High energy density alkaline iron-sulfur flow battery and preparation method thereof
By adjusting the solubility of ferricyanide/ferrocyanide and using high-performance separator materials, a high-energy-density alkaline iron-sulfur flow battery was constructed, which solved the problems of high installed cost and low energy density of all-vanadium flow batteries. Long cycle life and low-cost energy storage effects are achieved.
Patent Information
- Application Number
- CN202210897479.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-28
AI Technical Summary
Existing all-vanadium redox flow batteries use precious metal vanadium and high-cost separator materials, resulting in high installation costs and low energy density, which limits the improvement of their energy storage capacity.
By adjusting the type, quantity, and ratio of the positive and negative supporting electrolytes, increasing the solubility of ferricyanide/ferrocyanide, and using high-performance separators and high-catalytic activity electrode materials, a high-energy-density alkaline iron-sulfur solution was constructed The flow battery system suppresses the shuttle effect of polysulfides and reduces installation costs.
Alkaline iron-sulfur flow batteries achieve high energy density, long cycle life and low chemical cost, significantly reducing installation costs and providing technical support in the field of large-scale energy storage.
Smart Images

Figure CN115000480B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of liquid flow batteries and relates to a high energy density alkaline iron-sulfur liquid flow battery and a preparation method thereof. Background Art
[0002] Due to the excessive use of fossil energy, such as energy shortages and environmental pollution, secondary clean energy such as wind energy and solar energy has been used on a large scale. However, the inherent instability and discontinuity of wind energy and photovoltaic power generation limit their further promotion and use. Therefore, the development of large-scale energy storage technology with high energy storage efficiency, low installation cost and stable cycle has become the key to the promotion and use of renewable energy. Compared with existing electrochemical energy storage technologies such as lithium-ion batteries and lead-acid batteries, all-vanadium redox flow batteries have the advantages of capacity and power decoupling, long cycle life and high safety. It is one of the most promising long-term and efficient energy storage technologies for widespread deployment. However, the existing all-vanadium flow batteries with a high degree of commercial maturity use precious metal vanadium as electrolyte, and the diaphragm materials are heavily dependent on imports, resulting in excessively high battery installation costs. At the same time, the low energy density has always limited the energy storage capacity of vanadium flow batteries. Therefore, it is necessary to develop a new type of flow battery system.
[0003] Ferrocyanide / ferrocyanide has been widely used in various flow battery systems due to its abundant reserves, good stability, high electrochemical reversibility, and low chemical cost. Polysulfide is an ideal active substance due to its high solubility and low cost. Flow batteries constructed using ferrocyanide / ferrocyanide and polysulfide have shown excellent prospects and are expected to be gradually commercialized in the future. However, the low solubility of ferrocyanide / ferrocyanide on the positive electrode side makes the energy density of the battery too low (the solubility of sodium ferrocyanide and potassium ferrocyanide in pure water is only 0.56M and 0.76M). This physical and chemical property makes it difficult for the iron-sulfur flow battery system to achieve high energy density design. In addition, polysulfide on the negative electrode side has the problems of strong shuttle effect and low reaction activity. Therefore, the present invention adjusts the type, quantity and ratio of the positive and negative electrode supporting electrolytes, and uses high-performance diaphragms and electrode materials with high catalytic activity to successfully construct an alkaline flow battery system with high energy density, good cycle stability and low chemical cost. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a high energy density alkaline iron-sulfur flow battery, which improves the solubility of ferrocyanide / ferrocyanide, has the advantages of high energy density, long cycle life, low chemical cost, stable efficiency, etc., successfully inhibits the shuttle effect of polysulfides, and greatly reduces the installation cost of the flow battery, which has great practical significance for guiding the development of high energy density flow batteries.
[0005] Another object of the present invention is to provide a method for preparing a high energy density alkaline iron-sulfur liquid flow battery.
[0006] The technical solution adopted by the present invention is a high energy density alkaline iron-sulfur liquid flow battery, comprising a positive electrolyte, a negative electrolyte, a separator, positive and negative electrodes, the active substance in the positive electrolyte is ferrocyanide or ferrocyanide ion, and the concentration of the active substance on the positive electrode side is 0.1M~1.7M;
[0007] The active substance in the negative electrode electrolyte is a sulfide solution, and the concentration range of the negative electrode active substance is 0.1M~15M;
[0008] The supporting electrolytes in the positive and negative electrolytes are LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO with a molar concentration of 0.1M~6M. 3、 One or more of Li2CO3, LiHCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O; no matter how many supporting electrolytes are present at the positive and negative electrodes, it is necessary to ensure that the supporting electrolytes at the positive and negative electrodes have a common cation;
[0009] The diaphragm is any one of a porous membrane, a ceramic membrane or an ion exchange membrane that has been ionized;
[0010] The concentration range of the regulating ions in the positive and negative electrode electrolytes is 0.1M~2.0M, and the regulating ions are the same as the cations of the negative electrode active material and the supporting electrolyte.
[0011] Furthermore, the positive and negative electrodes are any one of carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode.
