A Zn-Se based alloy prepared directly by mechanical processing and its preparation method and application
By applying and laminating metal powder on Zn plates and performing hot rolling treatment, the complex preparation process of Zn-Se-based alloys in the prior art has been solved, and efficient alloying and mechanical properties have been achieved, and suitable for biomedical applications. .
Patent Information
- Application Number
- CN202210574043.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-25
AI Technical Summary
In the prior art, the preparation of Zn-Se-based alloys is complex and lengthy, and it is difficult to directly obtain efficient alloying effects through mechanical processing, and the mechanical properties of zinc alloys are not sufficient to meet biomedical applications.
By applying the solution containing metal powder on the Zn plate, stacking and preheating and single pass hot rolling, repeating the cutting-laminate-preheating-hot rolling process, controlling the temperature and deformation amount, and promoting the Zn-Se-based Alloy, acetone dispersed metal powder is used to ensure good brushing and drying.
It realizes the direct acquisition of Zn-Se-based alloy through mechanical processing, improves its mechanical properties and biocompatibility, and is suitable for anti-tumor degradable implantable materials.
Smart Images

Figure CN114951278B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradable zinc alloys, and in particular to a Zn-Se based alloy prepared directly by mechanical processing, and a preparation method and application thereof. Background Art
[0002] At present, bio-zinc-based biodegradable metal materials are considered to be potential new biomaterials that can be used as biodegradable implants. Compared with magnesium-based and iron-based materials, zinc-based biodegradable metal materials have ideal degradation rates. Zinc-based materials show attractive properties, making them potential alternatives for biomedical applications. However, the mechanical properties of pure zinc are not sufficient to meet the requirements of medical implants. Therefore, zinc alloy biodegradable biomaterials are mainly treated by adding alloying elements, rapid solidification, heat treatment, and deformation, etc., to effectively improve the mechanical properties of zinc alloys on the basis of meeting biocompatibility and degradation performance.
[0003] Selenium (Se) is one of the essential trace elements for the human body. Since the human body cannot synthesize selenium itself, it must be taken in from the outside to meet the needs of the human body, and more than 90% of this comes from food. Therefore, the daily intake of selenium is directly affected by the selenium content of food, and indirectly affected by the selenium content in water and soil in the environment and eating habits.
[0004] However, the Zn-Se phase diagram shows that the melting point of Zn is 420°C and the boiling point is 907°C, while the melting point of Se is 220°C and the boiling point is 685°C. The melting and boiling points are low, and the volatility is high and difficult to dissolve. More importantly, the solid solubility between Zn and Se is extremely poor. In the prior art, the micro-nanoscale Zn-Se alloy can only be obtained by deposition method.
[0005] The patent (CN113737056A) obtains a bulk Zn-Se based alloy material by combining smelting, casting with mechanical processing and heat treatment. It can be seen that the process flow is relatively lengthy. Summary of the invention
[0006] In view of the shortcomings of the prior art, the first object of the present invention is to provide a Zn-Se based alloy prepared directly by mechanical processing and a preparation method and application thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The invention discloses a method for preparing a Zn-Se based alloy directly prepared by mechanical processing, comprising the steps of: applying a solution containing metal powder on a Zn plate, and then stacking at least two Zn plates coated with metal powder to obtain a composite plate, preheating the composite plate at a temperature below 200°C, and then performing single-pass hot rolling to obtain a hot-rolled plate, cutting the hot-rolled plate into two pieces from the middle, stacking, preheating, and then performing single-pass hot rolling, and repeating cutting-stacking-preheating-single-pass hot rolling for 5 to 11 times to obtain a Zn-Se based alloy, wherein the metal in the metal powder contains Se.
[0009] In the preparation method of the present invention, the composite plate obtained by stacking Zn plates coated with Se powder is first preheated below 200°C, which is close to the melting point of Se. Preheating is beneficial to the combination of Se and the Zn plate surface. The mechanical processing method of rolling is directly performed after preheating, which can cause the zinc alloy to recrystallize and promote direct alloying with Se during the rolling process, so that the Zn-Se based alloy is obtained only through mechanical processing.
[0010] A preferred solution is to take three Zn plates, coat two of the Zn plates with a solution containing metal powder on one side, coat the other Zn plate on both sides, place the Zn plate coated with metal powder on both sides in the middle, and stack the other two Zn plates coated with metal powder on one side in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides, to obtain a composite plate.
[0011] The inventors have found that by stacking in the form of a sandwich, more alloying elements can be introduced in a more controllable manner to obtain better performance.
[0012] In a preferred embodiment, the process of obtaining the solution containing metal powder is to disperse the metal powder in acetone and then vibrate in ultrasound for 5-30 minutes.
