A high-transparency corrosion-resistant beaker and its manufacturing process

Through modified polytetrafluoroethylene granulation and multi-stage sintering process, the bursting and transparency problems of traditional beakers in strong acid and alkali environments have been solved, and the preparation of highly transparent and corrosion-resistant beakers has been achieved, with a wide operating temperature range and excellent electrical insulation properties.

CN114953541BActive Publication Date: 2024-10-22JINAN SINOFLON NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210590223.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-27
Publication Date
2024-10-22
Estimated Expiration
2042-05-27

AI Technical Summary

Technical Problem

Traditional glass beakers cannot store strong acid and alkali liquids, and there is a risk of bursting and they are opaque, which affects the accuracy of chemical analysis; the existing corrosion-resistant beakers are opaque in appearance, making it impossible to observe chemical reactions.

Method used

Using 100% modified polytetrafluoroethylene granules, a highly transparent and corrosion-resistant beaker is prepared through air pressure molding and multi-stage sintering processes to ensure that the material does not undergo chemical changes at high temperatures, and a stainless steel outer mold and a rubber bladder are used in the mold. forming.

Benefits of technology

A beaker with high transparency, corrosion resistance and high temperature resistance has been achieved, which can be used normally in the range of -196℃-250℃, has good chemical stability and electrical properties, and has excellent non-stickiness and lubricity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114953541B_ABST
    Figure CN114953541B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-transparency corrosion-resistant beaker and a manufacturing process thereof. The beaker adopts 100% modified polytetrafluoroethylene granules. The specific steps are: selecting a mold, filling materials, air pressure molding, demoulding, sintering, and shaping; the appearance of the beaker manufactured by the present invention is light-colored milky white and transparent, and has the characteristics of corrosion resistance and high temperature resistance; the manufacturing process retains the chemical stability of the original material, and other materials will not precipitate during the reaction process; various parameters in the manufacturing process are strictly controlled, and the prepared beaker has high transparency, corrosion resistance, is not easy to break, has a good anti-sticking effect, and is easy to clean.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of beaker manufacturing, and in particular relates to a high-transparency corrosion-resistant beaker and a manufacturing process thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Traditional beakers are made of glass and cannot store highly corrosive liquids such as strong acids and alkalis. In ultrapure chemical analysis, it is impossible to ensure that other materials will not precipitate or react, which will affect the accuracy of the analysis. Glass beakers are at risk of bursting in a heated environment, and the material itself is fragile, posing a safety hazard.

[0004] Common anti-corrosion beakers are made of polytetrafluoroethylene, which can meet experimental requirements. However, the appearance of polytetrafluoroethylene beakers is opaque pure white, which is not conducive to observing the scale of chemical media with the naked eye, and it is impossible to intuitively see the intensity of the chemical reaction in the beaker and the color change. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a high-transparency corrosion-resistant beaker and a manufacturing process thereof. By improving the material and manufacturing method of the beaker, the chemical stability of the original material is retained. For highly corrosive liquids, no chemical changes will occur even at high temperatures, and it can be used normally in the range of -196℃-250℃.

[0006] In order to solve the above technical problems, the following technical solutions are adopted:

[0007] In a first aspect of the present invention, a high-transparency corrosion-resistant beaker is provided, the raw material of which is 100% modified polytetrafluoroethylene granules.

[0008] In some embodiments of the present invention, the modified polytetrafluoroethylene granules are prepared by granulating modified polytetrafluoroethylene powder.

[0009] In a second aspect of the present invention, a process for making a high-transparency corrosion-resistant beaker is provided, comprising the following steps:

[0010] Select a mold, and choose a mold corresponding to the finished product to be manufactured. The mold includes an outer mold and an inner mold. The outer mold is made of stainless steel, and the inner mold is made of a rubber bladder of corresponding size, and the bladder is placed inside the corresponding mold;

[0011] Filling material, injecting low-pressure air into the rubber bladder, arranging the inflated rubber bladder to the required position, and filling the gap between the outer mold and the rubber bladder with modified polytetrafluoroethylene granules;

[0012] Air pressure molding: increase the air pressure in the rubber bladder, and maintain the pressure after the pressure reaches the set value;

[0013] Demoulding, slowly deflate the skin bag and take it out, remove the outer mould, and obtain the semi-finished beaker blank;

[0014] Sintering, including low temperature sintering, medium temperature sintering, high temperature sintering, and slow cooling;

[0015] Shaping: polishing the finished parts to remove irregularities such as burrs during the production process, and marking the corresponding scale marks.

[0016] In some embodiments of the present invention, during the air pressure forming process, the pressure is determined by the specifications and dimensions of the finished beaker, and is generally controlled at 15-30 MPa.