[0012] Furthermore, the diaphragm is a perfluorosulfonic acid diaphragm (Nafion diaphragm), a sulfonated polyetheretherketone diaphragm (SPEEK diaphragm), a sulfonated polyimide diaphragm (SPI diaphragm), a sulfonated polyfluorene ether ketone diaphragm (SPFEK diaphragm), a polyvinylidene fluoride diaphragm (PVDF diaphragm), a polyethersulfone diaphragm (PES diaphragm), a sulfonated polyaryletherketone diaphragm (SPPEK diaphragm), a polyaryletherketone diaphragm (PAEK diaphragm), a polysulfone fiber diaphragm (PSF diaphragm), a polyphthalazine etherketone diaphragm (PPEKK diaphragm), sulfonated polyethersulfone diaphragm (SPES diaphragm), tetrafluoroethylene diaphragm (ETFE diaphragm), polystyrene diaphragm (PS diaphragm), polyethylene diaphragm (PE diaphragm), polyphenylene diaphragm (PP diaphragm), polybenzimidazole diaphragm (PBI diaphragm), sulfonated polyarylether diaphragm, polyparaphenylene diaphragm, sulfonated polydiallyl bisphenol ether ketone diaphragm, polyfluorenyl ether ketone sulfone diaphragm, polyfluorenyl ether diaphragm, polyvinyl chloride acylation diaphragm, polyphenylene ether diaphragm or polyphenyl diaphragm.
[0013] Furthermore, the sulfide solution is a mixture of one or more of potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, thiol, thiophenol or thioether in any mass ratio.
[0014] Furthermore, when there are two supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.1M~6M, and the molar ratio of the two supporting electrolytes is in the range of 1 / 6~6 / 1.
[0015] Furthermore, when there are three supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.5M~5.0M, and the molar ratio of the three supporting electrolytes is in the range of 1:1:1~6:3:1.
[0016] Furthermore, when there are four supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.5M~4.0M, and the molar ratio of the four supporting electrolytes is in the range of 1:1:1:1~6:1:1:1.
[0017] A method for preparing a high energy density alkaline iron-sulfur flow battery comprises the following steps:
[0018] Preparation of the diaphragm: the diaphragm is any one of an ion exchange membrane, a porous membrane or a ceramic membrane; when the diaphragm is an ion exchange membrane, an ionization treatment is performed;
[0019] Preparation of electrodes: using carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode as electrode materials for batteries;
[0020] Preparation of negative electrode electrolyte: take potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, thiol, thiophenol or thioether, dissolve in an alkaline solution to obtain an alkaline solution of sulfide; then add 0.1M~2.0M regulating ions, the regulating ions are any one of LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4 or a mixture of multiple solutions, and use a magnetic stirrer to fully stir and dissolve;
[0021] Preparation of positive electrode electrolyte: dissolve one or more of potassium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, sodium ferrocyanide, ammonium ferrocyanide, ammonium ferrocyanide, lithium ferrocyanide or lithium ferrocyanide in an alkaline solution to prepare an alkaline solution of ferrocyanide / ferrocyanide; then add 0.1M~2.0M regulating ions, wherein the regulating ions are any one of LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4, or a mixture of multiple solutions, and stir and dissolve them fully with a magnetic stirrer;
[0022] The prepared positive and negative electrolytes, separators, positive and negative electrodes are assembled into an alkaline redox flow battery.
[0023] Furthermore, the alkaline solution in the preparation of the negative electrode electrolyte and the preparation of the positive electrode electrolyte is a supporting electrolyte, and the preparation method is: using deionized water to prepare LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO 3、 One or more alkaline solutions of Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O, with a total molar concentration of 0.1M~6M; no matter how many supporting electrolytes exist in the positive and negative electrodes, it is necessary to ensure that the positive and negative supporting electrolytes have a common cation.
[0024] Furthermore, in the preparation of the diaphragm, the ion exchange membrane is ionized by heating the ion exchange membrane at a constant temperature with any alkaline solution of LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO3, Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O with a concentration of 0.1M~6.0M, the heating temperature is 40~100°C, the heating time is 0.5h~8h, after the ionization process is completed, it is washed with deionized water and immersed in deionized water to obtain K + 、Na + , Li + or NH4 + type ion exchange membrane, and finally immersed in 0.1M~2.0M concentration of LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl, NH4Br or (NH4)2SO4 solution for standby use.
[0025] The beneficial effects of the present invention are:
[0026] 1. The present invention successfully increases the concentration of ferrocyanide / ferrocyanide to 1.7M by regulating the type, quantity and ratio of active substances and supporting electrolytes on the positive electrode side, unlocking the solubility limit of ferrocyanide / ferrocyanide, and can be completely dissolved at room temperature, which can achieve higher energy density than existing liquid flow battery technology. When high concentrations of ferrocyanide / ferrocyanide are used on the positive electrode side, the battery can still maintain excellent cycle stability, and no crystal precipitation is found on the positive electrode side, indicating that the iron compound electrolyte designed in this system has excellent physical and chemical properties.
[0027] 2. On the basis of increasing the concentration of the positive electrode iron compound, the present invention successfully inhibits the shuttle effect of polysulfide by constructing a strategy of consistent auxiliary ions and active material cations, and adjusts the type, quantity and proportion of supporting electrolytes, effectively extending the cycle life of the battery. At the same time, the present invention uses low-chemical-cost ferrocyanide / ferrocyanide and polysulfide as active materials, effectively solving the problem of high chemical cost of the electrolyte, that is, it has the advantages of high energy density, low chemical cost and long cycle life.
[0028] 3. In order to solve the problems of the shuttling effect and slow reaction activity of polysulfides, high-performance diaphragms and high-catalytic activity electrode materials are used to construct a long-term stable circulation alkaline iron-sulfur liquid flow battery system, which can provide support for the development of liquid flow batteries in the large-scale energy storage field.
[0029] 4. The active substances used in the embodiments of the present invention are abundant in reserves, low in cost, environmentally friendly and free of highly corrosive materials, which can effectively reduce equipment investment costs and operation and maintenance costs, and are conducive to the industrialization and scale-up of the technical solution of this application.