[0013] The inventors have found that using acetone to disperse the metal powder can ensure that the metal powder is well dispersed and is easy to dry after painting.
[0014] In a preferred embodiment, in the solution containing metal powder, the particle size of the metal powder is 30-50 µm and the purity is ≥ 99.9%.
[0015] The inventors found that the particle size of the metal powder needs to be effectively controlled. If the particle size is too small, it cannot be dispersed and will agglomerate, and it is easy to be lost during the drying process. If the particle size is too large, it will affect the combination of the metal powder and the Zn plate, thereby resulting in a poor alloying effect.
[0016] Preferably, the purity of the Zn plate is ≥99.9%.
[0017] In the actual operation process, the side of the Zn plate to which the powder is to be attached is first roughened with an electric drill, and then holes are drilled at the four corners of the Zn plate and fixed with thin copper wires. The Zn plate is then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying, and then the solution containing metal powder is brushed on the rough surface of the Zn plate.
[0018] In a preferred embodiment, the roughness of the Zn plate is flat-ground Ra0.2-0.8.
[0019] The inventors found that the roughness of the Zn plate needs to be effectively controlled. If the roughness is not enough, it will not only affect the amount of powder added, but also the plates will not be able to bond together.
[0020] Preferably, the composite plate is preheated at 150-200° C. for 5-30 min.
[0021] Preheating allows the Se powder to better bond with the surface of the Zn plate during the rolling process to achieve alloying.
[0022] In a preferred embodiment, the deformation of the composite plate in a single hot rolling process is 30%-50%.
[0023] The inventors have found that by controlling the deformation of the composite plate in a single hot rolling process within the above range, the metal powder and the plate can be well metallurgically bonded while avoiding cracking.
[0024] The preferred solution is that the hot-rolled plate is cut into two pieces from the middle, stacked, preheated, and then hot-rolled in a single pass. In the process of repeated cutting-stacking-preheating-single-pass hot rolling, the preheating temperature is 150-200°C, the preheating time is 5-30 minutes, and the deformation amount of each single-pass hot rolling is controlled to be equal and 30%-50%.
[0025] The inventors found that by adopting the above method, the single-pass hot-rolled plates are cut and then stacked, and then hot-rolled together, the thickness is increased, which is equivalent to a protective covering for the plates, making cracks less likely to occur and allowing the plates to be better combined.
[0026] In a preferred embodiment, the metal in the metal powder is selected from at least one of Ag, Cu, Sn, Mg and Se and contains Se.
[0027] More preferably, the metal in the metal powder is selected from at least one of Cu, Mg and Se and contains Se.
[0028] In a preferred embodiment, in the Zn-Se based alloy, by mass percentage, Se is 0.1% to 10%, X is 0 to 10%, and the balance is Zn, wherein X is selected from at least one of Ag, Cu, Sn, and Mg.
[0029] Further preferably, in the Zn-Se based alloy, by mass percentage, Se is 0.8% to 1.5%, and the balance is Zn. The inventors found that when the composition of the Zn-Se based alloy is controlled within the above range, the anti-tumor performance is optimal.
[0030] Further preferably, in the Zn-Se based alloy, by mass percentage, Se is 0.8% to 1.5%, X is 0.6% to 2.5%, and the balance is Zn, wherein X is selected from at least one of Cu and Mg. The inventors have found that when the composition of the Zn-Se based alloy is controlled within the above range, the mechanical properties are optimal.
[0031] The present invention also provides a Zn-Se based alloy prepared by the above preparation method.
[0032] The present invention also provides application of the Zn-Se based alloy prepared by the above preparation method, and the Zn-Se based alloy is used as an anti-tumor degradable implant material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.
[0034] Figure 1 Metallographic microstructure of the Zn-Se alloy with Se powder added after cumulative rolling in Example 1.
[0035] Figure 2 SEM image and EDS result of the Zn-Se alloy with Se powder added after cumulative rolling in Example 1.
[0036] Figure 3 The tensile deformation curve and corresponding tensile performance data and hardness value of the Zn-Se alloy to which Se powder was added after cumulative rolling in Example 1. DETAILED DESCRIPTION
[0037] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0038] Embodiment 1:
[0039] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9%, with a powder particle size of 50µm. Se powder was weighed according to the mass ratio of the two elements in the sample. The side of the Zn plate to which the powder was to be attached was first roughened with an electric drill to a roughness of Ra0.4. Then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The powder was dispersed in an acetone solution, and the acetone solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The dispersed powder was brushed on the Zn plate with a brush, and the plate was weighed before and after the powder was brushed to calculate the powder content ratio. A solution containing metal powder is applied to single-side coating of two of the Zn plates and to double-side coating of the other Zn plate. The Zn plate coated with metal powder on both sides is placed in the middle. The other two Zn plates coated with metal powder on one side are stacked in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
[0040] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 10 times.
