A preparation method of mesh nano silver and mesh nano silver

By introducing ultra-fine silver powder into the composite alcohol solution system, the fusion and cross-linked growth of linear nano-silver and ultra-fine silver powder are achieved, and network-shaped nano silver with better conductivity is prepared, which solves the problem of conductivity and stability in the existing technology. Insufficient problem, achieving high conductivity applications in flexible and stretchable electronic products.

CN114974646BActive Publication Date: 2024-10-29BEIJING INFORMATION SCI & TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210707981.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-21
Publication Date
2024-10-29
Estimated Expiration
2042-06-21

AI Technical Summary

Technical Problem

It is difficult to provide a nano-silver material with good conductivity and stable conductivity in the existing technology, especially in the field of flexible and stretchable electronic products, there is a lack of suitable materials.

Method used

By introducing ultra-fine silver powder into the composite alcohol solution system, the fusion and cross-linked growth of linear silver nanoparticles and ultra-fine silver powder particles are achieved, and network-shaped silver nanoparticles with better conductivity are prepared.

Benefits of technology

The prepared network silver nanoparticles have better conductivity and stability, with a sheet resistance of 0.16Ω·sq-1, can maintain high conductivity under tensile deformation, and are suitable for flexible and stretchable electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114974646B_ABST
    Figure CN114974646B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a mesh nano silver, comprising the following steps: 1) placing spherical silver powder in a solvent for treatment to obtain treated silver powder for standby use; 2) mixing propylene glycol and ethylene glycol evenly to obtain a mixed solution for standby use; 3) adding PVP to the mixed solution in step 2), stirring until dissolved, and then adding potassium bromide, silver chloride and treated silver powder to obtain a reaction solution; 4) adding silver nitrate to the mixed solution in step 2), stirring until dissolved to obtain a silver nitrate solution; 5) heating the reaction solution to 160° C. under stirring, and then dripping the silver nitrate solution into the reaction solution, continuing the reaction for a period of time, and obtaining a mesh nano silver wire solution. The invention introduces ultrafine silver powder into the composite alcohol solution system to achieve the fusion and cross-linking growth of linear nano silver and ultrafine silver powder particles, and prepares mesh nano silver, which has better conductivity than linear nano silver.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic information materials and components, and more particularly to a preparation method of mesh nano silver and the mesh nano silver. Background Art

[0002] The morphology of nanosilver particles is generally irregular. With the continuous development of physical and chemical methods for preparing nanomaterials, there are many methods for preparing nanosilver structures with different morphologies. Nanosilver particles mainly have sheets, rods, wires, strips, beams, tubes, bicones, cubes and polyhedron structures. The morphology of nanosilver particles has a key influence on their properties. Nanosilver particles with different structures have different properties and different applications. There are no related reports on mesh nanosilver structures. Mesh nanosilver has the high electrical conductivity and excellent thermal conductivity of silver, as well as the high specific surface area and excellent stretchability of one-dimensional metal nanomaterials. It is a key material for flexible and stretchable electronic technology. Mesh nanosilver effectively avoids the contact resistance formed by the cross-stacked nanosilver wires, and has better conductivity, especially under strong tensile deformation. It can maintain high conductivity and has great application potential in the field of flexible and stretchable electronic products.

[0003] Therefore, how to provide a method for preparing a nanosilver material with good conductivity and stable conductive performance is a technical problem that technicians in this field need to solve urgently.

[0004] The present invention introduces ultrafine silver powder into the composite alcohol solution system to achieve the fusion and cross-linking growth of linear nanosilver and ultrafine silver powder particles to prepare mesh nanosilver, which has better conductivity than linear nanosilver. Summary of the invention

[0005] In view of this, the present invention provides a method for preparing mesh nanosilver and mesh nanosilver, by introducing ultrafine silver powder into a composite alcohol solution system to achieve fusion and cross-linking growth of linear nanosilver and ultrafine silver powder particles, to prepare mesh nanosilver, which has better conductivity than linear nanosilver.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing mesh nanosilver comprises the following steps:

[0008] 1) placing the spherical silver powder in a solvent for treatment to obtain treated silver powder for later use;

[0009] 2) mixing propylene glycol and ethylene glycol uniformly to obtain a mixed solution for standby use;

[0010] 3) adding PVP to the mixed solution of step 2), stirring with a magnetic stirrer until dissolved, and then adding potassium bromide, silver chloride and treated silver powder to obtain a reaction solution;

[0011] 4) adding silver nitrate to the mixed solution of step 2), and stirring with a magnetic stirrer until the silver nitrate is dissolved to obtain a silver nitrate solution;

[0012] 5) The reaction solution is heated to 160° C. under stirring, and then a silver nitrate solution is added dropwise to the reaction solution. The reaction is continued for a period of time to obtain a network nanosilver solution, and the network nanosilver is obtained after drying.

