Silicon solar cell front conductive silver paste and preparation method thereof, silicon solar cell front electrode
By using a formula of combining glass powder and organic carrier in the conductive silver paste on the front of silicon solar cells, the problem of the existing silver paste showing differences under different process conditions is solved, and the balance between high welding tension and photoelectric conversion efficiency is achieved. In various silicon solar cell types, the overall performance of the battery is improved.
Patent Information
- Application Number
- CN202110197425.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-02-22
AI Technical Summary
The front conductive silver paste of existing silicon solar cells cannot meet different process needs at the same time, resulting in great differences under different process conditions, affecting the photoelectric conversion efficiency and welding tension of the battery.
Using a silicon solar cell front conductive silver paste, the formula includes 70.0%-94.0% silver powder, 0.1%-8.0% combined glass powder and 5.0%-30.0% organic carrier, the combined glass powder is composed of front reaction glass powder, Concentrated glass powder and rear-reactive glass powder, the front-reactive glass powder is composed of Te-O-Te structure, and the back-reactive glass powder is composed of Te-O-Si structure. The tackified glass powder provides a sintering effect during the sintering process and improves silver The density of the layer and the welding tension.
The silver paste can maintain high welding tension and excellent photoelectric conversion efficiency under different process conditions, adapt to various silicon solar cell types, and improve the output power and stability of silicon solar cells.
Smart Images

Figure BDA0002947560620000091 
Figure BDA0002947560620000092 
Figure BDA0002947560620000101
Abstract
Description
Technical Field
[0001] The present application belongs to the field of silicon solar cells, and in particular relates to a silicon solar cell front conductive silver paste and a preparation method thereof, and a silicon solar cell front electrode. Background Art
[0002] Silicon solar cells are semiconductor devices that use the photoelectric effect to convert solar energy into electrical energy. They are mainly composed of a front conductive electrode, an anti-reflection layer, a PN junction structure, a support surface, a silicon substrate, and a back electrode. Silicon solar cells are currently a relatively mature application technology for converting solar energy into electrical energy, and have also become a hot topic for research in various countries. The main focus of research on silicon solar cells is to improve the photoelectric conversion efficiency of cells. Against this background, silicon solar cells with various manufacturing processes, design structures, and doping concentrations have emerged, including conventional polycrystalline, polycrystalline black silicon, polycrystalline diamond wire, conventional single crystal cells, perc single crystal, Se-perc single crystal, etc. The front conductive silver paste of silicon solar cells is an important material for the front conductive electrode, which has an important influence on the output power of silicon solar cells. After the front conductive silver paste of silicon solar cells is printed on the front of the silicon solar cell by screen printing, it is sintered to form an electrode with good contact. Different processes also have great differences in the requirements for the properties of silver paste. Therefore, it is of great significance to develop a front conductive silver paste for crystalline silicon solar cells with structures that can adapt to various processes. Summary of the invention
[0003] The purpose of the present application is to provide a silicon solar cell front conductive silver paste and a preparation method thereof, as well as a silicon solar cell front electrode, in order to solve the problem that the existing solar cell front conductive silver paste cannot simultaneously meet different process requirements.
[0004] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0005] In a first aspect, the present application provides a silicon solar cell front conductive silver paste, which comprises the following raw material components in the following weight percentages, based on the total weight of the silicon solar cell front conductive silver paste being 100%:
[0006] Silver powder 70.0%-94.0%;
[0007] Combined glass powder 0.1%-8.0%;
[0008] Organic carrier 5.0%-30.0%;
[0009] The combined glass powder includes at least two of a front-reaction glass powder, a viscosity-enhancing glass powder and a rear-reaction glass powder; wherein both the front-reaction glass powder and the rear-reaction glass powder contain a Te-O-Te structure and a Te-O-Si structure, and the content of the Te-O-Te structure in the front-reaction glass powder is higher than that of the Te-O-Si structure, and the content of the Te-O-Te structure in the rear-reaction glass powder is lower than that of the Te-O-Si structure.
[0010] The second aspect of the present application provides a method for preparing a conductive silver paste on the front side of a silicon solar cell, comprising the following steps:
[0011] According to the formula of the conductive silver paste on the front side of the silicon solar cell provided in the first aspect, silver powder, front reaction glass powder, viscosity-enhancing glass powder, rear reaction glass powder and an organic carrier are provided;
[0012] The pre-reaction glass powder, the viscosity-enhancing glass powder and the post-reaction glass powder are mixed to obtain a combined glass powder;
[0013] The combined glass powder is mixed with the silver powder and the organic carrier and subjected to grinding treatment to prepare a conductive silver paste on the front side of a silicon solar cell.
[0014] The third aspect of the present application provides a method for preparing a front electrode of a silicon solar cell, comprising the following steps:
[0015] Providing a silicon semiconductor element, wherein an insulating film is disposed on one surface of the silicon semiconductor element;
[0016] Applying the conductive silver paste on the front side of the silicon solar cell provided in the first aspect or the conductive silver paste on the front side of the silicon solar cell obtained by the method provided in the second aspect to the silicon solar cell, drying the paste, and heating the paste to 700° C. to 950° C. for sintering;
[0017] The silicon solar cell front electrode is obtained by cooling.
[0018] The conductive silver paste for the front side of the silicon solar cell provided by the present application comprises a glass powder which is a combined glass powder, including a front reaction glass powder, a viscosity-enhancing glass powder and a rear reaction glass powder. The three glass powders have different glass structures and different properties. Two or more glass powders interact with each other, thereby improving the adaptability of the conductive silver paste for the front side of the silicon solar cell.