[0041] Specific data:
[0042] 1. The relative mass content of Se element in the Zn-Se laminated plate prepared in this embodiment is measured by X-ray fluorescence spectroscopy (XRF) to be 1.1%, and the rest is Zn.
[0043] 2. Figure 1 The metallographic microstructure of the Zn-Se alloy after cumulative rolling. In the Zn-Se sample, the layered microstructure along the rolling distribution can be seen. The overall metallographic structure shows a gray ZnSe phase structure, the stratification between the interfaces is not obvious, and there are a small amount of black Se single particles. After cumulative rolling, the Se single particles are extremely small, indicating that the rolling process effectively refines the structure and promotes mechanical alloying.
[0044] Figure 2The SEM image and EDS results of the Zn-Se sample after cumulative rolling treatment. The sample is mainly composed of a Zn phase with a close-packed hexagonal structure. After multiple cumulative rolling, EDS detection revealed that Se powder and synthesized ZnSe phase existed between the Zn plates, indicating that after cumulative rolling treatment, the Zn-Se plate sample underwent a phase change, achieved mechanical alloying, and promoted the fusion of Se powder and Zn plate. Se-rich ZnSe phases were generated between some Se particles and Zn, eliminating the interface between ZnSe and melted into the Zn matrix, which is consistent with the Figure 1 The change trend of the metallographic structure is consistent.
[0045] Figure 3 The tensile deformation stress-strain curve and the corresponding compression performance data and hardness value are obtained after accumulating 7 times of rolling. The tensile yield strength (CYS), tensile ultimate strength (UCS), elongation and hardness of the Zn-Se sample were 90.57MPa, 99.68MPa, 1.33% and 69.3HV at the 7th time. At the 8th time, they were 137.4MPa, 156.4MPa, 18.67% and 85.4HV, at the 9th time, they were 164.2MPa, 181.3MPa, 21.72% and 93.5HV, and at the 10th time, they were 184.3MPa, 199.7MPa, 29.48% and 111.7HV. And with the increase of the cumulative number of rolling, the strength, hardness and ductility of the alloy sample have been improved. After the cumulative rolling was carried out for 10 times, the sample had broken and could not be rolled further.
[0046] The electrochemical corrosion test in Hank's solution showed that the seventh corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se sample were -0.996 V, 0.632 μA / cm 2 and 20.80 mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -0.978V, 0.520 μA / cm 2 and 17.12 mm / y. The 9th corrosion potential, corrosion current density and corrosion rate are -0.982V, 0.418 μA / cm 2 and 13.75 mm / y. The 10th corrosion potential, corrosion current density and corrosion rate are -0.991V, 0.386μA / cm 2and 12.70 mm / y. With the increase of the number of rolling, the sample showed a slower corrosion current density and corrosion rate, making it have better corrosion resistance. After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the 7th rolling Zn-Se sample was 0.45 mm / y, the corrosion rate of the 8th rolling was 0.41 mm / y, the corrosion rate of the 9th rolling was 0.38 mm / y, and the corrosion rate of the 10th rolling was 0.31 mm / y. It is consistent with the change law of the data measured in the electrochemical corrosion experiment.
[0047] The effect of cumulative rolling samples on cell viability was tested in MC3T3 cells. The culture solution of the sample soaked after 10 cumulative rollings was diluted to different concentrations and cultured with MC3T3 cells for 3 days, and the cell viability in the culture dish was detected. The test results showed that when the cell immersion solution was diluted to 25% and 12.5%, the cell viability was higher than 100%, indicating that the alloy had zero cytotoxicity at this time and had complete biocompatibility. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of Zn-Se alloy inactivating bone cancer cells was 74% after 10 cumulative rollings. It shows that the cumulatively rolled Zn-Se alloy sample has a certain bone cancer inactivation rate, meets the requirements of clinical medical biomaterials, and has excellent biomedical value.
[0048] Example 2 (Mg added)
[0049] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9%, Se powder with a purity of 99.9%, and Mg powder with a purity of 99.9%, with a powder particle size of 50µm. The weights were weighed according to the mass ratio of each element contained in the sample, and the Se content was controlled at 1% and the Mg content was controlled at 1%. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.4, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. Se powder and Mg powder were mixed according to the mass ratio and dispersed in an acetone solution. The dispersed solution with powder was placed in an ultrasonic oscillation for 30 minutes. The powder was brushed on the Zn plate with a brush, and the stacked plates were weighed before and after the powder was brushed to calculate the powder content ratio. A solution containing metal powder is applied to single-side coating of two of the Zn plates and to double-side coating of the other Zn plate. The Zn plate coated with metal powder on both sides is placed in the middle. The other two Zn plates coated with metal powder on one side are stacked in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
[0050] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 9 times.