[0017] In some embodiments of the present invention, during the air pressure forming process, the holding time is 3-10 minutes.

[0018] In some embodiments of the present invention, during the sintering process, the low-temperature sintering temperature is controlled at 250°C-270°C, the medium-temperature sintering temperature is controlled at 310°C-330°C, and the high-temperature sintering temperature is controlled at 370°C-390°C.

[0019] In some embodiments of the present invention, the low-temperature sintering temperature is 260° C., the medium-temperature sintering temperature is 320° C., and the high-temperature sintering temperature is 400° C., and constant-temperature sintering is performed at each temperature point.

[0020] In some embodiments of the present invention, the cooling rate during the slow cooling process is 50-80°C / h, the temperature is reduced to below 100°C, the sintering furnace door is opened, and the temperature is slowly cooled to room temperature.

[0021] In some embodiments of the present invention, the maximum temperature during the sintering process does not exceed 400°C.

[0022] In some embodiments of the present invention, exhaust holes are provided on the outer mold to exhaust gas in the gaps between the materials.

[0023] One or more technical solutions of the present invention have the following beneficial effects:

[0024] 1. The high-transparency corrosion-resistant beaker made by the present invention adopts modified polytetrafluoroethylene granules as the raw materials for making the beaker. The appearance of the made beaker is light milky white and transparent. Its transparency allows the changes in the beaker to be seen at a glance, and it has the characteristics of corrosion resistance and high temperature resistance.

[0025] 2. The high-transparency corrosion-resistant beaker made by the present invention retains the chemical stability of the original polytetrafluoroethylene material. For highly corrosive liquids, no chemical changes will occur even at high temperatures. Its dielectric constant and dielectric loss tangent change with temperature. It does not absorb water and its electrical properties are not affected by temperature. The beaker can be used normally within the range of -196℃-250℃. No pollution, and no other materials will be precipitated during the reaction process.

[0026] 3. The production process provided by the present invention retains the original physical and chemical properties of the modified polytetrafluoroethylene granules, strictly controls various parameters in the production process, and the prepared beaker has high transparency, corrosion resistance, high strength, high toughness, good anti-sticking effect, and is easy to clean. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present application. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0028] Figure 1 The present invention is a process flow chart for manufacturing a high-transparency corrosion-resistant beaker. DETAILED DESCRIPTION

[0029] It should be noted that the following detailed descriptions are all illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0031] Traditional beakers are made of glass, which is not corrosion-resistant and cannot store highly corrosive liquids such as strong acids and alkalis. There is also a risk of bursting when heated. Existing corrosion-resistant beakers are made of polytetrafluoroethylene, and the appearance is opaque pure white, so it is impossible to accurately see the intensity of the chemical reaction and color changes in the beaker. The inventor found that the modified polytetrafluoroethylene powder is translucent after sintering. Therefore, it is proposed to prepare the modified polytetrafluoroethylene powder into modified polytetrafluoroethylene granules, and use the modified polytetrafluoroethylene granules as the raw material for making beakers. The appearance of the produced beaker is light milky white and transparent. Its transparency can clearly see the changes in the beaker, and it has the characteristics of corrosion resistance, high temperature resistance, and no adhesion of impurities and microorganisms.

[0032] Example 1

[0033] A high-transparency corrosion-resistant beaker is made of 100% modified polytetrafluoroethylene granules, which are prepared by granulating modified polytetrafluoroethylene powder.

[0034] The modified polytetrafluoroethylene powder (CGM3101 from Zhonghao Chenguang Chemical Research Institute) is prepared into modified polytetrafluoroethylene granules by a granulator. The modified polytetrafluoroethylene granules have the following advantages: 1. Good fluidity. When the mold is filled, the material can flow freely into narrow spaces and heterogeneous spaces, omitting the steps of traditional powder materials and multiple pounding and filling, and the density of the finished product is more uniform; 2. No agglomeration occurs, avoiding the occasional hard lumps in traditional powder materials; 3. High bulk density, the density of the finished product is higher than that of powdered material products produced by the same process; 4. During the molding process, the force conduction performance between particles is significantly better than that of powdered materials, and the force is more uniform; 5. It is suitable for thin-walled products, special-shaped parts, and automated continuous production conditions.

[0035] The beaker made of modified polytetrafluoroethylene granules has a high and more uniform density and a more uniform transparency.