[0030] In summary, the present invention greatly improves the solubility of ferrocyanide / ferrocyanide and the stability of negative electrode polysulfide during the cycle by adjusting the type, quantity and ratio of positive and negative electrode supporting electrolytes, and develops and uses high-performance diaphragm materials and electrodes with high catalytic activity, thereby realizing a high-energy density iron-sulfur liquid flow battery design with long-term cycle stability, which still has a long cycle life in the battery stack system. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 This is a cycle performance diagram of the liquid flow battery in Example 1 of the present invention.
[0033] Figure 2 This is a cycle performance diagram of the liquid flow battery in Example 2 of the present invention.
[0034] Figure 3 This is a cycle performance diagram of the liquid flow battery in Example 3 of the present invention.
[0035] Figure 4 This is a capacity-voltage diagram of the liquid flow battery in Example 3 of the present invention.
[0036] Figure 5 This is a rate performance diagram of the liquid flow battery in Example 3 of the present invention.
[0037] Figure 6 This is a cycle performance diagram of the liquid flow battery in Example 4 of the present invention.
[0038] Figure 7 This is a cycle performance diagram of the liquid flow battery in Example 5 of the present invention.
[0039] Figure 8 This is a cycle performance diagram of the liquid flow battery in Example 6 of the present invention.
[0040] Fig. 9 This is a cycle performance diagram of the liquid flow battery in Example 7 of the present invention.
[0041] Fig.10 This is a cycle performance diagram of the liquid flow battery in Example 8 of the present invention.
[0042] Fig.11 This is a cycle performance diagram of the liquid flow battery in Example 9 of the present invention.
[0043] Fig.12 This is a cycle performance diagram of the liquid flow battery in Example 10 of the present invention.
[0044] Fig.13 This is a cycle performance diagram of the liquid flow battery in Example 11 of the present invention.
[0045] Fig.14 This is a cycle performance diagram of the liquid flow battery in Example 12 of the present invention.
[0046] Fig.15 This is a cycle performance diagram of the liquid flow battery in Example 13 of the present invention.
[0047] Fig.16 This is a cycle performance diagram of the liquid flow battery in Example 14 of the present invention.
[0048] Fig.17 This is a cycle performance diagram of the liquid flow battery in Example 15 of the present invention.
[0049] Fig.18 This is a cycle performance diagram of the liquid flow battery in Example 16 of the present invention.
[0050] Fig.19 It is a cycle performance diagram in comparative example 1 of the present invention.
[0051] Fig. 20 It is a capacity-voltage comparison diagram of comparative example 4 and embodiment 6 of the present invention. DETAILED DESCRIPTION
[0052] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0053] The design concept of the present invention is:
[0054] Ferrocyanide / ferrocyanide, as a low-cost, chemically stable active substance, has always been limited by its low solubility, which has always been a constraint on its development and application. Even if polysulfides have good water solubility, it is difficult to achieve high volume capacity on both sides of the battery. The present invention changes the actual solubility of ferrocyanide / ferrocyanide by continuously adjusting the type, quantity and ratio of the supporting electrolyte, and finally obtains the optimal concentration of ferrocyanide / ferrocyanide. At the same time, in order to construct a long-term stable polysulfide, the influence of the negative electrode supporting electrolyte on the polysulfide during the cycle is further regulated, the type, quantity and ratio of the supporting electrolyte are screened, and the optimal supporting electrolyte concentration for stabilizing the polysulfide is further obtained. At the same time, in order to construct a long-term stable battery system, different types of diaphragms and different electrode materials are further designed and screened, which have a high effect on the substitute of battery performance, and finally a liquid flow battery system with strong practical usability is developed.
[0055] A high energy density alkaline iron-sulfur flow battery system, including a single cell or a battery stack composed of two or more single cells. The basic components of a single cell: external liquid storage tanks for positive and negative electrodes, positive half-cell, negative half-cell, diaphragm and corresponding transmission pipelines; the external liquid storage tanks for positive and negative electrodes are used to store positive and negative electrolytes. During battery testing, the electrolyte is transported to the inside of the battery under the action of a pump to complete the reaction. The positive half-cell is composed of an electrode, a tab and a sealing material, and the negative half-cell is the same; the positive and negative half-cells are separated by a diaphragm.
[0056] The diaphragm is any one of an ion exchange membrane, a porous membrane or a ceramic membrane. The principle of using an ion exchange membrane is to conduct protons / ions with the help of anions and cations, and the positive and negative active substances will not pass through the diaphragm. Porous membranes and ceramic membranes are a type of diaphragms with relatively large pore sizes. The reason why the shuttle effect of polysulfides does not occur in the present invention is that a strategy for regulating ions is added. Even if a diaphragm with a large pore size is used, the battery can still operate normally and stably.
[0057] The ion exchange membranes used are perfluorosulfonic acid membrane (Nafion membrane), sulfonated polyetheretherketone membrane (SPEEK membrane), sulfonated polyimide membrane (SPI membrane), sulfonated polyfluorene ether ketone membrane (SPFEK membrane), polyvinylidene fluoride membrane (PVDF membrane), polyethersulfone membrane (PES membrane), sulfonated polyaryletherketone membrane (SPPEK membrane), polyaryletherketone membrane (PAEK membrane), polysulfone fiber membrane (PSF membrane), polyphthalazine etherketone membrane (PPEKK membrane) , sulfonated polyethersulfone diaphragm (SPES diaphragm), tetrafluoroethylene diaphragm (ETFE diaphragm), polystyrene diaphragm (PS diaphragm), polyethylene diaphragm (PE diaphragm), polystyrene diaphragm (PP diaphragm), polybenzimidazole diaphragm (PBI diaphragm), sulfonated polyarylether diaphragm, polyparaphenylene diaphragm, sulfonated polydiallyl bisphenol ether ketone diaphragm, polyfluorenyl ether ketone sulfone diaphragm, polyfluorenyl ether diaphragm, polyvinyl chloride acylation diaphragm, polyphenyl ether diaphragm or polyphenyl diaphragm and other ion exchange membranes, porous membranes and ceramic membranes.
