A fixed abrasive polishing pad based on light-induced front-end polymerization reaction and a preparation method thereof
Through the method of light-initiated front-end polymerization reaction, combined with materials such as epoxy resin and abrasives, the problems of small depth and high energy consumption of resin-based fixed abrasive polishing pads during light curing or thermal curing are solved, achieving high strength and long-lasting Long-lasting polishing pad with simple process and low cost, suitable for various shapes and shaded parts.
Patent Information
- Application Number
- CN202210675406.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-15
AI Technical Summary
Existing resin-based fixed abrasive polishing pads have problems such as small depth, inability to solidify shaded areas, high energy consumption, limited size of curing equipment, low processing efficiency, and short service life during the light curing or thermal curing process.
A fixed abrasive polishing pad based on light-initiated front-end polymerization is used. Through a combination of epoxy resin binders, abrasives, fillers, reactive diluents, initiators and additives, UV light is used to initiate the polymerization reaction and combine the rigid and elastic layers. , to achieve uniform solidification of the grinding layer and avoid dependence on external energy.
A high-strength, long-life polishing pad is realized with simple process, low energy consumption and low cost. It avoids the defects of traditional methods, such as the size limitation and small depth of curing equipment, and can perform work on shadowed parts and irregular shapes. Effective curing.
Smart Images

Figure CN114952608B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mechanical manufacturing and processing, and relates to the preparation of a grinding pad, and in particular to a consolidated abrasive grinding pad based on a light-initiated front-end polymerization reaction and a preparation method thereof. Background Art
[0002] Sapphire, ceramics, glass, silicon wafers and other hard and brittle materials have played an important role in many fields such as electronic information, military industry, aerospace, etc. due to their unique high strength, high hardness, corrosion resistance, high temperature resistance, wear resistance and other excellent properties. At present, the grinding and polishing of hard and brittle materials mostly adopts free abrasive processing technology. There are problems such as random distribution of abrasive particles, low grinding efficiency, low abrasive utilization rate, and large waste liquid pollution in the processing process. The fixed abrasive grinding pad effectively avoids the above problems by fixing the abrasive in the binder matrix.
[0003] There are two commonly used curing methods for preparing resin-based fixed abrasive grinding pads: thermal curing and photocuring. The patent with publication number CN104772693 proposes a diamond grinding pad based on thermal curing, which has a stable processing rate and good service life, but the size of the grinding pad is limited by the size of the curing equipment, and the curing process is time-consuming and energy-intensive. The patent with publication number CN106826540A prepares a photocurable resin grinding pad, which has a simple preparation method, fast curing speed, and the grinding pad has good strength, stability and life, but it still cannot avoid the problems of small depth of photocuring, inability to cure the shadow part, and limited curing of colored systems and irregular shapes. Summary of the invention
[0004] In view of the problems existing in the current resin-based fixed abrasive grinding pads based on light curing or heat curing, the present invention proposes a fixed abrasive grinding pad based on light-induced front-end polymerization reaction and a preparation method thereof. The grinding pad prepared by the present invention has the advantages of high strength, good processing stability and long service life, low energy consumption in the preparation process, simple operation, small size of curing equipment and low cost.
[0005] In order to achieve the above object, the technical solution of the present invention is achieved as follows:
[0006] A fixed abrasive grinding pad based on light-initiated front-end polymerization reaction consists of a grinding layer, an elastic layer and a rigid layer. The grinding layer comprises the following raw materials in parts by weight: 35-55% of a resin binder, 3-20% of abrasive, 5-30% of a filler, 5-20% of a reactive diluent, 0.2-5% of an initiator, and 0.2-5% of other additives.
[0007] Furthermore, the resin binder is an epoxy resin or a modified epoxy resin, including any one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin or glycidyl ester epoxy resin.
[0008] Furthermore, the abrasive is any one or more combinations of diamond, SiC, CBN, zirconia, alumina or silicon dioxide.