[0051] Implementation Effect
[0052] The relative mass content of Se element in the cumulative roll-bonded Zn-Se-Mg sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.96%, Mg content to be 0.8%, and the rest to be Zn. In the metallographic microstructure observation, it was found that the layered microstructure structure distributed along the rolling can be seen in the Zn-Se-Mg sample, and the overall metallographic structure shows a gray ZnSe phase structure, fine stratification can be seen between the interfaces, and there are a small amount of black Se single particles. After the cumulative roll-bonding, the Se single particles are extremely small, indicating that the roll-bonding process effectively refines the organization and promotes mechanical alloying. After adding Mg powder, the cumulative roll-bonding times reached 9 times. After the 9th time, the sample had serious cracks and could not continue the roll-bonding work. The relevant data were measured from the 8th time. At the 8th time, they were 140.4MPa, 182.4MPa, 9.71% and 92.1HV respectively. At the 9th time, they were 209.5MPa, 230.2MPa, 7.17% and 118.3HV respectively. With the increase of cumulative rolling times, the mechanical properties are also increasing. Electrochemical corrosion tests in Hank's solution showed that the 8th corrosion potential, corrosion current density and corrosion rate were -1.102V, 0.832 μA / cm 2 and 31.95 mm / y. The 9th corrosion potential, corrosion current density and corrosion rate are -1.110V, 0.701μA / cm 2 and 26.92 mm / y. With the increase of the number of rolling laps, the powder in the sample is more evenly distributed in the matrix, thus showing a slower corrosion current density and corrosion rate, making it have better corrosion resistance.
[0053] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se-Mg sample with the 9th cumulative rolling was 0.43mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se-Mg alloy sample inactivating bone cancer cells after 9 cumulative rolling reached 52%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0054] Example 3 (adding Cu)
[0055] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9%, Se powder with a purity of 99.9%, and Cu powder with a purity of 99.9%, with a powder particle size of 50µm. And weigh according to the mass ratio of each element contained in the sample, the Se content is controlled at 1%, and the Cu content is controlled at 3%. First, use an electric drill to roughen the side of the Zn plate where the powder is to be attached, and the roughness reaches Ra0.4, then drill holes in the four corners of the Zn plate and fix it with fine copper wire, then clean and dry the Zn plate with alcohol, and then put it in acetone solution for cleaning, degreasing and drying. Mix Se powder and Cu powder according to the mass ratio and disperse them in acetone solution, and put the dispersed solution with powder into ultrasonic vibration for 30 minutes. Brush the powder on the Zn plate with a brush, and weigh the stacked plates before and after brushing the powder to calculate the powder content ratio. A solution containing metal powder is applied to single-side coating of two of the Zn plates and to double-side coating of the other Zn plate. The Zn plate coated with metal powder on both sides is placed in the middle. The other two Zn plates coated with metal powder on one side are stacked in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
[0056] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 9 times.
[0057] Implementation Effect
[0058] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.95%, the content of Cu was 2.1%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure structure distributed along the rolling can be seen in the Zn-Mg-Se sample, the overall metallographic structure shows a gray ZnSe phase structure, and fine stratification can be seen between the interfaces. After adding Cu powder, the cumulative number of lap rolling reached 9 times, and the relevant data was measured from the 7th time. At the 7th time, they were 134.4MPa, 149.8MPa, 31% and 85.6HV respectively. At the 8th time, they were 144.6MPa, 152.8MPa, 24% and 89.7HV respectively, and at the 9th time, they were 198.2MPa, 201.3MPa, 15% and 102.5HV respectively. With the increase of the cumulative number of lap rolling, the mechanical properties are also increasing. Electrochemical corrosion tests in Hank's solution showed that the seventh corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se-Cu sample were -0.997 V, 0.798 μA / cm 2and 31.85mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -0.978V, 0.711μA / cm 2 and 29.63 mm / y. The 9th corrosion potential, corrosion current density and corrosion rate are -1.001 V, 0.633 μA / cm 2 and 24.12 mm / y. With the increase of the number of rolling laps, the sample showed a slower corrosion current density and corrosion rate, which made it have better corrosion resistance.
