Repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent and preparation method and application thereof
Through the fluorine-free and plastic-free chitosan tannin-based water-based paper anti-oil agent, tannin-based epoxy resin and chitosan are prepared through high temperature, high pressure and alkali metal catalyst cross-linking reaction to form a highly cross-linked dense film, solving the problem The existing paper oil repellent agents are non-renewable and environmentally harmful. The paper achieves high performance oil repellent and gas barrier, improves the mechanical properties, and has good repulpability and environmental protection characteristics.
Patent Information
- Application Number
- CN202210695765.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-06-21
AI Technical Summary
Petroleum-based plastic films commonly used in existing paper anti-oil agents are non-renewable and harmful to the environment. Fluorine-containing chemicals can cause harm to the human body and the environment during use. Chitosan is expensive and has a large coating volume, making it difficult to Large-scale application.
Using fluorine-free and plastic-free chitosan, a tannin-based water-based paper oil-proof agent was prepared through the cross-linking reaction between tannin-based epoxy resin and chitosan, and was used as For paper surface coating, tannin-based polyether polyol is prepared using high temperature, high pressure and alkali metal catalysts, followed by epoxidation reaction and cross-linking reaction to form a highly cross-linked dense film to improve oil-proof performance.
It achieves high-performance oil-proof, gas barrier and improved mechanical properties of paper. It is green and sustainable, has simple process and low price. The coating has 100% repulpability and is suitable for applications in the paper packaging industry.
Smart Images

Figure CN114957739B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of paper coating preparation, relates to a paper oil-proofing agent and a preparation method thereof, and specifically relates to a completely repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent and a preparation method and application thereof. Background Art
[0002] The food packaging market is huge, among which paper products have become the largest share of packaging materials in the packaging industry due to their renewable sources, biodegradability, easy recycling, and low price, accounting for about 40% of the total sales of the food packaging industry. However, paper is a material with a three-dimensional network structure made of plant fibers as the main raw material. Its porous structure and high surface area can make grease easily penetrate the paper, resulting in a decrease in the mechanical properties of the paper, affecting the application of paper packaging. In addition, the porous structure of paper makes it lack the ability to block water vapor and oxygen, which is not conducive to the long-term storage of internal products. Therefore, improving the oil-proof and gas-barrier properties of paper is the key to the development of the paper packaging industry. At present, the food packaging industry usually uses coating (polyethylene, polypropylene, polyamide, etc.) on the surface of paper or applying low-surface-energy fluorine-containing chemicals (such as fluoroacrylates, fluoroalkyl polymers, etc.) to improve the oil-proof and gas-barrier properties of paper. However, petroleum-based plastic films are non-renewable, non-biodegradable, and not conducive to paper recycling. They are ultimately landfilled, which not only wastes a large amount of recyclable fiber resources, but also harms the environment. Fluorine-containing chemicals produce perfluorooctanoic acid (PFOA) that is harmful to the human body and the environment during preparation and use. Therefore, the development of a green, environmentally friendly, repulpable oil-proof coating has become an urgent issue for the development of the paper packaging industry.
[0003] Chitosan is a product of the deacetylation of the natural polysaccharide chitin. It has a huge reserve in nature and is widely found in the shells of shrimps and crabs. It is a renewable and biodegradable material. There are a large number of -NH2 and -OH in the structure of chitosan, which can form hydrogen bonds with the hydroxyl groups on the surface of paper. Under acidic conditions, the amino groups are protonated and positively charged, and can solidify into a film on the surface of paper through electrostatic adsorption with negatively charged paper fibers. CN 106702812 A discloses a coating type paper oil-proofing agent and a preparation method thereof, and CN 110685185 A discloses a preparation method of an environmentally friendly paper oil-proofing agent. After chitosan is applied to paper, the oil-proofing, gas barrier, antibacterial and mechanical properties of the paper can be improved. However, the high price and coating amount of chitosan make it difficult to be used on a large scale in the field of paper oil-proofing agents. Summary of the invention
[0004] In view of the above problems existing in the prior art, the first technical problem to be solved by the present invention is to provide a method for preparing a completely repulpable, fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent; the second technical problem to be solved by the present invention is to provide a paper oil-proofing agent prepared by the method; the third technical problem to be solved by the present invention is to provide the application of the completely repulpable, fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent as a paper surface coating.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent, the structural formula of which is as follows:
[0007]
[0008] In the formula, n=1, 2, 3, 4, 5.