[0058] Treatment of ion exchange membrane: The ion exchange membrane is heated at a constant temperature using any alkaline solution of LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO3, Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O. The heating temperature is 40~100℃ and the heating time is 0.5h~8h. After the ionization process is completed, it is washed with deionized water and immersed in deionized water to obtain K + 、Na + , Li + or NH4 + The ion exchange membrane is prepared by immersing it in LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl, NH4Br or (NH4)2SO4 solution for use. If the alkali solution is Li2O, Na2O or K2O, the prepared membranes are Li + 、Na + , K + Type diaphragm.
[0059] The porous membrane and the ceramic membrane do not need to be processed as described above and can be directly used in the liquid flow battery system of the embodiment of the present invention.
[0060] The electrode is any one of carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode. The electrode material with high catalytic activity (modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode) realizes the rapid reaction of polysulfide and can effectively increase the energy efficiency and power density of the battery. The basic principle is based on the problem of low electrical conductivity and few reaction active sites of carbon felt electrode materials. The prepared modified electrode effectively increases the electrical conductivity of the electrode on the one hand, and on the other hand, effectively loads sulfide on the original carbon felt, which can effectively increase the reaction active sites of polysulfide ions and ultimately accelerate the reaction rate of the active substance.
[0061] The positive electrode active material is ferrocyanide or ferrocyanide ion, and in some embodiments, it is two or more of potassium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, sodium ferrocyanide, ammonium ferrocyanide, ammonium ferrocyanide, lithium ferrocyanide or lithium ferrocyanide (mixed in a molar ratio of 1:). The concentration of the configured iron compound is related to the type, proportion and quantity of the corresponding compound and supporting electrolyte, and the concentration of the configured positive electrode side active material is 0.1M~1.7M.
[0062] The negative electrode active material is a highly water-soluble sulfide solution or a sulfur-containing organic compound.
[0063] The concentration range of the negative electrode active material in the negative electrode electrolyte is 0.1M~15M. Polysulfide is a highly water-soluble substance. The concentration range set in the embodiment of the present invention is because the inherent solubility of polysulfide is within this range. In addition, a higher concentration of polysulfide cannot be used for conventional iron-sulfur liquid flow batteries because the higher shuttle effect of polysulfide will reduce the cycle life of the battery. When the polysulfide is at a higher concentration, this effect will be more serious.
[0064] The highest concentration of polysulfide used in general iron-sulfur flow batteries is only 2.0M K2S, which means that the battery cannot construct a battery system with high energy density on both sides. The present invention constructs an alkaline iron-sulfur flow battery system with high energy density on both sides, and at the same time has a longer cycle life than general iron-sulfur flow batteries. On the one hand, ferrocyanide / ferrocyanide with higher solubility was successfully developed under alkaline conditions, and a high volume capacity design was achieved on the positive electrode side. On the other hand, an ion adjustment strategy was designed to successfully reduce the shuttle effect of polysulfide and extend the cycle life of the battery. In addition, high-performance diaphragms and electrode materials with high catalytic activity are further used. Highly ion-selective diaphragms can further help inhibit the shuttle effect of polysulfide, while electrode materials can enhance the reaction activity of polysulfide ions and improve the adsorption performance of polysulfide ions, and reduce the shuttle effect of polysulfide ions. Therefore, the alkaline iron-sulfur flow battery in the present invention has higher energy density, longer cycle life and lower chemical cost than previous iron-sulfur flow batteries.
[0065] The sulfide solution is a mixture of one or more of potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, mercaptan, thiophenol or thioether in any mass ratio. The polysulfide ion S with variable valence is used in the actual reaction process. X (X=1, 2, 3, 4, 5, 6, 7, 8).
[0066] The supporting electrolytes in the positive and negative electrolytes are LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO 3、 One or more of Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O, with a total molar concentration of 0.1M~6M.
[0067] Li2O, Na2O or K2O as supporting electrolytes provide an alkaline environment to ensure the solubility of ferrocyanide / ferrocyanide at the positive electrode. On the other hand, they ensure the ionic conductivity of the solution and ensure that the corresponding ions can be stably conducted under the corresponding cationic ion exchange membrane.
[0068] When two supporting electrolytes are used for both the positive and negative electrodes, the total molar concentration is 0.1M~6M, and the molar ratio is in the range of 1 / 6~6 / 1, especially in the range of 1 / 2~6 / 1. When three supporting electrolytes are used for the positive and negative electrodes, the sum of the total concentrations is 0.5M~5.0M, and the molar ratio is in the range of 1:1:1~6:3:1. When four supporting electrolytes are used for the positive and negative electrodes, the sum of the total concentrations is 0.5M~4.0M, and the molar ratio is in the range of 1:1:1:1~6:1:1:1.
[0069] When the cation of the supporting electrolyte in the negative electrode electrolyte is one, the cation is one of the cations of the supporting electrolyte in the positive electrode electrolyte, that is, no matter how many supporting electrolytes there are in the positive and negative electrodes, it is necessary to ensure that the supporting electrolytes have a common cation. When the battery is in a cycle test, when the cations of the positive and negative electrode electrolytes or active substances are inconsistent. Because it is a specific cation or anion exchange membrane, cations different from the diaphragm will gradually clog the diaphragm, increasing the polarization of the battery and ultimately affecting the cycle stability of the battery.