[0059] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se-Cu sample with the 9th cumulative rolling was 0.37mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se-Cu alloy sample inactivating bone cancer cells after 9 cumulative rolling reached 48%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0060] Example 4 (Ag powder)
[0061] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9%, Se powder with a purity of 99.9%, and Ag powder with a purity of 99.9%, with a powder particle size of 50µm. And weigh according to the mass ratio of each element contained in the sample, first use an electric drill to roughen the side of the Zn plate where the powder needs to be attached, and the roughness reaches Ra0.4, then drill holes in the four corners of the Zn plate, and fix it with fine copper wire, then clean and dry the Zn plate with alcohol, and then put it in acetone solution for cleaning, degreasing and drying. Mix the powders according to the mass ratio and disperse them in acetone solution, and put the dispersed solution with powder into ultrasonic vibration for 30 minutes. Brush the powder on the Zn plate with a brush, and weigh the stacked plates before and after brushing the powder to calculate the powder content ratio. A solution containing metal powder is applied to single-side coating of two of the Zn plates and to double-side coating of the other Zn plate. The Zn plate coated with metal powder on both sides is placed in the middle. The other two Zn plates coated with metal powder on one side are stacked in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
[0062] The prepared stacked plates are directly subjected to a single-pass rolling process, with each rolling deformation amount of 50%. After each rolling, the plates are cut in half, and the grinding and drilling steps are repeated again, and the cumulative stacking rolling is finally performed 9 times.
[0063] Implementation Effect
[0064] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.92%, the content of Ag was 1.2%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure structure distributed along the rolling can be seen in the Zn-Se-Ag sample, and the overall metallographic structure shows a gray ZnSe phase structure. After adding Ag powder, the cumulative number of lap rolling reached 9 times, and the relevant data was measured from the 8th time. At the 8th time, they were 133.6MPa, 150.1 MPa, 21% and 89.4HV, respectively, and at the 9th time, they were 189.3MPa, 201.1 MPa, 18% and 99.1HV, respectively. With the increase of the cumulative number of lap rolling, the mechanical properties are also increasing. The electrochemical corrosion test in Hank's solution showed that the 8th corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se-Ag sample were -1.104V, 0.796 μA / cm 2 and 35.86mm / y. The 9th corrosion potential, corrosion current density and corrosion rate are -1.021V, 0.714μA / cm 2 and 31.13 mm / y. With the increase of the number of rolling laps, the sample showed a slower corrosion current density and corrosion rate, which made it have better corrosion resistance.
[0065] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se-Ag sample with the 8th cumulative rolling was 0.46mm / y. The corrosion rate of the Zn-Se-Ag sample with the 9th rolling was 0.39mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se-Ag alloy sample inactivating bone cancer cells with a cumulative rolling of 9 times reached 43%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0066] Example 5 (Sn powder)
[0067] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9%, Se powder with a purity of 99.9%, and Sn powder with a purity of 99.9%, with a powder particle size of 50µm. And weigh according to the mass ratio of each element contained in the sample, first use an electric drill to roughen the side of the Zn plate where the powder needs to be attached, and the roughness reaches Ra0.4, then drill holes in the four corners of the Zn plate and fix it with fine copper wire, then clean and dry the Zn plate with alcohol, and then put it in acetone solution for cleaning, degreasing and drying. Mix the powders according to the mass ratio and disperse them in acetone solution, and put the dispersed solution with powder into ultrasonic vibration for 30 minutes. Brush the powder on the Zn plate with a brush, and weigh the stacked plates before and after brushing the powder to calculate the powder content ratio. A solution containing metal powder is applied to single-side coating of two of the Zn plates and to double-side coating of the other Zn plate. The Zn plate coated with metal powder on both sides is placed in the middle. The other two Zn plates coated with metal powder on one side are stacked in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
[0068] The prepared stacked plates are directly subjected to a single-pass rolling process, with each rolling deformation amount of 50%. After each rolling, the plates are cut in half, and the grinding and drilling steps are repeated again, and the cumulative stacking rolling is finally performed 8 times.
[0069] Implementation Effect
[0070] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.96%, the content of Sn was 0.9%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure structure distributed along the rolling can be seen in the Zn-Se-Sn sample. After the addition of Sn powder, the cumulative number of rolling laps reached 8 times, and the relevant data were measured from the 7th time. At the 7th time, they were 93.7MPa, 124.2 MPa, 15% and 75.6HV respectively. At the 8th time, they were 123.5MPa, 136.2 MPa, 13% and 82.3HV respectively. With the increase of the cumulative number of rolling laps, the mechanical properties are also increasing. The electrochemical corrosion test in Hank's solution showed that the 7th corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se-Sn sample were -1.101V, 0.752μA / cm 2 and 35.22 mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -1.078 V, 0.699 μA / cm 2 and 32.03 mm / y. With the increase of the number of rolling laps, the sample showed a slower corrosion current density and corrosion rate, which made it have better corrosion resistance.
[0071] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se-Sn sample with the 8th cumulative rolling was 0.31mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se-Sn alloy sample inactivating bone cancer cells after 8 cumulative rolling reached 38%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0072] Comparative Example 1 (Cold Rolled Zn-Se)
[0073] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9% were used, and the weights were weighed according to the mass ratio of each element contained in the sample. The powder particle size was 50µm. The Se content was controlled at 1%. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.4, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The Se powder was dispersed in an acetone solution, and the solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The powder was brushed on the Zn plate with a brush, and the stacked plates were weighed before and after the powder was brushed to calculate the powder content ratio.