[0009] Furthermore, the filler is a filler with electrical conductivity or thermal conductivity, including any one or more combinations of Cu powder, aluminum powder, graphite, carbon black, carbon fiber staple fibers, carbon nanotubes, graphene, alumina powder, BN, AlN, ZnO or MgO.
[0010] Furthermore, the reactive diluent is one or more combinations of aliphatic epoxy monomers, alicyclic epoxy monomers or aromatic epoxy monomers, including any one or more combinations of 3,4-epoxycyclohexanecarboxylate, propylene oxide phenyl ether, phenyl glycidyl ether, 1,3-bis(2,3-epoxypropoxy)-2,2-dimethylpropane, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, p-tert-butylphenyl glycidyl ether or 3-ethyloxetane-3-methanol.
[0011] Furthermore, the initiator is a composition of a cationic photoinitiator and a free radical thermal initiator, wherein the photoinitiator is a diaryl iodonium salt, including any one or more of bis(4-tert-butylbenzene)iodonium hexafluorophosphate, bis[4-(tert-butyl)phenyl]iodonium tetrakis(nonafluorotert-butoxy)aluminate or [4-[(2-hydroxytetradecyl)oxy]phenyl]phenyliodonium hexafluoroantimonate; and the thermal initiator is a carbon-carbon bond initiator, including any one or more of azobisisobutyronitrile, dibenzoyl peroxide, tetraphenylethylene glycol or tetraphenylsuccinonitrile.
[0012] Furthermore, the other auxiliary agents include silane coupling agents and / or defoaming agents.
[0013] Furthermore, the silane coupling agent is KH560 silane coupling agent, KH550 silane coupling agent, KH570 silane coupling agent, A151 silane coupling agent or A171 silane coupling agent; the defoaming agent is any one of a polyether defoaming agent (brand DF-8205, DF-876 or DF-886, etc.), an organosilicon defoaming agent (EL-2708 or EL-2713, etc.) or BYK-A555.
[0014] Furthermore, the rigid layer is a rigid polymer sheet with a thickness of 0.1 to 1.0 mm, and the rigid polymer is any one of PET, PC, PMMA, PS, PI, epoxy resin or phenolic resin.
[0015] Furthermore, the elastic layer is an elastic polymer sheet with a thickness of 0.1 to 1.0 mm, and the elastic polymer is any one of polyurethane, rubber elastomer or silicone elastomer.
[0016] Furthermore, the active diluent in the grinding layer plays a role in regulating the viscosity of the system, the filler plays a role in enhancing the strength of the grinding layer and regulating the end face velocity and temperature of the front polymerization reaction, the initiator plays a role in initiating the reaction and maintaining the reaction, and other additives play a role in improving the bonding strength, eliminating tiny bubbles in the system, and promoting uniform dispersion of abrasives and fillers.
[0017] Furthermore, the preparation method of the fixed abrasive polishing pad based on the photo-initiated front-end polymerization reaction comprises the following steps:
[0018] (1) Weigh the epoxy resin binder, abrasive, filler, reactive diluent, initiator and other additives in proportion, pour them into the prepared mixing container, stir them mechanically to make them uniform, and degas them to obtain a mixture;
[0019] (2) casting the mixture obtained in step (1) into a mold, allowing it to stand and level, and pasting a rigid layer on the surface;
[0020] (3) The polymerization reaction is initiated by locally irradiating the grinding layer raw material mixture with one or more ultraviolet lights of a certain intensity vertically. After the initiation, the ultraviolet lamp is removed and the reaction can continue without light or heating.
[0021] (4) The completely cured grinding layer obtained in step (3) is demolded, and the elastic layer is adhered to the side of the rigid layer away from the grinding layer using an acrylic pressure-sensitive adhesive, and the grinding pad is prepared.
[0022] Furthermore, the wavelength of the ultraviolet light is 254-420nm, and the light intensity reaching the surface of the grinding layer is 300-700mW / cm 2 .