[0036] Example 2

[0037] A manufacturing process of a high-transparency corrosion-resistant beaker, such as Figure 1 As shown, it includes the steps of selecting molds, filling materials, air pressure forming, demoulding, sintering, shaping, etc., specifically:

[0038] Select a mold, and choose a mold corresponding to the finished product to be manufactured. The mold includes an outer mold and an inner mold. The outer mold is made of stainless steel, and the inner mold is made of a rubber bladder of corresponding size, and the bladder is placed inside the corresponding mold;

[0039] The outer mold is made of stainless steel with good corrosion resistance, and the surface of the beaker produced will be smoother. The rubber bladder used in the inner mold has a high friction coefficient and high compressive strength. The wall thickness of the beaker can be changed by controlling the pressure charged into the rubber bladder.

[0040] Filling material, pour low-pressure air into the rubber bladder, adjust the inflated rubber bladder to the required position, and fill the weighed modified polytetrafluoroethylene granules in the gap between the outer mold and the rubber bladder; it should be ensured that the filled granular material can flow freely and can be evenly distributed in various parts of the beaker, so that the density of each part of the final beaker is uniform, thereby ensuring the same transparency of each part of the beaker.

[0041] The required position and the low-pressure air filled are determined according to the specifications of the beaker to be manufactured.

[0042] Air pressure molding, increase the air pressure in the rubber bladder, and maintain the pressure after the pressure reaches the set value; when increasing the air pressure in the bladder, the pressurization process should be ensured to be slow and continuous, so that the material is evenly stressed between the bladder and the outer mold. Depending on the specifications of the finished beaker, the pressure is usually controlled at 15-30Mpa. At the same time, open the exhaust hole on the outer mold to allow the gas in the gap between the materials to be slowly and completely discharged. After slowly reaching the set pressure, close the exhaust hole of the outer mold and maintain the pressure for 3-10 minutes.

[0043] The molding process adopts air pressure molding, which retains the original chemical stability of the modified polytetrafluoroethylene granules. Compared with the traditional molding process, the force is more uniform, which again ensures the uniformity of the density and transparency of the beaker. The beakers produced by this process have less burrs than those produced by traditional processes.

[0044] After the pressure reaches the set value, the pressure is maintained to prevent the raw materials in the mold from flowing back and ensure better molding of the beaker.

[0045] Demould, slowly deflate the skin bag and take it out, remove the outer mould, and obtain the semi-finished beaker blank.

[0046] Sintering includes low-temperature sintering, medium-temperature sintering, high-temperature sintering, and slow cooling. Usually, the maximum temperature in the low-temperature stage is controlled at 250℃-270℃, and constant temperature sintering is carried out in this stage for 0.5-1 hour. In the medium-temperature stage, the maximum temperature is controlled at 310℃-330℃, and constant temperature sintering is also carried out for 1-2 hours. In the high-temperature stage, the maximum temperature is controlled at 370℃-390℃, and constant temperature sintering is carried out for 2-4 hours. In the slow cooling stage, the cooling rate is usually 50-80℃ / hour. When the temperature drops below 100℃, the sintering furnace door can be opened, and the temperature is slowly cooled to room temperature. After cooling, the finished product of the beaker is obtained.

[0047] During low-temperature sintering, medium-temperature sintering and high-temperature sintering, the temperature rise rate should be controlled within 30-60℃ / hour. The temperature rise and temperature drop rates should not be too fast, which will easily cause the beaker to expand and shrink unevenly, and the beaker will cause deformation or cracking.

[0048] The higher the temperature, the longer the constant temperature sintering time. This is because during the sintering process, the indirect contact area of ​​the particles expands, the particles aggregate, and grain boundaries are gradually formed. The pores in the particles change from connected pores to isolated pores and gradually shrink. As the pores shrink, it becomes more difficult for the pores to be discharged from the crystal. At this time, the constant temperature sintering time is increased to gradually discharge the pores until all the pores are discharged from the crystal. Constant temperature sintering for a certain period of time at low temperature, medium temperature, and high temperature stages further improves the sintering effect.

[0049] The maximum sintering temperature should not exceed 400°C to avoid the decomposition of polytetrafluoroethylene and the generation of harmful gases.

[0050] Shaping: polishing the finished parts to remove irregularities such as burrs during the production process, and marking the corresponding scale marks.

[0051] The high transparency corrosion-resistant beaker produced by the present invention has the following properties:

[0052] 1. High chemical stability

[0053] It can withstand the effects of all strong acids, strong bases, strong oxidants, and reducing agents except molten alkali metals, fluorine elements, strong fluoriding media, and sodium hydroxide above 300°C. Its chemical corrosion resistance exceeds that of precious metals, glass, ceramics, enamels, and alloys, and it is not corroded even by uranium fluoride, a strong corrosive agent in the atomic energy industry.