[0074] The prepared stacked plates are directly subjected to a single-pass rolling process, with each rolling deformation amount of 50%. After each rolling, the plates are cut in half, and the grinding and drilling steps are repeated again, and the cumulative stacking rolling is finally performed 9 times.
[0075] Implementation Effect
[0076] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.98%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure distributed along the rolling can be seen in the Zn-Se sample, and the overall metallographic structure shows a gray Zn-Se phase structure, but the amount of ZnSe phase contained in the whole is small, and obvious stratification can be seen between the interfaces. There are also a small amount of black Se single particles. After cumulative rolling, the Se single particles are extremely small, indicating that the rolling process effectively refines the organization and promotes mechanical alloying. The relevant data were measured from the 7th time, and the 7th time was 95.9MPa, 101.5MPa, 12.97% and 76.5HV respectively. The 8th time was 120.4MPa, 128.6MPa, 10.69% and 82.1HV, respectively, and the 9th time was 154.1MPa, 162.3MPa, 8.18% and 88.9HV, respectively. With the increase of the cumulative number of roll bonding, the mechanical properties are also increasing. The electrochemical corrosion test in Hank's solution showed that the 7th corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se sample were -0.977V, 0.896μA / cm 2 and 28.39mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -0.969V, 0.830μA / cm 2 and 27.32 mm / y. The 9th corrosion potential, corrosion current density and corrosion rate are -0.990 V, 0.781 μA / cm 2 and 25.71 mm / y. With the increase of the number of rolling laps, the sample exhibits a slower corrosion current density and corrosion rate, which makes it have better corrosion resistance.
[0077] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se sample with the 9th cumulative rolling was 0.35mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se alloy sample inactivating bone cancer cells after 9 cumulative rolling reached 69%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0078] Comparative Example 2 (no heat preservation in each pass, only heat preservation at the beginning)
[0079] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9%, with a powder particle size of 50µm. And weigh according to the mass ratio of each element contained in the sample, first use an electric drill to roughen the side of the Zn plate where the powder needs to be attached, and the roughness reaches Ra0.4, then drill holes in the four corners of the Zn plate and fix it with fine copper wire, then clean and dry the Zn plate with alcohol, and then put it in acetone solution for cleaning, degreasing and drying. Disperse Se powder in acetone solution, and put the dispersed solution with powder into ultrasonic vibration for 30 minutes. Use a brush to brush the powder on the Zn plate, and weigh the stacked plates before and after brushing the powder to calculate the powder content ratio.
[0080] The prepared stacked plates are directly subjected to a single-pass rolling process, with each rolling deformation amount of 50%. After each rolling, the plates are cut in half, and the grinding and drilling steps are repeated again, and the cumulative stacking rolling is finally performed 8 times.
[0081] Implementation Effect
[0082] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.96%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure distributed along the rolling can be seen in the Zn-Se sample, and the overall metallographic structure shows a gray ZnSe phase structure. Fine stratification can be seen between the interfaces, and there are a small amount of black Se single particles. After cumulative rolling, the Se single particles are extremely small, indicating that the rolling process effectively refines the organization and promotes mechanical alloying. The relevant data were measured from the 7th time. At the 7th time, they were 91.7MPa, 98.6MPa, 11.6% and 74.3HV respectively. At the 8th time, they were 102.3MPa, 121.8MPa, 9.4% and 85.4HV respectively. With the increase of the cumulative rolling times, the mechanical properties are also increasing. The electrochemical corrosion test in Hank's solution showed that the seventh corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se sample were -0.988 V, 0.783 μA / cm 2 and 25.77 mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -1.002 V, 0.702 μA / cm 2 and 23.11 mm / y. With the increase of the number of rolling laps, the sample showed a slower corrosion current density and corrosion rate, which made it have better corrosion resistance.
[0083] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se sample with the 8th cumulative rolling was 0.38mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of inactivating bone cancer cells by the Zn-Se alloy sample with 8 cumulative rolling reached 68%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0084] Comparative Example 3 (hot-rolled Zn-Se, different deformation amounts each time)
[0085] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9% were used, and the weights were weighed according to the mass ratio of the two elements in the sample. The powder particle size was 50µm. The Se content was controlled at 1%. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.4, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The powder was dispersed in an acetone solution, and the solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The dispersed powder was brushed on the Zn plate with a brush, and the plate was weighed before and after the powder was brushed to calculate the powder content ratio.
[0086] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 30%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 8 times.