[0009] The preparation method of the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proof agent comprises the following steps: using crude tannin extract and epoxy compound as raw materials, preparing tannin-based polyether polyol at high temperature and high pressure under the action of alkali metal catalyst and organic solvent; then carrying out epoxidation reaction of the tannin-based polyether polyol under the action of epichlorohydrin, solid alkali and phase transfer catalyst to prepare tannin-based epoxy resin; then adding the required amount of tannin-based epoxy resin into chitosan solution for cross-linking reaction to prepare chitosan tannin-based water-based paper oil-proof agent.
[0010] Furthermore, the tannin-based epoxy resin and chitosan solution are cross-linked at 40-80° C. for 1-5 hours to obtain the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent; the molar ratio of the amino group in the chitosan to the epoxy group in the tannin-based epoxy resin is 1:0.125-1.
[0011] Furthermore, the concentration of the chitosan solution is 1-3 wt. %; the solvent of the chitosan solution is an acetic acid solution with a volume percentage of 0.5-2%.
[0012] Furthermore, the tannin-based epoxy resin is obtained by using tannin-based polyether polyol, epichlorohydrin, solid alkali and phase transfer catalyst as reactants, conducting an epoxidation reaction, filtering after the reaction, washing and neutralizing, and removing water and epichlorohydrin by reduced pressure distillation; the molar ratio of the hydroxyl group of the tannin-based polyether polyol, epichlorohydrin and solid alkali is 1:6-20:0.5-1.5; the amount of the phase transfer catalyst used is 0.05% to 0.5% of the total mass of the reactants.
[0013] Furthermore, the temperature of the epoxidation reaction is 30 to 80° C., and the time of the epoxidation reaction is 2 to 6 hours.
[0014] Furthermore, the solid base is sodium hydroxide or potassium hydroxide; the phase transfer catalyst is selected from one of benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride or tetradecyltrimethylammonium chloride.
[0015] Furthermore, the tannin-based polyether polyol is prepared with crude tannin extract and epoxy compound as raw materials under high temperature and high pressure under the action of alkali metal catalyst and organic solvent; the mass ratio of the epoxy compound to the crude tannin extract is 2 to 10:1; the mass ratio of the organic solvent to the crude tannin extract is 4 to 10:1.
[0016] Furthermore, the tannin-based polyether polyol is prepared by adding crude tannin, an alkali metal catalyst, and an organic solvent into a reactor, replacing the air in the reactor with N2 for 3 times, slowly heating the reactor to 100-110°C to liquefy the crude tannin; then, introducing a required amount of an epoxy compound at 90-150°C to carry out a ring-opening addition reaction, controlling the reaction pressure not to exceed 0.8MPa, and reacting for 3-8h. After the ring-opening reaction is completed, the polyether polyol is refined.
[0017] Furthermore, the crude tannin extract is derived from black wattle, myrica pubescens or bayberry; the epoxide compound is propylene oxide or ethylene oxide; the organic solvent is selected from one of dimethyl sulfoxide, dimethylformamide, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether or 1,4-dioxane; and the catalyst is selected from one of metallic sodium, sodium methoxide, sodium hydroxide, metallic potassium, potassium methoxide or potassium hydroxide.
[0018] The repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent is used as a paper surface coating.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention uses water as a solvent and utilizes tannin-based epoxy resin and chitosan to cross-link and prepare high-performance paper coatings, realizing the high added value utilization of tree bark in the field of high-end paper coatings, and has the characteristics of green sustainability, simple process, excellent performance, and low price. Highly cross-linked tannin-based epoxy resin and chitosan form a dense film on the surface of paper, blocking the holes between fibers, blocking grease, water vapor and oxygen from penetrating into the interior of the paper; the rigid benzene ring and flexible alkyl chain in the structure of tannin-based epoxy resin effectively improve the strength and flexibility of paper, and a large number of benzene rings give the coating good ultraviolet shielding ability, effectively protecting the paper from ultraviolet aging. The biodegradable coating has 100% repulpability, and the coated paper has good recyclability. A large amount of cheap tannin-based epoxy resin added helps to reduce the cost of the coating, and the coating has good practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the infrared spectra of crude tannin extract, tannin-based polyether polyol and tannin-based epoxy resin;
[0022] Figure 2 It is the nuclear magnetic hydrogen spectrum of crude tannin extract and tannin-based polyether polyol;
[0023] Figure 3 It is the nuclear magnetic hydrogen spectrum of tannin-based polyether polyol and tannin-based epoxy resin;
[0024] Figure 4 The NMR hydrogen spectra of chitosan and chitosan tannin-based oil-proofing agent;
[0025] Figure 5 This is a test chart of the repulping performance of coated paper. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments.