[0019] Specifically, on the one hand, the pre-reaction glass powder has a Te-O-Te structure as the main glass structure, the glass powder has a low melting point, and reacts strongly with the silver powder during the silver paste sintering process, and has a strong ability to enhance the oxidation and melting of silver, so that the conductive silver paste can carry more silver, thereby increasing the silver content of the silicon solar cell using the conductive silver paste. The post-reaction glass has a Te-O-Si structure as the glass structure, the glass powder has a moderate melting point, and the Te-O-Si structure has a larger polarity than the Te-O-Te structure or the Si-O-Si structure. Therefore, the Ag ions melted in the Te-O-Si structure are very easy to precipitate due to the difference in the force when the temperature is reduced, which is conducive to the precipitation of silver on the surface of the silicon solar cell. The combination of pre-reaction glass powder and post-reaction glass powder can enhance the melting ability of silver and promote the precipitation of melted silver and improve its stability through Te-O-Te structure and Te-O-Si structure respectively, which not only increases the silver content of the glass loading interface during the sintering process of silver paste, but also increases the number of silver nanoparticles precipitated during the sintering cooling process, reduces the contact resistance, and improves the photoelectric conversion efficiency. The viscosity-enhancing glass powder is extremely viscous and flows slowly in the pre-sintering stage, but has a strong sintering effect in the middle and late stages of sintering, which can reduce the influence of mixed melting of different glass powders, improve the sintering effect of silver paste and obtain a dense silver layer, and avoid the influence of multiple glass powder combinations on the interface between silver grid lines and silicon solar cells. On the other hand, three different glass powders can enhance the sintering effect of silver powder, which is conducive to the precipitation of silver powder on the surface and the formation of low-melting-point high-strength alloys with reduced low-melting-point metals, thereby improving the sintering density and fracture strength between silver powders, and improving the welding tensile force of the conductive silver paste on the front of silicon solar cells. In addition, the difference in melting points of the three glass powders causes the glass powders to melt at different stages of silver paste sintering, which is beneficial to the function and sintering stratification of each glass powder, and improves the ability to avoid deviations or changes caused by simultaneous melting and sintering of multiple glass powders.
[0020] In summary, the conductive silver paste for the front side of the silicon solar cell provided in the present application can well balance the relationship between the welding tension and the photoelectric conversion efficiency, ensuring that the conductive silver paste has high tension while having excellent photoelectric conversion efficiency, thereby giving it a wide range of adaptability and being able to adapt to various silicon solar cells prepared by different processes and of different types.
[0021] The method for preparing the conductive silver paste for the front side of a silicon solar cell provided in the present application is to mix the glass powders, and then mix them with the silver powder and the organic carrier and grind them to obtain the conductive silver paste. The method is simple to operate and has good product stability and reliability.
[0022] The present application provides a method for preparing the front electrode of a silicon solar cell, which comprises printing the conductive silver paste on the front of the silicon solar cell provided above on an insulating film on the surface of one side of a silicon semiconductor element. The method is simple to operate, easy to control, and is beneficial to improving the stability and reliability of the electrode product. DETAILED DESCRIPTION
[0023] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0024] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0025] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0026] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0027] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0028] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0029] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0030] In order for the silver paste on the front of the silicon solar cell to form a good contact effect during the sintering process, it is necessary to form an excellent conductive channel between the glass and the silver powder, and between the glass and the battery contact surface, which requires the glass to have certain sintering properties and corrosiveness. However, due to the differences in battery manufacturing processes and doping concentrations, the requirements for glass are getting higher and higher. It is of great research value to develop a glass system or glass matching system with strong adaptability to adapt to silicon solar cells with different design structures and doping concentrations. In view of this,
[0031] In a first aspect, an embodiment of the present application provides a conductive silver paste for the front side of a silicon solar cell, which comprises the following raw material components in the following weight percentages, based on the total weight of the conductive silver paste for the front side of the silicon solar cell being 100%:
[0032] Silver powder 70.0%-94.0%;
[0033] Combined glass powder 0.1%-8.0%;
[0034] Organic carrier 5.0%-30.0%;
[0035] The combined glass powder includes at least two of the following: pre-reaction glass powder, viscosity-enhancing glass powder and post-reaction glass powder; wherein both the pre-reaction glass powder and the post-reaction glass powder contain Te-O-Te structure and Te-O-Si structure, and the content of Te-O-Te structure in the pre-reaction glass powder is higher than that of Te-O-Si structure, and the content of Te-O-Te structure in the post-reaction glass powder is lower than that of Te-O-Si structure.
[0036] The conductive silver paste for the front side of the silicon solar cell provided in the embodiment of the present application is a combined glass powder, including a front reaction glass powder, a viscosity-enhancing glass powder and a rear reaction glass powder. The three glass powders have different glass structures and different properties. Two or more glass powders interact with each other, thereby improving the adaptability of the conductive silver paste for the front side of the silicon solar cell.
[0037] Specifically, on the one hand, the pre-reaction glass powder has a Te-O-Te structure as the main glass structure, the glass powder has a low melting point, and reacts strongly with the silver powder during the silver paste sintering process, and has a strong ability to enhance the oxidation and melting of silver, so that the conductive silver paste can carry more silver, thereby increasing the silver content of the silicon solar cell using the conductive silver paste. The post-reaction glass has a Te-O-Si structure as the glass structure, the glass powder has a moderate melting point, and the Te-O-Si structure has a larger polarity than the Te-O-Te structure or the Si-O-Si structure. Therefore, the Ag ions melted in the Te-O-Si structure are very easy to precipitate due to the difference in the force when the temperature is reduced, which is conducive to the precipitation of silver on the surface of the silicon solar cell. The combination of pre-reaction glass powder and post-reaction glass powder can enhance the melting ability of silver and promote the precipitation of melted silver and improve its stability through Te-O-Te structure and Te-O-Si structure respectively, which not only increases the silver content of the glass loading interface during the sintering process of silver paste, but also increases the number of silver nanoparticles precipitated during the sintering cooling process, reduces the contact resistance, and improves the photoelectric conversion efficiency. The viscosity-enhancing glass powder is extremely viscous and flows slowly in the pre-sintering stage, but has a strong sintering effect in the middle and late stages of sintering, which can reduce the influence of mixed melting of different glass powders, improve the sintering effect of silver paste and obtain a dense silver layer, and avoid the influence of multiple glass powder combinations on the interface between silver grid lines and silicon solar cells. On the other hand, three different glass powders can enhance the sintering effect of silver powder, which is conducive to the precipitation of silver powder on the surface and the formation of low-melting-point high-strength alloys with reduced low-melting-point metals, thereby improving the sintering density and fracture strength between silver powders, and improving the welding tensile force of the conductive silver paste on the front of silicon solar cells. In addition, the difference in melting points of the three glass powders causes the glass powders to melt at different stages of silver paste sintering, which is beneficial to the function and sintering stratification of each glass powder, and improves the ability to avoid deviations or changes caused by simultaneous melting and sintering of multiple glass powders.