[0070] The shuttling effect of polysulfides is an inherent problem, and this problem is more serious at high concentrations. How to solve the shuttling effect of polysulfides and further improve the cycle stability of iron-sulfur liquid flow battery systems is a current technical challenge. The present invention supports the cations in the electrolyte, polysulfides and auxiliary ions to remain consistent, which is used to reduce the shuttling effect of polysulfides.
[0071] Polysulfides are easily oxidized during the battery cycle, generating elemental sulfur precipitation, which affects the performance of the battery. The embodiment of the present invention uses potassium polysulfide, and the use of a solution containing potassium ions is better for battery performance. On the one hand, the cations of the supporting electrolyte and the active substance remain consistent, which can reduce the polarization of the battery during the cycle and extend the service life of the battery. On the other hand, in order to construct a bilateral high-energy-density iron-sulfur liquid flow battery system, a high concentration of potassium polysulfide is required on the negative electrode side, but the high concentration of potassium polysulfide has a strong shuttle effect, which affects the cycle performance of the battery. Adding a solution containing potassium ions as a supporting electrolyte can enhance the potassium ion conductivity of the solution and reduce the shuttling of polysulfide ions and their oxidation.
[0072] A method for preparing a high energy density alkaline iron-sulfur liquid flow battery system comprises the following steps:
[0073] (1) Use deionized water to prepare LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO 3、 Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Ca(OH)2, Li2O, Na2O, K2O, one or more alkaline solutions;
[0074] (2) Use perfluorosulfonic acid membrane (Nafion membrane), sulfonated polyetheretherketone membrane (SPEEK membrane), sulfonated polyimide membrane (SPI membrane), sulfonated polyfluorene ether ketone membrane (SPFEK membrane), polyvinylidene fluoride membrane (PVDF membrane), polyethersulfone membrane (PES membrane), sulfonated polyaryletherketone membrane (SPPEK membrane), polyaryletherketone membrane (PAEK membrane), polysulfone fiber membrane (PSF membrane), polyphthalazine etherketone membrane (PP EKK diaphragm), sulfonated polyethersulfone diaphragm (SPES diaphragm), tetrafluoroethylene diaphragm (ETFE diaphragm), polystyrene diaphragm (PS diaphragm), polyethylene diaphragm (PE diaphragm), polyphenylene diaphragm (PP diaphragm), polybenzimidazole diaphragm (PBI diaphragm), sulfonated polyarylether diaphragm, polyparaphenylene diaphragm, sulfonated polydiallyl bisphenol ether ketone diaphragm, polyfluorenyl ether ketone sulfone diaphragm, polyfluorenyl ether diaphragm, polyvinyl chloride acylation diaphragm, polyphenyl ether diaphragm or polyphenyl diaphragm, etc. as diaphragm;
[0075] (3) The membrane in step (2) includes an ion exchange membrane, a porous membrane and a ceramic membrane, which illustrates the wide applicability of the system of the present invention to the membrane. The ion exchange membrane is ionized according to the following steps: the ion exchange membrane is subjected to a constant temperature heating treatment in the alkaline solution (0.1M~6.0M) of step (1), and the heating time is 0.5~8h at 40~100℃. The purpose of the ionization treatment is to improve the ion conductivity of the membrane and transform the membrane into a specific ion exchange type membrane; the non-ion exchange membrane can be directly used in the liquid flow battery of this system;
[0076] (4) The specific ion exchange membrane converted in step (3) is repeatedly washed with deionized water until the aqueous solution in which the membrane is finally immersed is neutral, and then immersed in a 0.1M~2.0M LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4 solution for standby use;
[0077] (5) Carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode as battery electrode materials;
[0078] (6) taking potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, mercaptan, thiophenol, thioether and other sulfide solutions and sulfur-containing organic compounds, dissolving them in the alkaline solution prepared in the above step (1) to obtain an alkaline solution of sulfides;
[0079] (7) dissolving one or more of potassium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, sodium ferrocyanide, ammonium ferrocyanide, ammonium ferrocyanide, lithium ferrocyanide or lithium ferrocyanide in the alkaline solution prepared in step (1) above to prepare an alkaline solution of ferrocyanide / ferrocyanide;
[0080] (8) In order to construct the cycle stability of the positive and negative active materials regulated by the same ions, based on the solutions prepared in step (6) and step (7), 0.1M~2.0M regulating ions are LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4, or a plurality of solutions thereof, and the solution is fully stirred and dissolved using a magnetic stirrer, and finally used as the positive and negative electrolytes of the battery; the concentration added is continuously determined through experiments, including the specific type, quantity and corresponding proportion. If it exceeds the range, since the active material and the supporting electrolyte, as well as the above-mentioned substances added are all water-soluble, in terms of the positive and negative solutions requiring high volume capacity, the concentration of the other substances cannot be too high while ensuring a high concentration of the active material. Therefore, under the premise of ensuring the volume capacity, the concentration of the other substances cannot be too high.
[0081] (9) Assemble the electrolytes and key materials prepared in steps (3), (4), (5), (6), (7), and (8) into an alkaline redox flow battery, and test it using a battery testing system such as Newway, Blue Power, and Arbin.
[0082] Embodiment 1,
[0083] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L KOH; the negative electrode active material is 1.0 mol / L K2S, and the supporting electrolyte is 0.5 mol / L KOH; the diaphragm is a modified Nafion conductive K + Diaphragm; carbon felt is used for both positive and negative electrode materials. Among them, modified Nafion conducts K +Preparation of diaphragm: The ion exchange membrane was heated at a constant temperature of 40°C and a heating time of 8 h by using 0.1 M KOH. After the ionization process was completed, it was washed with deionized water and soaked in deionized water to obtain K + type ion exchange membrane, and finally immersed in a 0.1 M KCl solution for standby use.