[0027] The raw materials and reagents used in the following examples are: crude bayberry tannin extract, industrial grade, provided by Guangxi Wuming Tannin Extract Factory; propylene oxide, ethylene oxide, tetrabutylammonium bromide, tetrabutylammonium chloride, benzyltriethylammonium chloride, phosphoric acid, sodium hydroxide, potassium hydroxide, and DMF are provided by Yangzhou Chenhua New Materials Co., Ltd.; epichlorohydrin is industrial grade and provided by Anhui Xinyuan Technology Co., Ltd.; acetic acid, hydrochloric acid, and acetone are all analytical grade and provided by Nanjing Chemical Reagent Co., Ltd.; chitosan (deacetylation degree ≥95%) is provided by Shanghai MacLean Technology Co., Ltd.
[0028] Example 1
[0029] 40g of crude bayberry tannin extract, 13.0g of potassium hydroxide and 180g of dimethylformamide (DMF) were added to a high-pressure reactor. The air in the high-pressure reactor was replaced with nitrogen for 3 times. The agitator was turned on and the temperature was slowly raised to 110°C. Then, at a reaction temperature of 130°C, propylene oxide was continuously added dropwise to 200g. The reaction pressure was controlled to be lower than 0.8MPa. The reaction time was 5h and the temperature was kept until the reaction pressure no longer decreased. The temperature was lowered to below 60°C, the pressure was released and the material was discharged. The reaction solution was neutralized with phosphoric acid having a mass concentration of 40%, activated white clay and a refining agent magnesium silicate were added for adsorption and filtration, and the DMF solvent was recovered by vacuum distillation to obtain tannin-based polyether polyols. The appearance was a viscous red-brown liquid with a hydroxyl value of 422.3mgKOH / g and a yield of 61.2%. The crude tannin extract and tannin-based polyether polyols were characterized by infrared spectroscopy and nuclear magnetic hydrogen spectrum. Figure 1 It can be seen that the tannin-based polyether polyol has a molecular weight of 3413-3381 cm -1 The absorption peak of hydroxyl group is weakening, and the absorption peak is between 1118 and 1059 cm -1The absorption peak of COC is enhanced and is between 2970 and 2867 cm -1 The absorption peak of CH2 appeared at , but it did not appear in the crude tannin extract. Figure 2 It can be seen that the tannin-based polyether polyol has a methyl signal at 1.02ppm, while 1 The absorption peak did not appear in the H NMR spectrum. The successful preparation of tannin-based polyether polyols was confirmed by NMR and IR characterization.
[0030] The prepared tannin-based polyether polyol, epichlorohydrin and benzyltrimethylammonium chloride were added to a four-necked flask equipped with a mechanical stirrer, a reflux condenser, a thermometer and a constant pressure funnel. A 35% mass fraction of sodium hydroxide solution was added to the constant pressure funnel, n(tannin-based polyether polyol):n(ECH):n(NaOH)=1:8:1.1, and the amount of benzyltrimethylammonium chloride was 0.1% of the total mass of the reactants. The reaction was carried out at 40°C for 2 hours, and sodium hydroxide solution was dripped into the constant pressure funnel. The reaction was continued at 40°C for 2 hours. After the reaction was completed, the mixture was filtered, washed with water for neutralization, and then the epichlorohydrin and water were removed by vacuum distillation to obtain a tannin-based epoxy resin. The epoxy value was measured to be 0.27eq / 100g. The tannin-based epoxy resin was characterized by infrared and nuclear magnetic resonance. Figure 1 As shown, the tannin-based epoxy resin is at 3413-3381 cm -1 The absorption peak of hydroxyl group almost disappears at 910cm -1 The characteristic absorption peak of epoxy group appeared near Figure 3 As shown, the peaks near δ(ppm)=2.64, 2.82, and 3.19 are hydrogen on the methylene and methine groups connected to the epoxy groups. The successful preparation of tannin-based epoxy resin was proved by NMR and IR characterization.