[0038] In summary, the conductive silver paste on the front side of the silicon solar cell provided in the embodiment of the present application can well balance the relationship between tension and photoelectric conversion efficiency, ensuring that the conductive silver paste has high tension while having excellent photoelectric conversion efficiency, thereby giving it wide adaptability and being able to adapt to various silicon solar cells prepared by different processes and of different types.
[0039] Specifically, the conductive silver paste for the front side of the silicon solar cell provided by the present application, silver powder as the main component, is a key substance in the conductive silver paste. In the embodiment of the present application, the silver powder can be micron-grade silver powder, or it can be micron-grade nano-grade mixed silver powder. In some embodiments, the particle size of the silver powder is less than or equal to 5 microns. In the embodiment of the present invention, the weight percentage of the silver powder is 70.0%-94.0%. Exemplarily, the weight percentage of the silver powder can be 70.0%, 75.0%, 80.0%, 85.0%, 90.0%, 94.0% and other specific parts.
[0040] In the embodiment of the present invention, the glass material in the conductive silver paste on the front of the silicon solar cell is used to etch the anti-reflection film layer on the surface of the silicon solar cell, increase the incorporation of silver ions, and promote the silver powder to form a good ohmic contact with the silicon wafer. In order to improve the adaptability of the conductive silver paste on the front of the silicon solar cell to silicon solar cells prepared by different processes and of different types, the glass powder in the embodiment of the present application uses at least two glass powders with different components to form a combined glass powder, and the combined glass powder includes at least two of the pre-reaction glass powder, the viscosity-enhancing glass powder, and the post-reaction glass powder. The embodiment of the present application improves the comprehensive performance of the conductive silver paste on the front of the silicon solar cell by the mutual coordination of at least two of the pre-reaction glass powder, the viscosity-enhancing glass powder, and the post-reaction glass powder.
[0041] In the embodiments of the present application, the pre-reaction glass powder contains both Te-O-Te structure and Te-O-Si structure. It should be understood that the "Te-O-Te structure" and "Te-O-Si structure" in the embodiments of the present application do not refer to the molecular formula of the substance, but only the local microstructure of the substance containing the corresponding atomic connection relationship. Exemplarily, the "Te-O-Te structure" only represents a structure formed by an O atom connected to two Te atoms at the same time, and does not mean that the Te atom is connected to only one O atom; similarly, the "Te-O-Si structure" only represents a structure formed by an O atom connected to a Te atom and a Si atom at the same time, and does not mean that the Te atom and the Si atom are only connected to one O atom.
[0042] In the embodiment of the present application, the content of Te-O-Te structure in the pre-reaction glass powder is higher than that of Te-O-Si structure, and the Te-O-Te structure is the main structure of the glass. The melting point of the glass powder thus formed is relatively low. More importantly, the glass powder reacts more strongly with the silver powder during the sintering process of the silver paste, and has a stronger ability to enhance the oxidation and melting of silver, so that the conductive silver paste can carry more silver, thereby increasing the silver content of the contact layer interface of the silicon solar cell using the conductive silver paste.
[0043] In some embodiments, the elements in the pre-reaction glass powder include Te, Li, Na, K, Zn, Ca, Pb, Si, Mg, Cu, Ag, W, and Bi, and the total molar amount of oxides in the pre-reaction glass powder is 100%, and the molar percentages of TeO2, Li2O, and PbO in the pre-reaction glass powder are as follows:
[0044] TeO2 30.0%-70.0%;
[0045] Li2O 0-30.0%;
[0046] PbO 0-50.0%.
[0047] The above-mentioned pre-reaction glass, on the one hand, has a strong ability to oxidize and melt into silver after contacting with silver, so that the conductive silver paste can carry more silver, thereby increasing the silver content of the silicon solar cell using the conductive silver paste; on the other hand, the pre-reaction glass powder with the above-mentioned composition and content characteristics reacts with the silver powder in the pre-sintering stage to weakly etch the surface of the silicon solar cell, and reacts with the post-reaction glass powder in the post-sintering stage of the silver paste to reduce the corrosion effect on the silicon substrate, thereby avoiding over-corrosion.
[0048] In this embodiment, the pre-reaction glass powder contains, in addition to TeO2, Li2O and PbO, oxides formed by other elements, namely, first other oxides, which include at least one oxide formed by Na, K, Zn, Ca, Si, Mg, Cu, Ag, W and Bi. The total molar amount of the oxides in the pre-reaction glass powder is 100%, and the sum of the molar percentages of the first other oxides is 0 to 40%. It should be understood that the contents of Li2O, PbO and the first other oxide cannot be zero at the same time.
[0049] In the embodiment of the present application, the post-reaction glass powder contains both Te-O-Te structure and Te-O-Si structure, and the content of Te-O-Te structure is lower than that of Te-O-Si structure. The post-reaction glass powder thus obtained has Te-O-Si structure as the main glass structure. On the one hand, the glass powder melting point is moderate, which is higher than the melting point of the pre-reaction ratio. The difference in the melting points of the two effectively realizes the separation of the functions of the two, thereby avoiding insufficient sintering of the silver layer and effectively improving the sintering effect. On the other hand, the Te-O-Si structure has a larger polarity relative to the Te-O-Te structure or the Si-O-Si structure. Therefore, the Ag ions melted into the Te-O-Si structure are very easy to precipitate due to the difference in force when the temperature is reduced, which is conducive to the precipitation of silver on the surface of the silicon solar cell, and then forms an excellent ohmic contact.
[0050] In some embodiments, the elements in the post-reaction glass powder include Si, Li, Na, K, Zn, Ca, Pb, Te, Bi, Tl, Cu, W, Mo, Mg, and B, and the molar content of SiO2, PbO, TeO2, and Li2O in the post-reaction glass powder is as follows, based on the total molar amount of the oxides in the post-reaction glass powder being 100%.