[0084] The alkaline iron-sulfur flow battery of Example 1 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Figure 1 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.6%, the average voltage efficiency is 64.4%, and the average energy efficiency is 64.1%.
[0085] Embodiment 2,
[0086] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L KOH; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is 0.5 mol / L KOH, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified Nafion conductive K + Diaphragm; carbon felt is used for both positive and negative electrode materials. Among them, modified Nafion conducts K + Preparation of diaphragm: The ion exchange membrane was heated at a constant temperature of 60°C and a heating time of 3 h by using 6.0 M KOH. After the ionization process was completed, it was washed with deionized water and soaked in deionized water to obtain K + type ion exchange membrane, and finally immersed in a 2.0 M KCl solution for standby use.
[0087] The alkaline iron-sulfur flow battery of Example 2 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Figure 5 As shown, the average coulombic efficiency of the flow battery system in this embodiment is 98.8%, the average voltage efficiency is 82.5%, and the average energy efficiency is 83.5%. Compared with Example 1, it can be seen that the battery using the regulating ion under the same conditions is more efficient.
[0088] Embodiment 3,
[0089] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L KOH; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is 0.5 mol / L KOH, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified Nafion conductive K + The positive electrode material uses carbon felt, and the negative electrode material uses modified nickel mesh. Among them, the modified Nafion conducts K + Preparation of diaphragm: The ion exchange membrane was heated at a constant temperature of 100°C and a heating time of 0.5 h by using 2.0 M KOH. After the ionization process was completed, it was washed with deionized water and soaked in deionized water to obtain K + type ion exchange membrane, and finally immersed in a 1.0 M KCl solution for standby use.
[0090] The alkaline iron-sulfur flow battery of Example 3 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Figures 2~4 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.7%, the average voltage efficiency is 85.1%, and the average energy efficiency is 85.4%.
[0091] Comparison between Example 1 and Example 2 shows that the addition of auxiliary ions improves the battery performance. Comparison between Example 2 and Example 3 shows that the battery performance is further improved after the modified nickel mesh is used.
[0092] Embodiment 4,
[0093] A high energy density alkaline iron-sulfur liquid flow battery: the liquid flow battery positive electrode active material is 0.25 mol / L K4Fe(CN)6 and 0.25 mol / L Na4Fe(CN)6, the supporting electrolyte is KOH and NaOH, the molar ratio is 1:1, and the total molar concentration is 6.0 mol / L; the negative electrode active material is 2.0 mol / L K2S, the supporting electrolyte is 6.0 mol / L KOH, and 0.1 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm uses a porous diaphragm; the positive electrode material uses carbon felt, and the negative electrode material uses a modified nickel mesh.
[0094] The alkaline iron-sulfur flow battery of Example 4 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Figure 6 As shown, the average coulombic efficiency of the flow battery system in this embodiment is 98.3%, the average voltage efficiency is 87.8%, and the average energy efficiency is 88.4%. The above data show that the use of the porous membrane will not affect the cycle stability of the battery, indicating the wide adaptability of the system of the present invention to the use of the diaphragm.
[0095] Embodiment 5,
[0096] A high energy density alkaline iron-sulfur flow battery: The positive electrode active material of the flow battery is 0.85 mol / L K4Fe(CN)6 and 0.85 mol / L Na4Fe(CN)6, that is, the ferrocyanide ion concentration is 1.7M; the supporting electrolyte on the positive electrode side is KOH and NaOH, the molar ratio is 1:6, and the total concentration is 0.1 mol / L. The negative electrode active material is 2.0 mol / L K2S, the supporting electrolyte is KOH and NaOH, the molar ratio is 6:1, the total concentration is 2.0 mol / L, and 2.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0097] The alkaline iron-sulfur flow battery of Example 5 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Figure 7 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.7%, the average voltage efficiency is 85.0%, and the average energy efficiency is 85.3%.
[0098] The present invention successfully increases the concentration of ferrocyanide / ferrocyanide on the positive electrode side to 1.7M, which means that the volume capacity of the positive electrode side is 45.56Ah / L, while for a single concentration of potassium ferrocyanide, the solubility in pure water is 0.76M, i.e. 20.37Ah / L, which means that under more difficult to dissolve conditions, the volume capacity of the iron compound constructed by the embodiment of the present invention is more than twice that of the conventional one. At the same time, the auxiliary ion regulation strategy further constructed by the present invention enhances the cycle stability of the iron-sulfur liquid flow battery, allowing the battery to remain stable for an extremely long time, and the service life far exceeds the conventional iron-sulfur battery system.
[0099] Embodiment 6,
[0100] A high energy density alkaline iron-sulfur flow battery: The positive electrode active material of the flow battery uses 0.74 mol / L K4Fe(CN)6 and 0.74 mol / L Na4Fe(CN)6, that is, the ferrocyanide ion concentration is 1.48M; the supporting electrolyte on the positive electrode side is 0.5 mol / L KOH. The negative electrode active material is 15.0 mol / L K2S, the supporting electrolyte on the negative electrode side is 0.5 mol / L KOH, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm uses modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0101] The alkaline iron-sulfur flow battery of Example 6 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.3 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Figure 8 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 98.9%, the average voltage efficiency is 69.3%, the average energy efficiency is 70.1%, and both the positive and negative electrodes are tested using high-concentration active materials, showing high volume capacity characteristics.