[0023] Preferably, the wavelength of the ultraviolet light is 365 nm as the main wavelength.
[0024] The present invention has the following beneficial effects:
[0025] 1. The polishing pad prepared by the invention has the same level of hardness and elastic modulus as the polishing pad prepared by the traditional thermal curing method and the traditional light curing method. The hardness of the polishing pad of the present application is 87 and the elastic modulus is 2.01GPa. The processing effect on the workpiece is close to that of the traditional thermal curing polishing pad and better than that of the ultraviolet light curing polishing pad. The average material removal rate of the polishing pad of the present application is 0.80μm / min, the surface roughness is 0.40μm, and the polishing pad life is 70h.
[0026] 2. The traditional thermal curing method usually needs to be carried out in an oven, and the oven needs to be kept at 80°C for 2 hours; 100°C for 4 hours; and 120°C for 2 hours. Therefore, there are problems such as long reaction time, high energy consumption, and susceptibility to size restrictions of curing equipment. The traditional photocuring method usually also needs to be carried out in a photocuring device, and due to the limitations of ultraviolet light irradiation, there are disadvantages such as small curing depth, inability to cure the shadow part, dark filler light absorption weakening the curing ability of the underlying resin, and poor curing performance in dead corners of light irradiation. The photoinitiated front-end polymerization reaction of the present invention only requires light to initiate in the initial stage. Once the reaction is initiated, the heat energy generated by the polymerization reaction is used to convert the monomer into a polymer in a small reaction zone, and the reaction zone is spontaneously pushed to the entire reactor through thermal diffusion, including the bottom layer of the molding mixture that cannot be irradiated by ultraviolet light and the dead corners of the mold. The reaction can be continued without external energy until the grinding layer is completely cured. Therefore, it has the advantages of short reaction time, low energy consumption and simple process, and avoids the defects of traditional thermal curing and light curing. Compared with traditional thermal curing, it has the advantages of short reaction time, low energy consumption, less pollution and no limitation on the size of curing equipment. Compared with traditional light curing, it has the advantages of large curing depth, curable shadow part and no limitation on system color and shape. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is a diagram of the preparation process of the fixed abrasive polishing pad according to Example 1 of the present invention.
[0029] Figure 2 This is a schematic diagram of the preparation of the grinding layer in the consolidated abrasive grinding pad based on the photo-initiated front-end polymerization mechanism in Example 1 of the present invention, wherein 1 is a casting mold; 2 is a grinding layer substrate; 3 is an abrasive; 4 is a filler; and 5 is an ultraviolet light source.
[0030] Figure 3This is a schematic diagram of the structure of the fixed abrasive polishing pad prepared in Example 1 of the present invention, wherein 1 is the polishing layer; 2 is the rigid layer; and 3 is the elastic layer. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0034] The mixing ratio of the grinding layer is as follows: 40% epoxy resin binder, 15% diamond abrasive, 30% aluminum powder filler, 13% phenyl glycidyl ether, 0.7% photoinitiator, 0.7% thermal initiator, and 0.6% defoamer, wherein the photoinitiator is bis[4-(tert-butyl)phenyl]iodonium tetrakis(nonafluoro-tert-butoxy)aluminate, the thermal initiator is tetraphenyl glycol, and the defoamer is BYK-A555.
[0035] The grinding layer is a resin-type consolidated diamond abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PC film with a thickness of 0.15mm; and the elastic layer is a polyurethane sheet with a thickness of 0.5mm.