[0051]
[0052] On the one hand, the above-mentioned post-reaction glass is conducive to the precipitation of silver melted into the pre-reaction glass powder, thereby forming a dense silver layer on the surface of the silicon solar cell and improving the ohmic contact; on the other hand, the post-reaction glass powder mainly etches the anti-reflection film layer on the surface of the battery in the pre-sintering stage.
[0053] In this embodiment, the post-reaction glass powder contains, in addition to SiO2, PbO, TeO2 and Li2O, oxides formed by other elements, i.e., second other oxides, which include oxides formed by at least one of Na, K, Zn, Ca, Bi, Tl, Cu, W, Mo, Mg and B. The total molar amount of the oxides in the pre-reaction glass powder is 100%, and the sum of the molar percentages of the second other oxides is 0 to 20%. It should be understood that the contents of SiO2, PbO, TeO2 and Li2O and the second other oxides cannot be zero at the same time.
[0054] In some embodiments, the combined glass frit is a glass frit formed by combining a front-reaction glass frit and a post-reaction glass frit.
[0055] In some embodiments, the combined glass powder is a glass powder formed by combining a front-reaction glass powder and a rear-reaction glass powder, and the elements in the front-reaction glass powder include Te, Li, Na, K, Zn, Ca, Pb, Si, Mg, Cu, Ag, W, and Bi, and the total molar amount of oxides in the front-reaction glass powder is 100%. In the front-reaction glass powder, the molar percentages of the following components are as follows:
[0056]
[0057] The elements in the post-reaction glass powder include Si, Li, Na, K, Zn, Ca, Pb, Te, Bi, Tl, Cu, W, Mo, Mg, and B, and the total molar amount of oxides in the post-reaction glass powder is 100%. The molar percentages of the following components in the post-reaction glass powder are as follows:
[0058]
[0059] The combined glass powder thus formed, the pre-reaction glass powder can promote the melting of silver and improve the stability of the melted silver, and the post-reaction glass powder can improve the precipitation of the silver after melting. The combination of the two not only increases the silver content of the glass powder loading interface during the silver paste sintering process, but also increases the number of silver nanoparticles precipitated during the sintering cooling process, and in the post-sintering stage, it interacts with the pre-reaction glass to form an excellent ohmic contact, reducing the contact resistance and improving the photoelectric conversion efficiency. In addition, there are differences in melting point and fluidity after melting between the above two glass powders, which can effectively achieve full sintering of the two without mutual interference during the silver paste sintering process, thereby realizing the separation of the functions of the two.
[0060] In the embodiments of the present application, the viscosity of the thickened glass powder is extremely high in the pre-sintering stage and flows slowly. At the same time, it has a strong sintering-aiding effect and weak corrosiveness in the middle and late stages of sintering. Therefore, it can improve the density of the silver layer sintered by the silver paste and reduce the effect on the pre-reaction and post-reaction glass and the impact on the contact effect.
[0061] In some embodiments, in the thickened glass powder, the sum of the molar percentages of the metal element oxides is greater than or equal to 60%, based on the total molar amount of the element oxides in the thickened glass powder being 100%. In this case, the metal oxides interact with the residual organic carrier during the sintering process of the silver paste and are reduced to corresponding metal microparticles, which react with the silver powder particles to form a silver alloy, thereby helping to burn the silver layer. The thickened glass with a high metal oxide content is easy to reduce to a low-melting-point metal, which can react well with the silver powder on the surface of the silver powder to form a low-melting-point high-strength alloy, thereby improving the sintering density and fracture strength between the silver powders.
[0062] In some embodiments, the elements in the tackifying glass powder include W, Bi, Li, Na, K, Si, Zn, Ca, Pb, Te, Mg, and Ge, and based on the total molar amount of oxides in the tackifying glass powder as 100%, the molar percentages of WO3, Bi2O3, Li2O, PbO, and TeO2 in the tackifying glass powder are as follows:
[0063]
[0064]
[0065] In this embodiment, on the one hand, the viscosity-enhancing glass powder contains a high content of WO3 and Bi2O3, a large amount of WO structure and Bi-O structure, which gives the viscosity-enhancing peeling a higher melting point. When the combination glass powder contains viscosity-enhancing glass powder, a melting point difference is formed between the viscosity-enhancing glass powder and the pre-reaction glass powder and / or the post-reaction glass powder, thereby realizing the functions and sintering stratification of the two or three, so that the components interact and restrict each other at different stages, avoiding the problem that the single glass sintering window is too narrow, resulting in confusion of glass powder functions, and then affecting the effect of each glass powder. On the other hand, the network intermediates and structural exosomes in the above-mentioned viscosity-enhancing glass powder are mostly metal oxides. These metal oxide compositions are easy to interact with the residual organic carrier during the silver paste sintering process, and are reduced to corresponding metal microparticles, and the metal microparticles then interact with the silver powder particles to form a silver alloy, which plays a role in assisting the firing of the silver layer. In particular, when the combination glass powder contains both the pre-reaction glass powder and the post-reaction glass powder, the embodiment of the present application adds the above-mentioned viscosity-enhancing glass powder to improve the sintering effect of the silver layer, avoiding the problem of insufficient sintering of the silver layer.
[0066] In this embodiment, the viscosity-enhancing glass powder contains oxides formed by other elements in addition to WO3, Bi2O3, Li2O, PbO and TeO2, namely, the third other oxide, which includes at least one oxide formed by Na, K, Si, Zn, Ca, Mg and Ge. Taking the total molar amount of the oxides in the viscosity-enhancing glass powder as 100%, the sum of the molar percentages of the third other oxides is 0 to 20%. It should be understood that the contents of WO3, Bi2O3, Li2O, PbO, TeO2 and the third other oxide cannot be zero at the same time.