[0102] When the polysulfide concentration is higher, the reaction rate on the electrode will not be able to proceed in time due to the increase in its own concentration, and the viscosity of the electrolyte will increase, and the time from the liquid storage tank to the electrode will also be extended. The present invention solves the problem of poor battery cycle stability caused by the shuttle effect of polysulfide at high concentrations and improves the stability of the battery system.
[0103] Embodiment 7,
[0104] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery adopts 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, the supporting electrolyte is LiOH, KOH and NaOH, the molar ratio is maintained in the range of 1:1:1-6:3:1, and the total concentration is 2.0 M; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is 0.5 mol / L KOH, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm adopts modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0105] The alkaline iron-sulfur flow battery of Example 7 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig. 9 As shown, in this embodiment, when the molar ratio of LiOH, KOH and NaOH is 1:2:2, the average energy efficiency of the system is 88.45%.
[0106] Embodiment 8,
[0107] A high energy density alkaline iron-sulfur flow battery: the flow battery stack system consists of 9 single cells, the positive electrode active material is 20L of 0.1mol / L K4Fe(CN)6 and 0.1mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L KOH; the negative electrode active material is 40L of 1.0mol / L K2S, the supporting electrolyte is 0.5mol / L KOH, and 1.0mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified Nafion conductive K + Diaphragm; the positive and negative electrode materials are both made of carbon felt.
[0108] The alkaline iron-sulfur liquid flow battery of Example 8 was subjected to a constant current charge-discharge cycle performance test, with a charge cut-off voltage of 11.7 V, a discharge cut-off voltage of 4.5 V, and a current density of 20 mA / cm 2 ;like Fig.10 As shown, the average coulombic efficiency of the flow battery system in this embodiment is 99.4%, the average voltage efficiency is 85.8%, and the average energy efficiency is 86.3%. Example 8 confirms the feasibility of using the battery stack in actual energy storage in the system of the present invention, providing a basis for subsequent practical applications.
[0109] Embodiment 9,
[0110] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.85 mol / L K4Fe(CN)6 and 0.85 mol / L Na4Fe(CN)6, and the supporting electrolyte is 0.5 mol / L KOH; the negative electrode active material is 2.0 mol / L K2S, and the supporting electrolyte is 0.5 mol / L KOH; and 1.0 M of KCl As the regulating ions of positive and negative electrodes; the diaphragm adopts modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and MoS2 modified electrode is used as the negative electrode material.
[0111] The alkaline iron-sulfur flow battery of Example 9 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Fig.11 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.1%, the average voltage efficiency is 88.0%, and the average energy efficiency is 88.7%.
[0112] MoS2 is a typical transition metal disulfide and a graphite-like two-dimensional layered material. When it grows on the surface of a carbon material matrix, it retains the excellent properties of a two-dimensional structure in the form of a nanosheet structure. MoS2 has two main phase structures, namely 2H phase (2H- MoS2) and 1T phase (1T- MoS2). Nanostructured MoS2 has a larger specific surface area, stronger adsorption capacity and better catalytic performance. In addition, MoS2 has a wider interlayer spacing, which can provide channels for electron transfer and active material transport. The growth of MoS2 on pristine carbon felt can accelerate the reaction kinetics of polysulfide. On the one hand, it is due to the catalytic activity of MoS2, which is mainly manifested in promoting the reaction rate of polysulfide on the electrode and reducing the overpotential and reaction energy barrier of the reaction; on the other hand, the unique layered structure of MoS2 can provide channels for the transport of active substances.
[0113] Embodiment 10,
[0114] A high energy density alkaline iron-sulfur liquid flow battery: the positive electrode active material of the liquid flow battery is 0.1 mol / L K3Fe(CN)6, and the supporting electrolyte is 0.1 mol / L Na2O; the negative electrode active material is 0.1 mol / L K2S, the supporting electrolyte is 0.1 mol / L Na2O, and 1.0 mol / L KBr or K2SO4 is added as auxiliary ions to adjust the positive and negative electrolytes; the diaphragm is a ceramic membrane; the positive electrode material uses carbon felt, and the negative electrode material uses a CuS modified electrode.
[0115] The alkaline iron-sulfur flow battery of Example 10 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Fig.12 As shown, the average voltage efficiency of the liquid flow battery system in this embodiment is 86.8%, and the average energy efficiency is 85.6%.
[0116] Embodiment 11,
[0117] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, the supporting electrolyte is LiOH, KOH and NaOH, the molar ratio is 1:2:2, and the total concentration is 0.5M; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is LiOH, KOH and NaOH, the molar ratio is 1:2:2, and the total concentration is 0.5M, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0118] The alkaline iron-sulfur flow battery of Example 11 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig.13 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.6%, the average voltage efficiency is 84.8%, and the average energy efficiency is 85.2%.
[0119] Embodiment 12,
[0120] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, the supporting electrolyte is LiOH, KOH and NaOH, the molar ratio is 1:2:2, and the total concentration is 5.0 M; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is LiOH, KOH and NaOH, the molar ratio is 1:2:2, and the total concentration is 5.0 M, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0121] The alkaline iron-sulfur flow battery of Example 12 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig.14 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.8%, the average voltage efficiency is 86.0%, and the average energy efficiency is 86.1%.
[0122] Embodiment 13,
[0123] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery adopts 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, the supporting electrolyte is LiOH, NaOH, KOH, NH3·H2O, the molar ratio is 1:1:1:1, and the total concentration is 0.5M; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is LiOH, NaOH, KOH, NH3·H2O, the molar ratio is 1:2:1:2, the total concentration is 4.0M, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm adopts modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0124] The alkaline iron-sulfur flow battery of Example 13 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig.15 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.3%, the average voltage efficiency is 85.1%, and the average energy efficiency is 85.7%.