[0054] 2. High transparency

[0055] It has high transparency, which is higher than the general beaker made of polytetrafluoroethylene. The chemical changes of the solution in the cup can be seen at any time, which is convenient for recording the experimental process and can meet the experimental requirements.

[0056] 3. Wide operating temperature range

[0057] It can be used in a wide range of -196 to 250°C, and can maintain a certain flexibility even at an ultra-low temperature of -196°C; at 250°C, its breaking strength still remains at around 5MPa (about 1 / 5 of room temperature), and its yield strength reaches 1.4MPa.

[0058] 4. Outstanding non-stickiness

[0059] The surface tension is only 0.019N / m. Almost all solid materials cannot adhere to its surface. Only liquids with a surface tension below 0.02N / m can completely wet its surface.

[0060] 5. Abnormal lubricity

[0061] Since the mutual attraction between large molecules is small and the surface has little attraction to other molecules, the friction coefficient is very small.

[0062] 6. Excellent electrical insulation performance

[0063] It has extremely good dielectric properties and arc resistance. During high voltage discharge, it only releases some cracked non-conductive gas without carbonization causing short circuit.

[0064] 7. Excellent aging resistance and radiation resistance

[0065] There are no photosensitive groups in the molecule, so it is not only dimensionally stable at low and high temperatures, its performance remains unchanged in harsh environments, it is not attacked by microorganisms in a humid state, and it has extremely high protection against various types of radiation.

[0066] 8. Extremely low water absorption

[0067] The water absorption rate is generally around 0.001% to 0.005%, and its permeability is also low.

[0068] Although the beaker made of traditional glass has good transparency, it cannot hold strong acid and alkali solutions and is fragile; although the beaker made of polytetrafluoroethylene can hold strong acid and alkali solutions, it is not possible to visually see the reaction in the beaker due to its opaque pure white appearance; the beaker made of modified polytetrafluoroethylene granules of the present invention has a transparency that allows direct observation of the reaction in the beaker and has corrosion resistance. The modified polytetrafluoroethylene granules are prepared from modified polytetrafluoroethylene powder, have good fluidity compared to modified polytetrafluoroethylene powder, will not agglomerate during the preparation process, and the transparency of the prepared beaker is more uniform.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for producing a high-transparency corrosion-resistant beaker, characterized in that: The following steps are involved: Select a mold, and choose a mold corresponding to the finished product to be manufactured. The mold includes an outer mold and an inner mold. The outer mold is made of stainless steel, and the inner mold is made of a rubber bladder of corresponding size, and the bladder is placed inside the corresponding mold; Filling material, inject low-pressure air into the rubber bladder, adjust the inflated rubber bladder to the required position, and fill the weighed modified polytetrafluoroethylene granules in the gap between the outer mold and the rubber bladder; The modified polytetrafluoroethylene granulated material is prepared by granulating modified polytetrafluoroethylene powder; The modified polytetrafluoroethylene powder is Zhonghao Chenguang Chemical Research Institute, CGM3101; Air pressure molding: increase the air pressure in the rubber bladder, and maintain the pressure after the pressure reaches the set value; During the air pressure forming process, the pressure is determined by the specifications and dimensions of the finished beaker and is controlled at 15-30Mpa; Demoulding, slowly deflate the skin bag and take it out, remove the outer mould, and obtain the semi-finished beaker blank; Sintering, including low temperature sintering, medium temperature sintering, high temperature sintering, and slow cooling; Shaping: polishing the finished parts to remove irregular appearances such as burrs during the production process, and marking the corresponding scale marks; The outer mold is provided with exhaust holes to discharge the gas in the gap between the materials; During the sintering process, the low temperature sintering temperature is controlled at 250℃-270℃. In this stage, constant temperature sintering treatment is carried out, and the constant temperature sintering time is 0.5-1 hour; The medium temperature sintering temperature is controlled at 310℃-330℃. Constant temperature sintering treatment is carried out in this stage, and the constant temperature sintering time is 1-2 hours; High temperature sintering is controlled at 370℃-390℃. Constant temperature sintering is performed at this stage for 2-4 hours. The cooling rate during the slow cooling process is 50-80℃ / h. When the temperature drops below 100℃, open the sintering furnace door and slowly cool down to room temperature. During low temperature sintering, medium temperature sintering and high temperature sintering, the temperature rise rate is controlled at 30-60℃ / hour; The high transparency corrosion-resistant beaker has a use temperature of -196-250°C; at 250°C, the breaking strength is 5MPa and the yield strength is 1.4MPa; The surface tension of the high-transparency corrosion-resistant beaker is 0.019 N / m, and the water absorption rate is 0.001%-0.005%.