, good uniformity and good stability, and can be used as a standard material for energy dispersive X-ray fluorescence spectrometer for evaluation of the energy nonlinearity of the instrument. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The standard substance prepared in Example 1 was tested by EDXRF, and the fitting working curves of the measured characteristic responses of Al, Mn, Y, and Ag and the theoretical characteristic responses were established.
[0036] Figure 2 The standard substance prepared in Example 1 was tested by another EDXRF, and the fitting working curves of the measured characteristic responses of Al, Mn, Y, and Ag and the theoretical characteristic responses were established.
[0037] Figure 1 and Figure 2 The corresponding data are shown in Table 1 and Table 2, respectively, from which it can be seen that the standard substance of the present invention can well distinguish the difference in energy nonlinearity of the two instruments.
[0038] Table 1 Figure 1 Corresponding data
[0039]
[0040] Table 2 Figure 2 Corresponding data
[0041]
[0042] Figure 3 After the standard substance prepared in Example 1 was stored for 6 months, Figure 1 For the same EDXRF test, the fitting working curves established by comparing the measured characteristic responses of Al, Mn, Y, and Ag with the theoretical characteristic responses are
[0043] Figure 3 The corresponding data are shown in Table 3, from which it can be seen that after the standard substance of the present invention is stored for 6 months, the fitting working curve established is basically the same as that 6 months ago ( Figure 1 ), indicating that the standard substance has good stability.
[0044] Table 3 Figure 3 Corresponding data
[0045]
[0046] Figure 4The sample prepared in Comparative Example 1 was used Figure 1 The same EDXRF was tested on the same day, and the fitting working curves were established by comparing the measured characteristic responses of Al, Mn, Y, and Ag with the theoretical characteristic responses.
[0047] Figure 5 After the sample prepared in Comparative Example 1 was stored for 6 months, Figure 3 The same EDXRF was tested on the same day, and the fitting working curves were established by comparing the measured characteristic responses of Al, Mn, Y, and Ag with the theoretical characteristic responses.
[0048] Figure 4 and Figure 5 The corresponding data are shown in Tables 4 and 5, respectively. It can be seen that after 6 months of storage, the energy nonlinear data of the sample prepared by boric acid tabletting is very different from the results 6 months ago, and the stability is far worse than that of the standard substance of the present invention.
[0049] Table 4 Figure 4 Corresponding data
[0050]
[0051] Table 5 Figure 5 Corresponding data
[0052] DETAILED DESCRIPTION
[0053] The present invention is further described below in conjunction with the embodiments, which can enable those skilled in the art to more fully understand the present invention, but does not limit the present invention in any way.
[0054] Example 1
[0055] The invention discloses a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer, which contains, by mass percentage, 1.89% of aluminum oxide, 3.16% of manganese dioxide, 3.76% of copper oxide, 5.08% of yttrium oxide, 5.37% of silver oxide, 3% of polyethylene wax, 6% of polypropylene, and the balance of polyethylene.
[0056] The melt index of the polyethylene used is 25g / 10min, the melt index of the polypropylene is 75g / 10min, the polyethylene is high-density polyethylene (HDPE), the molecular weight of the polyethylene wax is 4000, the particle size of aluminum oxide is 500 mesh, the particle size of manganese dioxide is 550 mesh, the particle size of copper oxide is 200 mesh, the particle size of yttrium oxide is 2500 mesh, and the particle size of silver oxide is 600 mesh.
[0057] The preparation method comprises the following steps:
[0058] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0059] (2) All raw materials were extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 170° C., a screw aspect ratio of 64, and a screw speed of 550 r / min;
[0060] (3) The sample was injection molded by an injection molding machine. The injection temperature was divided into 4 zones, zone 1 160°C, zone 2 175°C, zone 3 185°C, and nozzle zone 200°C. Screw speed: 90r / min, injection pressure 12Mpa, and molding cycle 180s.
[0061] Example 2
[0062] The invention discloses a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer, which contains, by mass percentage, 3.57% of aluminum oxide, 1.58% of manganese dioxide, 6.26% of copper oxide, 6.35% of yttrium oxide, 2.48% of silver oxide, 2% of polyethylene wax, 4% of polypropylene, and the balance of polyethylene.