[0013] Preferably, the solvent in step 1) is an acetone solution.

[0014] Preferably, the volume ratio of propylene glycol to ethylene glycol in step 2) is 2:1.

[0015] Preferably, in step 3), the mass volume ratio of the PVP to the mixed solution is 3.35 g: 200 ml; and the viscosity average molecular weight of the PVP is 40,000.

[0016] Preferably, in step 3), the mass ratio of potassium bromide, silver chloride and treated silver powder is 0.075:0.255:2.

[0017] Preferably, the mass volume ratio of silver nitrate to the mixed solution in step 4) is 3.4 g:100 ml.

[0018] Preferably, the step of adding the silver nitrate solution dropwise is to add the silver nitrate solution dropwise at a speed of 50 rpm through a constant flow pump.

[0019] Preferably, the reaction time is 12-36 hours.

[0020] A mesh nano silver is prepared by the mesh nano silver preparation method.

[0021] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0022] The mesh nanosilver prepared by the present invention is a new morphology of nanosilver with a square resistance of 0.16Ω·sq -1 The flexible stretchable conductive film prepared using it as a conductive filler has stable conductivity under tensile deformation. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0024] Figure 1This is a scanning electron microscope (SEM) image of the mesh nanosilver prepared in the present invention. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] A method for preparing mesh nanosilver comprises the following steps:

[0028] 1) placing the spherical silver powder in an acetone solution to obtain treated silver powder for later use;

[0029] 2) Propylene glycol and ethylene glycol are mixed uniformly in a volume ratio of 2:1 to obtain a mixed solution for later use;

[0030] 3) 3.35g PVP mv=40000 Add to 200 ml of the mixed solution in step 2), stir magnetically until dissolved, then add 0.075 g of potassium bromide, 0.255 g of silver chloride and 2 g of treated silver powder to obtain a reaction solution;

[0031] 4) adding 3.4 g of silver nitrate to 100 ml of the mixed solution in step 2), and stirring with a magnetic stirrer until the mixture is dissolved to obtain a silver nitrate solution;

[0032] 5) The reaction solution was heated to 160° C. under stirring, and then a silver nitrate solution was added dropwise to the reaction solution at a speed of 50 rpm using a constant flow pump for 24 hours to obtain a mesh nanosilver solution, which was then dried to obtain a mesh nanosilver.

[0033] Example 2

[0034] The microscopic morphology of the mesh nanosilver prepared in Example 1 was observed by scanning electron microscopy (SEM: EVO-18, ZEISS, Germany). Figure 1 ,Depend on Figure 1 It can be seen that the nanosilver particles are intertwined and fused to grow into a network.

[0035] Example 3

[0036] The resistance of the mesh nanosilver prepared in Example 1 was tested by a four-probe resistance meter and the result was 0.16Ω·sq -1 That is, the mesh nanosilver provided by the present invention has better conductivity.

[0037] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0038] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing mesh nanosilver, characterized in that: The following steps are involved: 1) placing the spherical silver powder in a solvent to obtain treated silver powder, and drying it for later use; 2) mixing propylene glycol and ethylene glycol uniformly to obtain a mixed solution for standby use; 3) adding PVP to the mixed solution of step 2), stirring until dissolved, and then adding potassium bromide, silver chloride and treated silver powder to obtain a reaction solution; 4) adding silver nitrate to the mixed solution in step 2) and stirring until dissolved to obtain a silver nitrate solution; 5) heating the reaction solution to 160° C. under stirring, then dropping a silver nitrate solution into the reaction solution, and continuing the reaction for 12 to 36 hours to obtain a network nanosilver solution, and then drying to obtain a network nanosilver; In step 3), the mass volume ratio of the PVP to the mixed solution is 3.35 g: 200 ml; the viscosity average molecular weight of the PVP is 40,000; the mass ratio of the potassium bromide, silver chloride and treated silver powder is 0.075: 0.255: 2; The mass volume ratio of silver nitrate to the mixed solution in step 4) is 3.4 g:100 ml; The step of adding the silver nitrate solution dropwise is to add the silver nitrate solution dropwise at a speed of 50 rpm through a constant flow pump.

2. The method for preparing a mesh-shaped nanosilver according to claim 1, characterized in that: The solvent in step 1) is an acetone solution.

3. The method for preparing a mesh-shaped nanosilver according to claim 1, characterized in that: The volume ratio of propylene glycol to ethylene glycol in step 2) is 2:

1.

4. A mesh-shaped nanosilver, characterized in that: The nanosilver mesh is prepared by the preparation method of any one of claims 1 to 3.