[0067] In some embodiments, the combined glass powder is a glass powder formed by combining a pre-reaction glass powder and a viscosity-enhancing glass powder, and the elements in the pre-reaction glass powder include Te, Li, Na, K, Zn, Ca, Pb, Si, Mg, Cu, Ag, W, and Bi, and the total molar amount of oxides in the pre-reaction glass powder is 100%. In the pre-reaction glass powder, the molar percentages of the following components are as follows:
[0068]
[0069]
[0070] The elements in the viscosity-enhancing glass powder include W, Bi, Li, Na, K, Si, Zn, Ca, Pb, Te, Mg, and Ge. Taking the total molar amount of the oxides in the viscosity-enhancing glass powder as 100%, the molar percentages of WO3, Bi2O3, Li2O, PbO, and TeO2 in the viscosity-enhancing glass powder are as follows:
[0071]
[0072] The combination of viscosity-enhancing glass powder and pre-reaction glass powder can increase the silver loading of silver paste and enhance the sintering effect of silver powder, which is beneficial for the precipitation of silver powder on the surface and the formation of low-melting-point high-strength alloy with reduced low-melting-point metal, thereby improving the sintering density and fracture strength between silver powders and enhancing the balanced welding tension of the conductive silver paste on the front of silicon solar cells.
[0073] In some embodiments, the combined glass powder is a glass powder formed by combining a post-reaction glass powder and a tackifying glass powder, and the elements in the tackifying glass powder include W, Bi, Li, Na, K, Si, Zn, Ca, Pb, Te, Mg, and Ge, and based on the total molar amount of oxides in the tackifying glass powder as 100%, the molar percentages of WO3, Bi2O3, Li2O, PbO, and TeO2 in the tackifying glass powder are as follows:
[0074]
[0075] The elements in the post-reaction glass powder include Si, Li, Na, K, Zn, Ca, Pb, Te, Bi, Tl, Cu, W, Mo, Mg, and B, and the total molar amount of oxides in the post-reaction glass powder is 100%. The molar percentages of the following components in the post-reaction glass powder are as follows:
[0076]
[0077] The combination of viscosity-enhancing glass powder and post-reaction glass powder can enhance the sintering effect of silver powder, facilitate the precipitation of silver powder on the surface and form a low-melting-point high-strength alloy with the reduced low-melting-point metal, thereby improving the sintering density and fracture strength between silver powders, and enhancing the balanced welding tension of the conductive silver paste on the front of silicon solar cells.
[0078] In some embodiments, the combined glass powder is a glass powder formed by combining a pre-reaction glass powder, a viscosity-enhancing glass powder, and a post-reaction glass powder. The elements in the pre-reaction glass powder include Te, Li, Na, K, Zn, Ca, Pb, Si, Mg, Cu, Ag, W, and Bi, and the total molar amount of oxides in the pre-reaction glass powder is 100%. In the pre-reaction glass powder, the molar percentages of the following components are as follows:
[0079]
[0080] The elements in the post-reaction glass powder include Si, Li, Na, K, Zn, Ca, Pb, Te, Bi, Tl, Cu, W, Mo, Mg, and B, and the total molar amount of oxides in the post-reaction glass powder is 100%. The molar percentages of the following components in the post-reaction glass powder are as follows:
[0081]
[0082]
[0083] The elements in the viscosity-enhancing glass powder include W, Bi, Li, Na, K, Si, Zn, Ca, Pb, Te, Mg, and Ge. Taking the total molar amount of the oxides in the viscosity-enhancing glass powder as 100%, the molar percentages of WO3, Bi2O3, Li2O, PbO, and TeO2 in the viscosity-enhancing glass powder are as follows:
[0084]
[0085] In this embodiment, the glass structures and compositions of the various glass powders at the glass melting points are quite different (there are also large differences in the main core elements), and the glass powders are different. In addition, the viscosity-enhancing glass powder can improve the sintering effect on the silver layer. Therefore, in the process of sintering the silver paste into the silver layer, the problem of insufficient sintering can be avoided, and the adverse effects of the mixed melting of the glass powders on the sintering of the silver layer can be avoided. As a result, the three different glass powders play different roles in different sintering stages, which can better assist the sintering of the silver powder to ensure better welding tension, while ensuring a good contact effect and improving the output power of the battery. Specifically, the pre-reaction glass reacts with silver powder in the pre-sintering stage to weakly etch the battery surface, and reacts with the post-reaction glass in the post-sintering stage to reduce the corrosion effect on the silicon substrate and avoid over-corrosion; the post-reaction glass mainly etches the battery surface in the pre-sintering stage of the reaction, and reacts with the pre-reaction glass in the post-sintering stage to promote the formation of excellent ohmic contact; the viscosity-enhancing glass has a very strong sintering-aiding effect and milder corrosion in the middle and late stages of sintering, thereby ensuring the density of the silver layer sintering while avoiding the impact on the interface between the silver grid line and the silicon battery.
[0086] Due to differences in structure and doping concentration, different process cells have different corrosion and contact requirements for glass. The combined glass powder provided in the embodiment of the present application can improve ohmic contact by the interaction of front-reaction glass powder and post-reaction glass powder. The degree of corrosion can also be improved by changing the ratio between different glass powders, so that the obtained conductive silver paste on the front side of the silicon solar cell can be widely used in silicon solar cells with different processes.
[0087] In an embodiment of the present application, the weight percentage of the combined glass powder is 0.1%-8.0%. For example, the weight percentage of the combined glass powder can be 0.1%, 0.5%, 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%, 7.0%, 8.0% and other specific proportions.
[0088] In the embodiments of the present invention, the organic carrier is mainly used to adjust the printability of the silver paste. The quality of the organic carrier directly determines the screen printing effect of the conductive silver paste on the front of the silicon solar cell. Therefore, a stable and reliable organic carrier is a prerequisite for the formation of the front electrode of the crystalline silicon solar cell. In some embodiments, the organic carrier includes an organic solvent, a resin, a thickener, and a sodium-containing organic stabilized anticoagulant. Among them, the organic chain end of the sodium-containing organic stabilized anticoagulant has good compatibility with the organic solvent, and the sodium-containing organic stabilized anticoagulant can free Na + ions, these Na +Ions can lower the freezing point of organic solvents and the volatility of organic solvents at room temperature, thereby improving the stability of conductive silver paste for silicon solar cells and broadening the temperature and humidity range in which the silver paste can work stably. The resulting silver paste still has good stability and suitable viscosity even when the temperature or humidity fluctuates, thus avoiding the impact of storage and transportation of the silver paste on printing performance.
[0089] In some embodiments, the mass percentage of the sodium-containing organic stable anticoagulant is 0.1%-10.0% based on the total weight of the organic carrier as 100%. In this case, the sodium-containing organic stable anticoagulant can improve the stability of the conductive silver paste on the front of the silicon solar cell in a temperature difference environment and a humidity difference environment, and the content is appropriate and will not affect other properties of the silver paste.