[0063] The melt index of the polyethylene used is 28 g / 10 min, the melt index of the polypropylene is 80 g / 10 min, the polyethylene is high-density polyethylene (HDPE), the molecular weight of the polyethylene wax is 5000, the particle size of aluminum oxide is 400 mesh, the particle size of manganese dioxide is 500 mesh, the particle size of copper oxide is 250 mesh, the particle size of yttrium oxide is 2000 mesh, and the particle size of silver oxide is 500 mesh.
[0064] The preparation method comprises the following steps:
[0065] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0066] (2) All raw materials were extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 175° C., a screw aspect ratio of 48, and a screw speed of 500 r / min;
[0067] (3) The sample was injection molded by an injection molding machine. The injection molding temperature was divided into 4 zones, zone 1 170°C, zone 2 170°C, zone 3 180°C, and nozzle zone 200°C. Screw speed: 85r / min, injection pressure 12Mpa, and molding cycle 180s.
[0068] Example 3
[0069] The invention discloses a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer, which contains, by mass percentage, 6.42% of aluminum oxide, 5.36% of manganese dioxide, 1.25% of copper oxide, 4.36% of yttrium oxide, 3.55% of silver oxide, 3.5% of polyethylene wax, 3% of polypropylene, and the balance of polyethylene.
[0070] The melt index of the polyethylene used is 30g / 10min, the melt index of the polypropylene is 70g / 10min, the polyethylene is low-density polyethylene (LDPE), the molecular weight of the polyethylene wax is 4500, the particle size of aluminum oxide is 450 mesh, the particle size of manganese dioxide is 550 mesh, the particle size of copper oxide is 250 mesh, the particle size of yttrium oxide is 2200 mesh, and the particle size of silver oxide is 400 mesh.
[0071] The preparation method comprises the following steps:
[0072] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0073] (2) All raw materials were extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 180° C., a screw aspect ratio of 48, and a screw speed of 600 r / min;
[0074] (3) The sample was injection molded by an injection molding machine. The injection temperature was divided into 4 zones, zone 1 160°C, zone 2 180°C, zone 3 185°C, and nozzle zone 200°C. Screw speed: 90r / min, injection pressure 12Mpa, and molding cycle 180s.
[0075] Example 4
[0076] The invention discloses a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer, which contains, by mass percentage, 4.31% of aluminum oxide, 7.91% of manganese dioxide, 3.55% of copper oxide, 1.27% of yttrium oxide, 4.86% of silver oxide, 4% of polyethylene wax, 8% of polypropylene, and the balance of polyethylene.
[0077] The melt index of the polyethylene used is 28 g / 10 min, the melt index of the polypropylene is 72 g / 10 min, the polyethylene is low-density polyethylene (LDPE), the molecular weight of the polyethylene wax is 4000, the particle size of aluminum oxide is 500 mesh, the particle size of manganese dioxide is 600 mesh, the particle size of copper oxide is 300 mesh, the particle size of yttrium oxide is 2000 mesh, and the particle size of silver oxide is 400 mesh.
[0078] The preparation method comprises the following steps:
[0079] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0080] (2) All raw materials were extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 175° C., a screw aspect ratio of 56, and a screw speed of 500 r / min;
[0081] (3) The sample was injection molded by an injection molding machine. The injection molding temperature was divided into 4 zones, zone 1 165°C, zone 2 175°C, zone 3 190°C, and nozzle zone 200°C. Screw speed: 85r / min, injection pressure 12Mpa, and molding cycle 180s.
[0082] Example 5
[0083] The invention discloses a standard substance for energy nonlinear evaluation of an energy dispersive X-ray fluorescence spectrometer, which contains, by mass percentage, 9.44% of aluminum oxide, 6.22% of manganese dioxide, 2.38% of copper oxide, 3.22% of yttrium oxide, 1.07% of silver oxide, 2.5% of polyethylene wax, 5% of polypropylene, and the balance of polyethylene.
[0084] The melt index of the polyethylene used is 26 g / 10 min, the melt index of the polypropylene is 70 g / 10 min, the polyethylene is high-density polyethylene (HDPE), the molecular weight of the polyethylene wax is 5000, the particle size of aluminum oxide is 400 mesh, the particle size of manganese dioxide is 600 mesh, the particle size of copper oxide is 200 mesh, the particle size of yttrium oxide is 2500 mesh, and the particle size of silver oxide is 600 mesh.