[0036] The specific steps are as follows:
[0037] (1) Weigh epoxy resin binder, diamond abrasive, aluminum powder filler, phenyl glycidyl ether, photoinitiator, thermal initiator, and defoamer in proportion, pour into the prepared mixing container, mechanically stir evenly, and degas;
[0038] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick the PC film on the surface;
[0039] (3) Use 365nm UV lamp at 700mW / cm 2 The light intensity is locally irradiated on the grinding layer raw material until the front-end reaction is initiated, and the front-end reaction continues after the ultraviolet lamp is removed until the grinding layer is completely cured;
[0040] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PC film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0041] Example 2
[0042] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0043] The mixing ratio of the grinding layer is as follows: 45% bisphenol A epoxy resin binder, 8% SiC abrasive, 25% copper powder filler, 18% 3,4-epoxycyclohexanecarboxylate, 1% photoinitiator, 1% thermal initiator, 0.6% defoamer, and 1.4% silane coupling agent, wherein the photoinitiator is bis(4-tert-butylbenzene) iodine hexafluorophosphate, the thermal initiator is azobisisobutyronitrile, the defoamer is BYK-A555, and the silane coupling agent is KH560 silane coupling agent.
[0044] The grinding layer is a resin-type consolidated diamond abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PET film with a thickness of 0.1mm; and the elastic layer is a rubber elastic sheet with a thickness of 1.0mm.
[0045] The specific steps are as follows:
[0046] (1) Weigh bisphenol A epoxy resin binder, SiC abrasive, copper powder filler, 3,4-epoxycyclohexane carboxylate, photoinitiator, thermal initiator and defoamer according to proportion, pour into the prepared mixing container, mechanically stir evenly and defoam;
[0047] (2) Weigh the required weight of the grinding layer mixture and cast it into the prepared mold, let it stand to level, and stick a PET film on the surface;
[0048] (3) Use 365nm UV lamp at 300mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0049] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PET film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0050] Example 3
[0051] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0052] The mixing ratio of the grinding layer is as follows: 35% of polyphenol type glycidyl ether epoxy resin binder, 20% of CBN abrasive, 25% of carbon black filler, 15% of 1,4-butanediol diglycidyl ether, 0.7% of photoinitiator, 0.7% of thermal initiator, 0.6% of defoamer, and 3% of silane coupling agent, wherein the photoinitiator is [4-[(2-hydroxytetradecyl)oxy]phenyl]phenyl iodine hexafluoroantimonate, the thermal initiator is dibenzoyl peroxide, the defoamer is BYK-A555, and the silane coupling agent is KH550 silane coupling agent.
[0053] The grinding layer is a resin-type consolidated CBN abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PMMA film with a thickness of 0.2mm; and the elastic layer is a silicone elastomer sheet with a thickness of 0.5mm.
[0054] The specific steps are as follows:
[0055] (1) Weigh polyphenol type glycidyl ether epoxy resin binder, CBN abrasive, carbon black filler, 1,4-butanediol diglycidyl ether, photoinitiator, thermal initiator, defoamer and silane coupling agent in proportion, pour into the prepared mixing container, mechanically stir evenly and degas;
[0056] (2) Weigh the required weight of the grinding layer mixture and cast it into the prepared mold, let it stand to level, and stick a PMMA film on the surface;
[0057] (3) Use 365nm UV lamp at 400mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0058] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PMMA film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0059] Example 4
[0060] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0061] The mixing ratio of the grinding layer is as follows: 55% aliphatic glycidyl ether epoxy resin binder, 15% silica abrasive, 5% BN filler, 20% 1,3-bis(2,3-epoxypropoxy)-2,2-dimethylpropane, 1.5% photoinitiator, 1.5% thermal initiator, and 2% defoamer, wherein the photoinitiator is bis(4-tert-butylbenzene) iodine hexafluorophosphate, the thermal initiator is tetraphenylsuccinonitrile, and the defoamer is silicone defoamer EL-2708.
[0062] The grinding layer is a resin-type consolidated silica abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PI film with a thickness of 0.5mm; and the elastic layer is a polyurethane sheet with a thickness of 0.4mm.