[0090] In some embodiments, the organic carrier may contain one sodium-containing organic stable anticoagulant, or may contain two or more sodium-containing organic stable anticoagulants. In some embodiments, the sodium-containing organic stable anticoagulant is selected from at least one of sodium citrate, sodium dodecylbenzene sulfonate, sodium carboxymethyl cellulose, sodium carboxymethyl cellulose, sodium dodecyl sulfate, sodium carboxymethyl starch, sodium phenol, and sodium stearate.
[0091] The conductive silver paste for the front side of the silicon solar cell provided in the embodiment of the present application has high welding tension and excellent photoelectric conversion efficiency. Since the silver paste can better balance the relationship between welding tension and photoelectric conversion efficiency, it has a wide range of adaptability and can be adapted to various silicon solar cells prepared by different processes and of different types. It can also well adapt to the problem of poor printability of the silver paste due to changes in temperature or humidity.
[0092] The conductive silver paste on the front side of the silicon solar cell provided in the embodiment of the present application can be prepared by the following method.
[0093] Accordingly, in a second aspect, an embodiment of the present application provides a method for preparing a conductive silver paste on the front side of a silicon solar cell, comprising the following steps:
[0094] S01. According to the first aspect of the silicon solar cell front conductive silver paste formula provided by providing silver powder, pre-reaction glass powder, viscosity-enhancing glass powder, post-reaction glass powder and an organic carrier;
[0095] S02. The pre-reaction glass powder, the viscosity-enhancing glass powder and the post-reaction glass powder are mixed to obtain a combined glass powder;
[0096] S03. The combined glass powder is mixed with silver powder and an organic carrier and then ground to obtain a conductive silver paste for the front side of a silicon solar cell.
[0097] The method for preparing the conductive silver paste for the front side of a silicon solar cell provided in the embodiment of the present application is to mix the glass powders, mix them with the silver powder and the organic carrier, and grind them to obtain the conductive silver paste. The method is simple to operate, and more importantly, the conductive silver paste for the front side of a silicon solar cell obtained thereby has a wide range of adaptability and can be adapted to silicon solar cells prepared by various processes and of different types.
[0098] In the above step S01, the formula of the conductive silver paste on the front side of the silicon solar cell is as described above, and will not be repeated here to save space.
[0099] In the above step S02, the pre-reaction glass powder, the viscosity-enhancing glass powder and the post-reaction glass powder are mixed so that each glass powder is evenly distributed in the conductive silver paste.
[0100] In some embodiments, the preparation methods of the pre-reaction glass powder, the viscosity-enhancing glass powder, and the post-reaction glass powder are as follows:
[0101] The raw material precursors of each glass powder are weighed, and the raw material precursors of the pre-reaction glass powder, the raw material precursors of the thickening glass powder and the raw material precursors of the post-reaction glass powder are mixed and treated respectively, and then high-temperature fast melting, water quenching, drying, and crushing are carried out in sequence to obtain the pre-reaction glass powder, the thickening glass powder, and the post-reaction glass powder, respectively, wherein the temperature of the high-temperature fast melting is 1000° C. to 1200° C., and the time is 3 min to 24 min. In this case, the physical properties and component compositions of the obtained glass powders are consistent, which is conducive to improving the welding tensile force of the silver paste.
[0102] In some embodiments, the preparation method of the organic carrier is:
[0103] The organic solvent is divided into a first organic solvent and a second organic solvent in a mass ratio of (7.5-9.5): (0.5-2.5), the resin, the thickener, the sodium-containing organic stabilizer anticoagulant and the first organic solvent are mixed, and then the organic solvent is added and mixed again to obtain an organic vehicle. In this case, the organic solvent is added in batches to improve the dispersion uniformity of the components in the organic vehicle.
[0104] In a third aspect, an embodiment of the present application provides a method for preparing a front electrode of a silicon solar cell, comprising the following steps:
[0105] E01 provides a silicon semiconductor element, the silicon semiconductor element has an insulating film disposed on one side of the surface;
[0106] E02. The conductive silver paste on the front of the silicon solar cell provided in the first aspect or the conductive silver paste on the front of the silicon solar cell provided in the second aspect is dried and heated to 700 ℃ ~ 950 ℃ for sintering;
[0107] E03. Cool down to obtain the front electrode of the silicon solar cell.
[0108] The method for preparing the front electrode of a silicon solar cell provided in the embodiment of the present application is to print the front conductive silver paste of the silicon solar cell provided above on the insulating film on the surface of one side of the silicon semiconductor element. The method is simple to operate and easy to control. More importantly, since the front conductive silver paste of the silicon solar cell described above is used, the method can be adapted to the preparation of the front electrodes of silicon solar cells prepared by various processes and of different types.
[0109] In the embodiments of the present application, the structure of the silicon semiconductor element is not limited. In some embodiments, the insulating film is a stacked layer formed by one or more of silicon nitride, titanium oxide, aluminum oxide, and silicon oxide.
[0110] The following describes the invention in conjunction with specific embodiments.
[0111] 1. Preparation of composite glass powder:
[0112] Take the glass raw materials with the contents shown in Table 1, respectively, mix the glass raw materials in A1-5, B1-5 and C1-5, melt them at 1150° C. for 30 min, pour them into a cold water bucket for water quenching, filter out the quenched glass slag, dry them, and grind them to obtain the pre-reaction glass powder A1-5, the tackifying glass powder B1-5 and the post-reaction glass powder C1-5, respectively;
[0113] Pre-reaction glass powders A1-A5, viscosity-enhancing glass powders B1-B5 and post-reaction glass powders C1-C6 were mixed in the mass proportions shown in Table 2 to obtain combined glass powders D1-D8.
[0114] In Table 2, the glass number / mass mixing ratio refers to the mass fraction of the glass with the corresponding number. Taking D1 as an example, it means: the glass powders numbered A2, B3, and C2 are mixed in a mass ratio of 1:1:2 to obtain a combined glass powder.