[0031] Comprehensive analysis of infrared spectrum and nuclear magnetic data shows that the structural formula of its main components is as follows:
[0032]
[0033] The general structure of R1 is shown below:
[0034]
[0035] The general structure of R2 is shown below:
[0036]
[0037] Where n=1, 2,…, 5.
[0038] Example 2
[0039] 50g of crude bayberry tannin extract, 3.6g of potassium hydroxide and 200g of dimethylformamide (DMF) were added to an autoclave, and the air in the autoclave was replaced by nitrogen for 3 times. The agitator was turned on and the temperature was slowly raised to 110°C. Then, at a reaction temperature of 130°C, ethylene oxide was continuously added dropwise to 200g, and the reaction pressure was controlled to be lower than 0.8MPa. The reaction time was 5h, and the temperature was kept until the reaction pressure no longer decreased. The temperature was lowered to below 60°C, and the pressure was released and the material was discharged. The reaction solution was neutralized with phosphoric acid having a mass concentration of 30%, activated clay and a refining agent magnesium silicate were added for adsorption and filtration, and the DMF solvent was recovered by vacuum distillation to obtain a tannin-based polyether polyol, which was a viscous reddish-brown liquid in appearance, with a hydroxyl value of 450.5mgKOH / g and a yield of 60.5%. The prepared tannin-based polyether polyol, epichlorohydrin and benzyltrimethylammonium chloride are added to a four-necked flask equipped with a mechanical stirrer, a reflux condenser, a thermometer and a constant pressure funnel. A sodium hydroxide solution with a mass fraction of 35% is added to the constant pressure funnel, n(tannin-based polyether polyol):n(ECH):n(NaOH)=1:7:1.1, and the amount of benzyltrimethylammonium chloride is 0.1% of the total mass of the reactants. The reaction is carried out at 40°C for 2h, and sodium hydroxide solution is dripped into the constant pressure funnel. The reaction is continued at 40°C for 2h. After the reaction is completed, the mixture is filtered, washed with water for neutralization, and then the epichlorohydrin and water are removed by reduced pressure distillation to obtain a tannin-based epoxy resin. The epoxy value is measured to be 0.31eq / 100g.
[0040] Example 3
[0041] Add 0.245 ml of acetic acid to distilled water to a total volume of 49 ml to prepare a 1% (v:v) acetic acid solution. Add 1 g of chitosan and 49 ml of 0.5% (v:v) acetic acid solution into a closed flask with mechanical stirring, turn on the stirrer until the chitosan is completely dissolved, and prepare a 2wt% chitosan solution. According to the molar ratio of epoxy group to amino group of 1:8, add 0.24 g of tannin-based epoxy resin obtained in Example 2 to the above-obtained 2wt% chitosan solution, stir at room temperature for 10 minutes under closed conditions until the two are evenly mixed, then slowly raise the temperature to 60°C, and the reaction time is 3 hours to prepare a chitosan tannin-based oil-proofing agent. The properties of chitosan and chitosan tannin-based oil-proofing agents were determined. 1 H NMR. Figure 4 It can be seen that the peaks at δ(ppm)=4.16 and 2.70 are hydrogen on the methyl and methylene groups connected to the secondary amino groups, and the peak at δ(ppm)=7.9 is hydrogen on the secondary amine group, which proves that chitosan and tannin-based epoxy resin have successfully undergone cross-linking reaction.
[0042] Example 4
[0043] 0.245 ml of acetic acid was added to distilled water to a total volume of 49 ml to prepare a 1% (v:v) acetic acid solution. 1 g of chitosan and 49 ml of 0.5% (v:v) acetic acid solution were added to a closed flask with mechanical stirring, and the stirrer was turned on until the chitosan was completely dissolved to prepare a 2 wt% chitosan solution. According to the molar ratio of epoxy group to amino group being 1:4, 0.47 g of the tannin-based epoxy resin obtained in Example 2 was added to the above-obtained 2 wt% chitosan solution, and stirred at room temperature for 10 min under closed conditions until the two were evenly mixed, and then the temperature was slowly raised to 60°C and reacted for 3 h to obtain a chitosan tannin-based oil-proofing agent.
[0044] Example 5
[0045] 0.245 ml of acetic acid was added to distilled water to a total volume of 49 ml to prepare a 1% (v:v) acetic acid solution. 1 g of chitosan and 49 ml of 0.5% (v:v) acetic acid solution were added to a closed flask with mechanical stirring, and the stirrer was turned on until the chitosan was completely dissolved to prepare a 2 wt% chitosan solution. According to the molar ratio of epoxy group to amino group being 1:2, 0.95 g of the tannin-based epoxy resin obtained in Example 2 was added to the above-obtained 2 wt% chitosan solution, and stirred at room temperature for 10 min under closed conditions until the two were evenly mixed, and then the temperature was slowly raised to 60°C and reacted for 3 h to obtain a chitosan tannin-based oil-proofing agent.