[0063] The specific steps are as follows:
[0064] (1) Weigh aliphatic glycidyl ether epoxy resin binder, silica abrasive, BN filler, 1,3-bis(2,3-epoxypropoxy)-2,2-dimethylpropane, photoinitiator, thermal initiator and defoamer according to proportion, pour into the prepared mixing container, mechanically stir evenly and defoam;
[0065] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick the PI film on the surface;
[0066] (3) Use 365nm UV lamp at 500mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0067] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PI film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0068] Example 5
[0069] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0070] The proportion of the grinding layer mixture is: 45% glycidyl ester epoxy resin binder, 17% zirconium oxide abrasive, 18% MgO filler, 15% 3-ethyloxetane-3-methanol, 2% photoinitiator, 2% thermal initiator, and 1% defoamer, wherein the photoinitiator is triaryl siloxane, the thermal initiator is tetraphenyl glycol, and the defoamer is BYK-A555.
[0071] The grinding layer is a resin-type consolidated zirconium oxide abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a phenolic resin film with a thickness of 1.0mm; and the elastic layer is a silicone elastomer sheet with a thickness of 0.1mm.
[0072] The specific steps are as follows:
[0073] (1) Weigh the glycidyl ester epoxy resin binder, zirconium oxide abrasive, MgO filler, 3-ethyloxetane-3-methanol, photoinitiator, thermal initiator and defoamer in proportion, pour them into the prepared mixing container, stir them mechanically to make them uniform and defoam them;
[0074] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick a phenolic resin film on the surface;
[0075] (3) Use 365nm UV lamp at 600mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0076] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the phenolic resin film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0077] Example 6
[0078] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0079] The proportion of the grinding layer mixture is: 55% bisphenol F epoxy resin binder, 15% alumina abrasive, 19.8% MgO filler, 5% 3-ethyloxetane-3-methanol, 2.5% photoinitiator, 2.5% thermal initiator, and 0.2% defoamer, wherein the photoinitiator is bis[4-(tert-butyl)phenyl]iodonium tetrakis(nonafluoro-tert-butoxy)aluminate, the thermal initiator is tetraphenyl glycol, and the defoamer is BYK-A555.
[0080] The grinding layer is a resin-type consolidated aluminum oxide abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PS film with a thickness of 0.15mm; and the elastic layer is a polyurethane sheet with a thickness of 0.5mm.
[0081] The specific steps are as follows:
[0082] (1) Weigh bisphenol F epoxy resin binder, alumina abrasive, MgO filler, 3-ethyloxetane-3-methanol, photoinitiator, thermal initiator and defoamer according to proportion, pour into the prepared mixing container, mechanically stir evenly and defoam;
[0083] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick the PC film on the surface;
[0084] (3) Use 254nm UV lamp at 700mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0085] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PS film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0086] Example 7
[0087] This embodiment is a method for preparing a fixed abrasive polishing pad based on a photo-initiated front-end polymerization reaction, and the steps are as follows:
[0088] The proportion of the grinding layer mixture is: 55% of glycidyl ester epoxy resin binder, 3% of diamond abrasive, 20% of aluminum powder filler, 16.8% of phenyl glycidyl ether, 0.1% of photoinitiator, 0.1% of thermal initiator, and 5% of defoamer, wherein the photoinitiator is bis[4-(tert-butyl)phenyl]iodonium tetrakis(nonafluoro-tert-butoxy)aluminate, the thermal initiator is tetraphenyl glycol, and the defoamer is BYK-A555.
[0089] The grinding layer is a resin-type consolidated diamond abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PC film with a thickness of 0.15mm; and the elastic layer is a polyurethane sheet with a thickness of 0.5mm.