[0085] The preparation method comprises the following steps:
[0086] (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours;
[0087] (2) All raw materials were extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 170° C., a screw aspect ratio of 64, and a screw speed of 550 r / min;
[0088] (3) The sample was injection molded by an injection molding machine. The injection temperature was divided into 4 zones, zone 1 170°C, zone 2 170°C, zone 3 180°C, and nozzle zone 200°C. Screw speed: 80r / min, injection pressure 12Mpa, and molding cycle 180s.
[0089] Comparative Example 1
[0090] 1.89% aluminum oxide, 3.16% manganese dioxide, 3.76% copper oxide, 5.08% yttrium oxide, 5.37% silver oxide and the remainder of boric acid were mixed and ground for 30 minutes, and pressed into sample tablets by a tablet press.
[0091] The test results of the standard substances obtained in Examples 1-5 and Comparative Example 1 are as follows, where:
[0092] (1) Environmental stability was evaluated by storing the standard substance in a temperature and humidity chamber at 30°C and 75% RH for 24 h.
[0093] (2) Homogeneity: The signal intensity of the standard material is tested by EDXRF and evaluated by the relative standard deviation of the measurement results of 5 pieces. The smaller the relative standard deviation, the better.
[0094] (3) Performance stability was evaluated by measuring the energy nonlinearity of the EDXRF of the same instrument and based on the difference between the measured values before and after 6 months. The smaller the difference, the better. The results are shown in the following table:
[0095]
[0096]
[0097] It can be seen from the test results of comparative example 1 in the above table that the standard substance prepared by the boric acid tabletting method is not resistant to deliquescence, and its uniformity and stability are poor; it can be seen from the test results of Examples 1 to 5 that the standard substance prepared by the present invention is resistant to deliquescence, and has good uniformity and stability.
[0098] The above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention is described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A standard substance for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer, characterized in that: The component contents are calculated by weight percentage: Aluminum oxide 1.89% to 9.44%, manganese dioxide 1.58% to 7.91%, copper oxide 1.25% to 6.26%, yttrium oxide 1.27% to 6.35%, silver oxide 1.07% to 5.37%, polyethylene wax 2% to 4%, polypropylene 3% to 8%, and the balance polyethylene; The particle size of aluminum oxide is 400-500 mesh; the particle size of manganese dioxide is 500-600 mesh; the particle size of copper oxide is 200-300 mesh; the particle size of yttrium oxide is 2000-2500 mesh; the particle size of silver oxide is 400-600 mesh; the melt index of polypropylene is 70-80 g / 10min; and the melt index of polyethylene is 25-30 g / 10min.
2. The standard material for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer according to claim 1, characterized in that: The polyethylene is selected from high-density polyethylene; the molecular weight of the polyethylene wax is 4000-5000.
3. The standard material for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer according to claim 1, characterized in that: The dosage of polyethylene wax is 3%-4%; the dosage of polypropylene is 5%~6%.
4. The method for preparing the standard substance for energy nonlinear evaluation of energy dispersive X-ray fluorescence spectrometer according to claim 1, characterized in that: The following steps are involved: (1) Aluminum oxide, manganese dioxide, copper oxide, yttrium oxide, silver oxide, polyethylene wax, polypropylene, and polyethylene were dried in a vacuum oven at 60°C and 0.01 atmosphere for 6 hours; (2) All raw materials are extruded and granulated three times in a twin-screw extruder granulator, with a granulation temperature of 170-180°C, a screw aspect ratio of 48-64, and a screw speed of 500-600 r / min; (3) The sample was injection molded by an injection molding machine. The injection molding temperature was divided into four zones: zone 1 160-170°C, zone 2 170-180°C, zone 3 180-190°C, nozzle zone 200°C, screw speed: 80-90 r / min, injection pressure 12 MPa, and molding cycle 180 s.
Citation Information
Patent Citations
Nano-silver granularity standard substance and preparation method thereof
CN108627528A
Testing method of zinc oxide and alkali metal in fly ash
CN109580326A
Plastic standard material and its manufacturing method
JP2004257809A
Drift correction sample for fluorescent x-ray analysis, fluorescent x-ray analysis method using the same, and method of manufacturing the same
JP2010204087A
The standard material for polyethylene resin analysisand the non-destructive quantitative analysis ofenvironmetal hazadous elements in polyethylene resin
KR1020050112376A