[0046] Example 6
[0047] 0.245 ml of acetic acid was added to distilled water to a total volume of 49 ml to prepare a 1% (v:v) acetic acid solution. 1 g of chitosan and 49 ml of 0.5% (v:v) acetic acid solution were added to a closed flask with mechanical stirring, and the stirrer was turned on until the chitosan was completely dissolved to prepare a 2 wt% chitosan solution. According to the molar ratio of epoxy group to amino group being 1:1, 1.90 g of the tannin-based epoxy resin obtained in Example 2 was added to the above-obtained 2 wt% chitosan solution, and stirred at room temperature for 10 min under closed conditions until the two were evenly mixed, and then the temperature was slowly raised to 60°C and reacted for 3 h to obtain a chitosan tannin-based oil-proofing agent.
[0048] Comparative Example 1
[0049] Without adding epoxy tannin resin, a 2wt% chitosan solution was used as a control sample to explore the effect of adding epoxy tannin resin on the performance of the paper sample. 0.245ml of acetic acid was added to distilled water to a total volume of 49ml to prepare a 1% (v:v) acetic acid solution. 1g of chitosan and 49ml of 0.5% (v:v) acetic acid solution were added to a closed flask with mechanical stirring, and the stirrer was turned on until the chitosan was completely dissolved to prepare a 2wt% chitosan solution. The coating components of Examples 3 to 6 and Comparative Example 1 are shown in Table 1:
[0050] Table 1 Coating ingredients of Examples 3 to 6 and Comparative Example 1
[0051] Example Epoxy tannin resin(g) Chitosan(g) Molar ratio of epoxy groups to amino groups Comparative Example 1 0 1 - Example 3 0.24 1 0.125 Example 4 0.47 1 0.25 Example 5 0.95 1 0.5 Example 6 1.90 1 1
[0052] Example 7
[0053] The chitosan-based oil-proofing agents obtained in Examples 3 to 6 and the 2 wt% chitosan solution obtained in Comparative Example 1 were applied to the surface of paper to test the physical properties of the paper. 2 The surface of the corrugated paper, one end of the corrugated paper is fixed on the coating machine, take an appropriate amount of coating and evenly apply it to one end of the corrugated paper, start the coating machine, when the coating rod moves forward slowly, the coating is evenly applied on the surface of the corrugated paper, control the coating amount of each group to be almost the same (3 ~ 4g / m 2 ), dry the coated paper at room temperature for 24 hours, and then place it under constant temperature and humidity conditions of 25°C and 50% RH for 24 hours to prepare for the test of physical properties. Refer to the determination of fat resistance of paper and paperboard GB / T 22805.2-2008 to test the oil resistance of paper; refer to the test method for air permeability of plastic film and sheet GB / T 1037-1988 to test the water vapor transmission rate (WVTR) of paper; refer to the oxygen permeability test of plastic film and sheet GB / T 19789-2005 to test the oxygen transmission rate (OP) of paper samples; refer to the determination of tensile strength of paper and paperboard GB / T 453-2002 to test the tensile strength, breaking length and elongation of paper; refer to the determination method of paper bursting resistance GB / T 454-2020 to test the bursting resistance of paper; refer to the test method for artificial weathering of plastics, coatings and rubber materials for mechanical industrial products GB / T 14522-2008, UVA-340 fluorescent UV lamp was used to UV age the paper samples at 25°C and 50% RH for 24 hours, and the mechanical properties of the aged samples were tested and compared with those of the unaged samples to characterize the UV shielding ability of the coating. The physical properties data of the chitosan-based oil-proofing agent coated paper are shown in Table 2:
[0054] Table 2 Performance indexes of paper coated with chitosan tannin-based oil-proofing agent
[0055]
[0056] As can be seen from Table 2, compared with base paper, the oil-proof performance and gas barrier performance of the chitosan tannin-based oil-proof agent coated on the surface of the paper are significantly enhanced, the Kit value increases from 0 / 12 to 12 / 12, the water vapor transmission rate decreases by 76.1%, and the oxygen transmission rate decreases by 63.0%. This is because the highly cross-linked chitosan and tannin-based epoxy resin form a dense film on the surface of the paper, blocking the pores between the fibers, and effectively preventing grease, water vapor and oxygen from penetrating into the interior of the paper. In addition, the rigid benzene ring and flexible alkyl chain in the tannin-based epoxy resin structure effectively improve the mechanical properties of the paper. Compared with base paper, the tensile strength, breaking length, bursting strength and elongation at break of Example 6 increased by 23.1%, 23.1%, 56.8% and 66.7%, respectively. The benzene ring in the tannin-based epoxy resin structure can absorb ultraviolet rays, and the coating has good ultraviolet shielding ability. Compared with the base paper, the mechanical properties of the paper coated with chitosan tannin-based oil-proof agent lose little after ultraviolet aging.