[0090] The specific steps are as follows:
[0091] (1) Weigh the glycidyl ester epoxy resin binder, diamond abrasive, aluminum powder filler, phenyl glycidyl ether, photoinitiator, thermal initiator and defoamer in proportion, pour them into the prepared mixing container, stir them mechanically to make them uniform and defoam them;
[0092] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick the PC film on the surface;
[0093] (3) Use 420nm UV lamp at 700mW / cm 2 The light intensity is irradiated to the grinding layer raw material until the front reaction is initiated, and the front reaction continues until the grinding layer is completely cured after the ultraviolet lamp is removed;
[0094] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PC film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0095] Comparative Example 1
[0096] This comparative example is a method for preparing a polishing pad prepared by a conventional thermal curing reaction, and the steps are as follows:
[0097] The mixing ratio of the grinding layer is as follows: 40% epoxy resin binder, 15% diamond abrasive, 30% aluminum powder filler, 13% phenyl glycidyl ether, 1.4% thermal initiator, and 0.6% defoamer, wherein the thermal initiator is tetraphenyl glycol and the defoamer is BYK-A555.
[0098] The grinding layer is a resin-type consolidated diamond abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PC film with a thickness of 0.15mm; and the elastic layer is a polyurethane sheet with a thickness of 0.5mm.
[0099] The specific steps are as follows:
[0100] (1) Weigh epoxy resin binder, diamond abrasive, aluminum powder filler, phenyl glycidyl ether, thermal initiator and defoamer in proportion, pour into the prepared mixing container, stir mechanically to make them uniform and defoam;
[0101] (2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level it, and stick the PC film on the surface;
[0102] (3) Place the mold filled with the mixture in a blast oven and cure it completely according to the curing process of "80℃ for 2h; 100℃ for 4h; 120℃ for 2h";
[0103] (4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PC film away from the grinding layer using an acrylic pressure-sensitive adhesive. The grinding pad is thus prepared.
[0104] Comparative Example 2
[0105] This comparative example is a method for preparing a polishing pad prepared by a conventional photocuring reaction, and the steps are as follows:
[0106] The mixing ratio of the grinding layer is as follows: 40% epoxy resin binder, 15% diamond abrasive, 30% aluminum powder filler, 13% phenyl glycidyl ether, 1.4% triaryl hexafluoroantimonate sulfonium salt cationic photoinitiator, 0.6% defoamer, and the defoamer is BYK-A555.
[0107] The grinding layer is a resin-type consolidated diamond abrasive grinding pad with a specification size of Ф381mm*0.8mm; the rigid layer is a PC film with a thickness of 0.15mm; and the elastic layer is a polyurethane sheet with a thickness of 0.5mm. The specific steps are as follows:
[0108] 1) Weigh the epoxy resin binder, diamond abrasive, aluminum powder filler, phenyl glycidyl ether, photoinitiator and defoamer in proportion, pour them into the prepared mixing container, stir them mechanically to make them uniform and defoam;
[0109] 2) Weigh the grinding layer mixture according to the required weight and cast it into the prepared mold, let it stand and level, and stick the PC film on the surface;
[0110] 3) Place the mold filled with the mixture into a UV oven, light cure for 5 minutes, and cool naturally to room temperature;
[0111] 4) The grinding layer is demolded, and the elastic layer is adhered to the side of the PC film away from the grinding layer using an acrylic pressure-sensitive adhesive, and the grinding pad is prepared.
[0112] The hardness, elastic modulus, and grinding effect (with high borosilicate glass as the workpiece) of the polishing pad prepared in Example 1 and the polishing pad prepared in the comparative example were tested. The test results are shown in the following table.
[0113]
[0114] The above test results show that, compared with Comparative Examples 1 and 2, the embodiments of the present invention have the same level of hardness and elastic modulus as the polishing pads prepared by the traditional heat curing method and the traditional light curing method under the condition of local light-induced front-end polymerization, and the processing effect on the workpiece is close to that of the traditional heat curing polishing pad and better than that of the ultraviolet light curing polishing pad.
[0115] After local irradiation by one or more ultraviolet lights, the front-end polymerization reaction is initiated by light. The initial stage requires light to initiate. Once initiated, the reaction can continue without external energy until the grinding layer is completely cured. Therefore, compared with the prior art, the grinding pad prepared by the present invention has the advantages of simple preparation process, low cost, short reaction time, low energy consumption, less pollution, no limitation on the size of the curing equipment, large curing depth, curable shadow part, and no limitation on the color and shape of the system.