[0115] Table 1
[0116]
[0117] Table 2
[0118] Combination glass number A Glass number / mass mixing ratio B Glass number / mass mixing ratio C Glass number / mass mixing ratio D1 A2 / 1 B3 / 1 C2 / 2 D2 A5 / 1 C1 / 4 D3 A1 / 1 C5 / 5 D4 A3 / 1 B4 / 4 C4 / 1 D5 A3 / 1 B4 / 3 D6 B2 / 2 C6 / 3 D7 A6 / 1 B1 / 10 C5 / 4 D8 A4 / 1 B5 / 1 C3 / 8 D9 A4 / 3 B5 / 1 C3 / 3
[0119] 2. Preparation of organic carrier:
[0120] After mixing and stirring the resin, thickener, sodium-containing organic stabilizer anticoagulant of the type and content shown in Table 3 below, and 90% by weight of an organic solvent (i.e., the first organic solvent), add -10% of an organic solvent (i.e., the second organic solvent), and stir again to obtain organic carriers numbered E1-E6, respectively.
[0121] Table 3
[0122]
[0123] Examples 1-10
[0124] A silicon solar cell front silver paste, the preparation method of which is as follows:
[0125] Based on a total mass of 400 g of silver paste, silver powder, glass powder and an organic carrier were weighed according to the types and contents of raw materials shown in Table 4, mixed and then subjected to three-roll milling to prepare conductive silver pastes numbered F1-F10, respectively.
[0126] Comparative Examples 1-5
[0127] A silicon solar cell front silver paste, the preparation method of which is as follows:
[0128] Based on a total mass of 400 g of silver paste, silver powder, glass powder and an organic carrier were weighed according to the raw material types and contents shown in Table 4, mixed and then subjected to three-roll milling to prepare conductive silver pastes numbered X1-5, respectively.
[0129] Table 4
[0130]
[0131] Test Example 1
[0132] The silver paste on the front side of the silicon solar cell prepared in Example 1-2 and Comparative Example 1-2 was printed under the printing processing conditions in Table 5. Four parallel tests were set up in each group. The printing results are shown in Table 5 below.
[0133] Table 5
[0134]
[0135]
[0136] As can be seen from Table 5, the silver pastes on the front side of the silicon solar cell prepared in Examples 1-2 (numbered F1-F2) and Comparative Example 1 (numbered X1) have basically no broken grids and have good printing effects; while the silver paste corresponding to the silver paste on the front side of the silicon solar cell prepared in Comparative Example 2 (numbered X2) has poor printing, many broken grids, and even cannot be printed. This is attributed to the fact that the silver paste corresponding to numbered X2 does not contain a sodium-containing organic stabilized anticoagulant. It can be seen that the presence of a sodium-containing organic stabilized anticoagulant can improve the printing effect of the silver paste on the front side of the silicon solar cell.
[0137] Test Example 2
[0138] The front silver paste of the silicon solar cell prepared in Examples 1-10 and Comparative Examples 1-5 was printed on the surface of one side of the insulating film of the silicon semiconductor element, and sintered to form a silver layer to obtain a silicon solar cell. The photoelectric conversion efficiency and welding tensile force of the obtained silicon solar cell and the EL test results of the cells with different processes were tested, and the results are shown in Table 6.
[0139] Table 6
[0140] Silver paste number Battery Type EL status Photoelectric conversion efficiency Welding tension X1 Conventional single crystal No EL black spots 19.82% 2.65N F1 Conventional single crystal No EL black spots 19.88% 2.72N F2 Conventional single crystal No EL black spots 19.90% 2.70N X2 Conventional single crystal No EL black spots 19.85% 2.05N X3 Conventional single crystal EL black spots 9.02% 3.95N X4 Conventional single crystal No EL black spots 19.80% 1.95N X5 Conventional single crystal No EL black spots 19.85% 2.05N F3 Conventional single crystal No EL black spots 19.96% 2.80N F4 Conventional single crystal No EL black spots 19.86% 3.77N F6 Conventional single crystal No EL black spots 19.84% 2.23N F7 Conventional single crystal No EL black spots 19.93% 2.89N F8 Conventional single crystal No EL black spots 19.91% 3.13N F9 Conventional single crystal No EL black spots 19.88% 2.93N X1 Polycrystalline Black Silicon No EL black spots 18.52% 1.82N F1 Polycrystalline Black Silicon No EL black spots 18.56% 1.96N F2 Polycrystalline Black Silicon No EL black spots 18.66% 1.97N X2 Polycrystalline Black Silicon No EL black spots 18.56% 1.51N X3 Polycrystalline Black Silicon EL black spots 10.77% 3.17N X4 Polycrystalline Black Silicon No EL black spots 18.51% 1.95N X5 Polycrystalline Black Silicon No EL black spots 18.53% 1.41N F1 Perc single crystal No EL black spots 21.76% 2.36N F2 Perc single crystal No EL black spots 21.83% 2.55N X2 Perc single crystal Edge foggy black spots 18.72% 2.32N X3 Perc single crystal EL black spots 3.02% 4.23N X4 Perc single crystal No EL black spots 21.58% 1.89N X5 Perc single crystal Large area of EL black spots 19.55% 1.39N F1 Se-Perc Single Crystal No EL black spots 22.12% 2.38N F2 Se-Perc Single Crystal No EL black spots 22.17% 2.52N X2 Se-Perc Single Crystal EL black spots 21.88% 2.35N X3 Se-Perc Single Crystal EL black spots 3.02% 3.98N X4 Se-Perc Single Crystal Dot EL black spots 21.58% 1.58N X5 Se-Perc Single Crystal Fog EL black spots 19.55% 1.73N F5 Se-Perc Single Crystal No EL black spots 22.09% 2.94N F10 Se-Perc Single Crystal No EL black spots 22.21% 2.74N
[0141] As can be seen from Table 6, the conductive silver paste (F1-10, X1) prepared by the combined glass powder is printed and sintered to form a silver layer, and the cell EL test has no EL black spots; and the various types of solar cells obtained have both good photoelectric conversion efficiency and welding tension, which can be applied to the use requirements of silicon solar cells of various processes. However, when the conductive silver paste X2-X5 prepared by the single glass powder X2-X5 is printed and sintered to form a silver electrode, when making conventional monocrystalline silicon solar cells, the obtained solar cells have a relatively small welding tension or photoelectric conversion efficiency, and some even have black spots, which cannot be used; when making polycrystalline silicon solar cells, the obtained solar cells have a relatively small welding tension, and the photoelectric conversion efficiency or welding tension is also relatively low, and some even have black spots, which cannot be used; when making Perc monocrystalline silicon solar cells, the obtained solar cells have a relatively small photoelectric conversion efficiency, and there are edge foggy black spots on the surface of the silver layer; when making Se-Perc monocrystalline silicon solar cells, the photoelectric conversion efficiency or welding tension is low, and there are dot-shaped black spots on the surface of the silver layer, and Se-Perc monocrystalline silicon solar cells cannot be used.