[0087] Implementation Effect
[0088] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.96%, and the rest was Zn. In the metallographic microstructure observation, it was found that the layered microstructure distributed along the rolling can be seen in the Zn-Se sample, and the overall metallographic structure shows a gray Zn-Se phase structure, but the amount of ZnSe phase contained in the whole is small, and obvious stratification can be seen between the interfaces. There are also a small amount of black Se single particles, and the overall bonding morphology of the sample is not good, with obvious cracks and stratification. The relevant data were measured from the 7th time, and the 7th time was 78.6MPa, 82.5MPa, 8.54% and 74.1HV respectively. The 8th time was 102.5MPa, 121.6MPa, 6.54% and 89.4HV respectively. With the increase of the cumulative number of rolling, the mechanical properties are also increasing. The electrochemical corrosion test in Hank's solution showed that the seventh corrosion potential, corrosion current density and corrosion rate of the rolled Zn-Se sample were -0.987 V, 0.746 μA / cm 2 and 29.21mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -0.996V, 0.723μA / cm 2 and 25.64 mm / y. With the increase of the number of rolling laps, the sample showed a slower corrosion current density and corrosion rate, which made it have better corrosion resistance.
[0089] After immersion in Hank's solution for 30 days, the experiment showed that the corrosion rate of the Zn-Se sample with the 8th cumulative rolling was 0.32mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of the Zn-Se alloy sample inactivating bone cancer cells after 8 cumulative rolling reached 69%. It can also meet the requirements of clinical medical biomaterials and has good biomedical value.
[0090] Comparative Example 4 (Two Plates Rolled Together)
[0091] First, two Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9% were used, and the weights were weighed according to the mass ratio of the two elements in the sample. The powder particle size was 50µm. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.4, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The powder was dispersed in an acetone solution, and the solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The dispersed powder was brushed on the Zn plate with a brush, and the plate was weighed before and after the powder was brushed to calculate the powder content ratio.
[0092] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 8 times.
[0093] Implementation Effect
[0094] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.72%, and the rest was Zn. In the metallographic microstructure observation, it was found that the microstructure structure distributed along the rolling can be seen in the Zn-Se sample, but the layered structure is significantly reduced. There are a small amount of black Se single particles, and the relevant data were measured from the 7th time. At the 7th time, they were 84.5MPa, 102.6 MPa, 7.6% and 65.3HV, respectively, and at the 8th time, they were 118.6MPa, 131.4 MPa, 5.7% and 82.3HV, respectively. The electrochemical corrosion test in Hank's solution showed that the 7th corrosion potential, corrosion current density and corrosion rate of the laminated Zn-Se sample were -0.998V, 0.598μA / cm 2 and 19.80 mm / y. The 8th corrosion potential, corrosion current density and corrosion rate are -1.002 V, 0.510 μA / cm 2 and 16.9mm / y. With the increase of the number of rolling laps, the samples showed slower corrosion current density and corrosion rate.
[0095] After immersion in Hank's solution for 30 days, the corrosion rate of the Zn-Se sample with the 7th cumulative rolling was 0.36mm / y. The corrosion rate of the Zn-Se-Ag sample with the 8th cumulative rolling was 0.27mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of inactivating bone cancer cells by the Zn-Se alloy sample with 8 cumulative rolling reached 58%. Due to the limited amount of Se powder applied in the two plates, the related performance was also reduced.
[0096] Comparative Example 5 (Se powder added with a particle size of 80 µm)
[0097] First, three Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9% were used, and the weights were weighed according to the mass ratio of the two elements in the sample. The powder particle size was 80µm. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.4, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The powder was dispersed in an acetone solution, and the solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The dispersed powder was brushed on the Zn plate with a brush, and the plate was weighed before and after the powder was brushed to calculate the powder content ratio.
[0098] Before rolling, the prepared plate was placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, the plate was cut in half, and the grinding and drilling steps were repeated again, and the cumulative rolling was performed, and the final cumulative rolling number was 7 times.
[0099] Implementation Effect
[0100] The relative mass content of Se element in the powder metallurgy Zn-Se sample prepared in this embodiment was measured by X-ray fluorescence spectroscopy (XRF) to be 0.39%, and the rest was Zn. In the metallographic microstructure observation, it was found that the microstructure structure distributed along the rolling can be seen in the Zn-Se sample, but the layered structure is significantly reduced, and there are a small amount of black Se single particles. The relevant data were measured from the 7th time. At the 7th time, they were 79.2MPa, 98.5MPa, 5.2% and 61.4HV respectively. The electrochemical corrosion test in Hank's solution showed that the 7th corrosion potential, corrosion current density and corrosion rate of the laminated Zn-Se sample were -1.012V, 0.629μA / cm 2and 21.50mm / y. With the increase of the number of rolling laps, the samples showed slower corrosion current density and corrosion rate.