[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A fixed abrasive polishing pad based on photo-initiated front polymerization reaction, comprising a polishing layer, an elastic layer and a rigid layer, characterized in that: The grinding layer comprises the following raw materials by weight: 35-55% resin binder, 3-20% abrasive, 5-30% filler, 5-20% reactive diluent, 0.2-5% initiator, and 0.2-5% additive; The resin binder is an epoxy resin or a modified epoxy resin, including any one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin or glycidyl ester epoxy resin; The initiator is a composition of a cationic photoinitiator and a free radical thermal initiator, wherein the photoinitiator is a diaryl iodonium salt, including any one or more of bis(4-tert-butylbenzene)iodonium hexafluorophosphate, bis[4-(tert-butyl)phenyl]iodonium tetra(nonafluorotert-butyloxy)aluminate or [4-[(2-hydroxytetradecyl)oxy]phenyl]phenyliodonium hexafluoroantimonate; the thermal initiator is a carbon-carbon bond initiator, including any one or more of azobisisobutyronitrile, dibenzoyl peroxide, tetraphenylethylene glycol or tetraphenylsuccinonitrile; the mass ratio of the cationic photoinitiator to the free radical thermal initiator is 1:1; The steps of the method for preparing the fixed abrasive grinding pad are as follows: (1) Weigh the epoxy resin binder, abrasive, filler, reactive diluent, initiator and additive according to the proportion, pour them into the prepared mixing container, stir them mechanically to make them uniform, and degas them to obtain a mixture; (2) casting the mixture obtained in step (1) into a mold, allowing it to stand and level, and pasting a rigid layer on the surface; (3) Locally irradiating the grinding layer raw material of step (2) with an ultraviolet lamp until a front-end reaction is initiated, and then removing the ultraviolet lamp, and the front-end reaction continues until the grinding layer is completely cured; the wavelength of the ultraviolet light is 254 to 420 nm, and the light intensity reaching the surface of the grinding layer formula is 300 to 700 mW / cm 2 ; (4) The completely cured grinding layer obtained in step (3) is demolded, and the elastic layer is adhered to the side of the rigid layer away from the grinding layer using an acrylic pressure-sensitive adhesive, and the grinding pad is prepared.
2. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 1, characterized in that: The abrasive is any one or more combinations of diamond, SiC, CBN, zirconium oxide, aluminum oxide or silicon dioxide.
3. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 2, characterized in that: The filler is a filler with electrical conductivity or thermal conductivity, including any one or more combinations of Cu powder, aluminum powder, graphite, carbon black, carbon fiber staple fibers, carbon nanotubes, graphene, alumina powder, BN, AlN, ZnO or MgO.
4. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 3, characterized in that: The reactive diluent is one or more combinations of aliphatic epoxy monomers, alicyclic epoxy monomers or aromatic epoxy monomers, including any one or more of 3,4-epoxycyclohexanecarboxylate, propylene oxide phenyl ether, phenyl glycidyl ether, 1,3-bis(2,3-epoxypropoxy)-2,2-dimethylpropane, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, p-tert-butylphenyl glycidyl ether or 3-ethyloxetane-3-methanol.
5. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 4, characterized in that: The auxiliary agent includes a silane coupling agent and / or a defoaming agent.
6. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 5, characterized in that: The rigid layer is a rigid polymer sheet with a thickness of 0.1 to 1.0 mm, and the rigid polymer is any one of PET, PC, PMMA, PS, PI, epoxy resin or phenolic resin.
7. The fixed abrasive polishing pad based on photo-initiated front polymerization reaction according to claim 6, characterized in that: The elastic layer is an elastic polymer sheet with a thickness of 0.1 to 1.0 mm, and the elastic polymer is any one of polyurethane, rubber elastomer or silicone elastomer.