[0142] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A conductive silver paste for the front side of a silicon solar cell, characterized in that: Taking the total weight of the conductive silver paste on the front side of the silicon solar cell as 100%, the following raw material components are included in the following weight percentages: Silver powder 70.0%-94.0%; Combined glass powder 0.1%-8.0%; Organic carrier 5.0%-30.0%; The combined glass powder includes at least two of a front-reaction glass powder, a viscosity-enhancing glass powder and a rear-reaction glass powder; wherein the front-reaction glass powder and the rear-reaction glass powder both contain a Te-O-Te structure and a Te-O-Si structure, and the content of the Te-O-Te structure in the front-reaction glass powder is higher than the content of the Te-O-Si structure, and the content of the Te-O-Te structure in the rear-reaction glass powder is lower than the content of the Te-O-Si structure; The elements in the pre-reaction glass powder include Te, Li, Na, K, Zn, Ca, Pb, Si, Mg, Cu, Ag, W, and Bi, and based on the total molar amount of oxides in the pre-reaction glass powder as 100%, the molar percentages of TeO2, Li2O, and PbO in the pre-reaction glass powder are as follows: TeO2 30.0%-70.0%; Li2O0-30.0%; PbO0-50.0%; The elements in the viscosity-enhancing glass powder include W, Bi, Li, Na, K, Si, Zn, Ca, Pb, Te, Mg, and Ge, and taking the total molar amount of oxides in the viscosity-enhancing glass powder as 100%, the molar percentages of WO3, Bi2O3, Li2O, PbO, and TeO2 in the viscosity-enhancing glass powder are as follows: WO310.0%-30.0%; Bi2O35.0%-30.0%; Li2O10.0%-40.0%; PbO0-30.0%; TeO20-30.0%; The elements in the post-reaction glass powder include Si, Li, Na, K, Zn, Ca, Pb, Te, Bi, Tl, Cu, W, Mo, Mg, and B. Taking the total molar amount of oxides in the post-reaction glass powder as 100%, the molar percentages of SiO2, PbO, TeO2, and Li2O in the post-reaction glass powder are as follows: SiO2 15.0%-30.0%; PbO15.0%-30.0%; TeO2 15.0%-35.0%; Li2O10.0%-20.0%.
2. The conductive silver paste for the front side of a silicon solar cell according to claim 1, characterized in that: In the viscosity-enhancing glass powder, based on the total molar amount of element oxides in the viscosity-enhancing glass powder being 100%, the sum of the molar percentages of metal element oxides is greater than or equal to 60%.
3. The conductive silver paste for the front side of a silicon solar cell according to claim 1, characterized in that: The organic carrier comprises an organic solvent, a resin, a thickener and an organic stabilizing anticoagulant containing sodium.
4. The conductive silver paste for the front side of a silicon solar cell according to claim 3, characterized in that: Based on the total weight of the organic carrier as 100%, the mass percentage of the sodium-containing organic stable anticoagulant is 0.1%-10.0%; and / or The sodium-containing organic stable anticoagulant is selected from at least one of sodium citrate, sodium dodecylbenzene sulfonate, sodium carboxymethyl cellulose, sodium carboxymethyl cellulose, sodium dodecyl sulfate, sodium carboxymethyl starch, sodium phenol, and sodium stearate.
5. A method for preparing conductive silver paste for the front side of a silicon solar cell, characterized in that: The following steps are involved: According to the formula of the conductive silver paste for the front side of the silicon solar cell according to any one of claims 1 to 4, silver powder, front reaction glass powder, viscosity-enhancing glass powder, rear reaction glass powder and an organic carrier are provided; The pre-reaction glass powder, the viscosity-enhancing glass powder and the post-reaction glass powder are mixed to obtain a combined glass powder; The combined glass powder is mixed with the silver powder and the organic carrier and subjected to grinding treatment to prepare a conductive silver paste on the front side of a silicon solar cell.
6. The method for preparing the conductive silver paste for the front side of a silicon solar cell according to claim 5, characterized in that: The preparation methods of the pre-reaction glass powder, the viscosity-enhancing glass powder, and the post-reaction glass powder are as follows: Weighing the raw material precursors of each glass powder, mixing the raw material precursor of the pre-reaction glass powder, the raw material precursor of the viscosity-enhancing glass powder and the raw material precursor of the post-reaction glass powder respectively, and then sequentially performing high-temperature rapid melting, water quenching, drying and pulverizing to obtain the pre-reaction glass powder, the viscosity-enhancing glass powder and the post-reaction glass powder respectively, wherein the temperature of the high-temperature rapid melting is 1000° C. to 1200° C., and the time is 3 min to 24 min; and / or The preparation method of the organic carrier is: The organic solvent is divided into a first organic solvent and a second organic solvent in a mass ratio of (7.5-9.5): (0.5-2.5), a resin, a thickener, a sodium-containing organic stabilizing anticoagulant and the first organic solvent are mixed, and then the organic solvent is added and mixed again to obtain the organic carrier.
7. A method for preparing a front electrode of a silicon solar cell, comprising the following steps: Providing a silicon semiconductor element, wherein an insulating film is disposed on one surface of the silicon semiconductor element; Printing the conductive silver paste for the front side of the silicon solar cell according to any one of claims 1 to 4 or the conductive silver paste for the front side of the silicon solar cell obtained by the method according to any one of claims 5 to 6 on the insulating film, drying it, and heating it to 700° C. to 950° C. for sintering; The silicon solar cell front electrode is obtained by cooling.