[0101] After immersion in Hank's solution for 30 days, the corrosion rate of the Zn-Se sample with the 7th cumulative rolling was 0.21mm / y. In the MC3T3 cytotoxicity test, when the extract was diluted to 25% and 12.5%, it showed complete biocompatibility to cells and no cytotoxicity. In the ischemic platelet plasma (PPP) of mice containing bone cancer cells, the survival rate of inactivating bone cancer cells by the Zn-Se-Ag alloy sample with 7 cumulative rollings reached 42%.
[0102] Comparative Example 6 (smoother roughness)
[0103] First, two Zn plates of the same size (1mmх25mmх50mm) with a purity of 99.9% and Se powder with a purity of 99.9% were used, and the weights were weighed according to the mass ratio of the two elements in the sample. The powder particle size was 50µm. First, the side of the Zn plate to which the powder was to be attached was roughened with an electric drill to a roughness of Ra0.1, and then holes were drilled at the four corners of the Zn plate and fixed with fine copper wire. The Zn plate was then cleaned and dried with alcohol, and then placed in an acetone solution for cleaning, degreasing and drying. The powder was dispersed in an acetone solution, and the solution with the powder after dispersion was placed in an ultrasonic oscillation for 30 minutes. The dispersed powder was brushed on the Zn plate with a brush, and the plate was weighed before and after the powder was brushed to calculate the powder content ratio.
[0104] Before rolling, the prepared plates were placed in a muffle furnace at 200°C for 25 minutes, and then taken out for single-pass rolling with a deformation of 50%. After the first rolling, it was found that the plates could not be combined together due to insufficient roughness, and cracks appeared after the first rolling.
Claims
1. A method for preparing a Zn-Se based alloy directly by mechanical processing, characterized in that: A solution containing metal powder is applied on a Zn plate, and then at least two Zn plates coated with metal powder are stacked to obtain a composite plate, the composite plate is first preheated at a temperature below 200° C., and then single-pass hot rolling is performed to obtain a hot-rolled plate, the hot-rolled plate is cut into two pieces from the middle, stacked, preheated, and then single-pass hot rolling is performed, and cutting-stacking-preheating-single-pass hot rolling is repeated 5-11 times to obtain a Zn-Se based alloy, wherein the metal in the metal powder includes Se; The process of obtaining the solution containing metal powder is to disperse the metal powder in acetone and then vibrate in ultrasound for 5-30 minutes; In the solution containing metal powder, the particle size of the metal powder is 30-50µm and the purity is ≥99.9%; The purity of the Zn plate is ≥99.9%; the roughness of the Zn plate is flat grinding Ra0.2-0.8; The composite plate is preheated at 150-200°C for 5-30 minutes; the deformation of the composite plate in a single hot rolling is 30%-50%.
2. The method for preparing a Zn-Se based alloy directly by mechanical processing according to claim 1, characterized in that: Take three Zn plates, apply a solution containing metal powder to single-side of two of them and to double-side of the other one, place the Zn plate coated with metal powder on both sides in the middle, and stack the other two Zn plates coated with metal powder on one side in such a way that the side coated with metal powder is in contact with the Zn plate coated with metal powder on both sides to obtain a composite plate.
3. The method for preparing a Zn-Se based alloy directly by mechanical processing according to claim 1, characterized in that: The hot-rolled plate is cut into two pieces from the middle, stacked, preheated, and then hot-rolled in a single pass. In the process of repeated cutting-stacking-preheating-single-pass hot rolling, the preheating temperature is 150-200°C, the preheating time is 5-30 minutes, and the deformation of each single-pass hot rolling is controlled to be equal and 30%-50%.
4. The method for preparing a Zn-Se based alloy directly by mechanical processing according to claim 1, characterized in that: The metal in the metal powder is selected from at least one of Ag, Cu, Sn, Mg, and Se and contains Se; In the Zn-Se based alloy, by mass percentage, Se: 0.1% to 10%, X: 0 to 10%, and the balance is Zn, wherein X is selected from at least one of Ag, Cu, Sn, and Mg.
5. The Zn-Se based alloy prepared by the preparation method according to any one of claims 1 to 4.
6. Application of the Zn-Se based alloy prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The Zn-Se based alloy is used for anti-tumor degradable implant material.
Citation Information
Patent Citations
Zn-Se-based alloy material and preparation method and application thereof
CN113737056A
A high plasticity degradable LiZn4-X intermetallic compound and its preparation method
AU2020102567A4
Method for manufacturing stanningmetal plate
CN101063202A
Reinforced nonferrous metal plate and preparation method thereof
CN110125180A
Preparation method of multilayer ceramic particle tough composite configuration aluminum alloy plate
CN111299320A