[0057] Example 8
[0058] The chitosan-based oil-proofing agent obtained in Example 6 was used to coat the corrugated base paper to obtain the coated paper for the repulping performance test of the paper. The coated paper was cut into small pieces, soaked in hot water at 50-80°C for 1 hour, and the paper was dissociated into single fibers using a fiber disintegrator. The slurry was washed with distilled water several times, and then paper was made using a sheet making machine. The steps are as follows: Figure 5 The surface of recycled paper is uniform and free of impurities, and the coating is 100% repulpable.
Claims
1. A method for preparing a re-pulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent, It is characterized in that The tannin-based epoxy resin and chitosan solution are cross-linked at 40-80°C for 1-5h to obtain the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent; the molar ratio of the amino group in the chitosan to the epoxy group in the tannin-based epoxy resin is 1:0.125-1; the tannin-based epoxy resin is obtained by using tannin-based polyether polyol, epichlorohydrin, solid alkali and phase transfer catalyst as reactants to carry out epoxidation reaction, filtering after the reaction, washing and neutralizing, and removing water and epichlorohydrin by reduced pressure distillation.
2. The method for preparing the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 1, It is characterized in that The concentration of the chitosan solution is 1-3 wt. %; the solvent of the chitosan solution is an acetic acid solution with a volume percentage of 0.5-2%.
3. The preparation method of the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 1, It is characterized in that The molar ratio of the hydroxyl group of the tannin-based polyether polyol, epichlorohydrin and solid alkali is 1:6-20:0.5-1.5; the amount of the phase transfer catalyst is 0.05%-0.5% of the total mass of the reactants.
4. The method for preparing the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 1, It is characterized in that The temperature of the epoxidation reaction is 30-80° C., and the time of the epoxidation reaction is 2-6 hours.
5. The preparation method of the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 1, It is characterized in that The solid alkali is sodium hydroxide or potassium hydroxide; the phase transfer catalyst is selected from one of benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride or tetradecyltrimethylammonium chloride.
6. The method for preparing the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 1, It is characterized in that The tannin-based polyether polyol is prepared from crude tannin extract and epoxy compound as raw materials under high temperature and high pressure under the action of alkali metal catalyst and organic solvent; the mass ratio of the epoxy compound to the crude tannin extract is 2-10:1; the mass ratio of the organic solvent to the crude tannin extract is 4-10:
1.
7. The method for preparing the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 6, It is characterized in that The tannin-based polyether polyol is prepared by adding tannin crude product, alkali metal catalyst and organic solvent into a reaction kettle. 2 The air in the reactor was replaced for 3 times, and the temperature was slowly raised to 100-110°C to liquefy the crude tannin extract; then, the required amount of epoxy compound was introduced at 90-150°C for ring-opening addition reaction, and the reaction pressure was controlled not to exceed 0.8MPa. The reaction time was 3-8h. After the ring-opening reaction, it was refined to obtain the product.
8. The method for preparing the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 7, It is characterized in that The crude tannin extract is derived from black wattle, myrica pubescens or myrica rubra; the epoxide compound is propylene oxide or ethylene oxide; the organic solvent is selected from one of dimethyl sulfoxide, dimethylformamide, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether or 1,4-dioxane; the alkali metal catalyst is selected from one of metallic sodium, sodium methoxide, sodium hydroxide, metallic potassium, potassium methoxide or potassium hydroxide.
9. The repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent obtained by the preparation method of the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to any one of claims 1 to 8.
10. Use of the repulpable fluorine-free and plastic-free chitosan tannin-based water-based paper oil-proofing agent according to claim 9 as a paper surface coating.