[0125] Embodiment 14,
[0126] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery adopts 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, the supporting electrolyte is LiOH, NaOH, KOH, NH3·H2O, the molar ratio is 6:1:1:1, and the total concentration is 2.0 M; the negative electrode active material is 1.0 mol / L K2S, the supporting electrolyte is LiOH, NaOH, KOH, NH3·H2O, the molar ratio is 6:1:1:1, and the total concentration is 2.0 M, and 1.0 mol / L KCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm adopts modified Nafion conductive K + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0127] The alkaline iron-sulfur flow battery of Example 14 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig.16As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.3%, the average voltage efficiency is 84.2%, and the average energy efficiency is 85.8%.
[0128] Embodiment 15,
[0129] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L Li4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 2.0M LiHCO3; the negative electrode active material is 1.0 mol / L lithium polysulfide, the supporting electrolyte is 2.0M Li2HCO3, and 1.0 mol / L LiI is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified SPEEK diaphragm to conduct Li + Diaphragm; carbon felt is used as the positive electrode material, and SnS2 modified electrode is used as the negative electrode material.
[0130] The alkaline iron-sulfur flow battery of Example 15 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 ,like Fig.17 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.4%, the average voltage efficiency is 85.1%, and the average energy efficiency is 85.6%.
[0131] Embodiment 16,
[0132] A high energy density alkaline iron-sulfur flow battery: the positive electrode active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L NaOH; the negative electrode active material is 1.0 mol / L Na2S2, the supporting electrolyte is 0.5 mol / L NaOH, and 1.0 mol / L NaCl is added as an auxiliary ion to adjust the positive and negative electrolytes; the diaphragm is a modified Nafion conductive Na + Diaphragm; carbon felt is used as the positive electrode material, and modified nickel mesh is used as the negative electrode material.
[0133] The alkaline iron-sulfur flow battery of Example 16 was subjected to a constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.2 V, the discharge cut-off voltage was 0.6 V, and the current density was 20 mA / cm 2 ,like Fig.18 As shown, the average coulombic efficiency of the liquid flow battery system in this embodiment is 99.3%, the average voltage efficiency is 84.2%, and the average energy efficiency is 84.8%.
[0134] The embodiment of the present invention constructs a strategy for regulating the stability of active substances by similar ions. The diaphragm is immersed in a related solution, laying the foundation for the subsequent construction of a strategy for regulating the stability of active substances by similar ions. Similar ions are added to regulate the stability of active substances; at the same time, the type, quantity and proportion of auxiliary ions are adjusted. On the one hand, it is used to regulate the solubility of ferrocyanide / ferrocyanide on the positive electrode side, and on the other hand, it is used to stabilize polysulfides, achieve a lower shuttle effect of polysulfide ions, and finally build a battery system with long-term stable operation. By constructing a strategy in which auxiliary ions and active material cations are consistent, the present invention successfully suppresses the shuttle effect of polysulfides and greatly improves the solubility of ferrocyanide / ferrocyanide, thereby constructing a high energy density and long cycle life alkaline flow battery system.
[0135] Comparative Example 1,
[0136] The positive active material of the flow battery is 0.1 mol / L K4Fe(CN)6 and 0.1 mol / L Na4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L NaOH; the negative active material is 1.0 mol / L K2S, and the supporting electrolyte is 0.5 mol / L NaOH; the diaphragm is a modified Nafion conductive Na + Diaphragm; carbon felt is used for both positive and negative electrode materials.
[0137] The alkaline iron-sulfur flow battery of Example 1 was subjected to constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.3 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 .like Fig.19 As shown, the battery in this comparative example has a high internal resistance and a large polarization, and the battery cannot cycle normally. On the one hand, since the negative electrode uses carbon felt, the low catalytic reaction rate of polysulfides is a key influencing factor that limits the overall reaction rate of the battery. The reaction kinetics of carbon felt on polysulfides cannot achieve a relatively fast effect, resulting in a relatively large polarization of the battery during the battery cycle. At the same time, due to the difference between the cations of the negative electrode supporting electrolyte and the active substance in this embodiment, this will cause the continuous accumulation of sodium ions on the diaphragm during the battery cycle. The diaphragm uses a potassium ion conductive diaphragm, resulting in a relatively large polarization of the battery.
[0138] Comparative Example 2,
[0139] The positive electrode electrolyte is 1.0 mol / L K4Fe(CN)6, and the supporting electrolyte is NaCl; the negative electrode electrolyte is 1.0 mol / L Na2S2, and the supporting electrolyte is NaCl. For details, see the literature (Journal of The Electrochemical Society, 163, A5150-A5153, 2016). The diaphragm is made of modified Nafion conductive K + Diaphragm; carbon felt is used for both positive and negative electrode materials.
[0140] The flow rate of the positive electrolyte and the negative electrolyte of Comparative Example 2 is 20 mL / min, the charge cut-off voltage is 1.3 V, the discharge cut-off voltage is 0.4 V, and the current density is 20 mA / cm 2 It is difficult for the battery to achieve long-term stable cycling. This is because the auxiliary ions are inconsistent with the cations of the active substances, and the conductivity at the diaphragm is inconsistent, resulting in the continuous accumulation of ions at the diaphragm, causing the polarization of the battery to continue to increase during the cycle, and ultimately making the battery's cycle stability worse, making it difficult to achieve long-term operation.
[0141] Comparative Example 3,
[0142] The positive electrode electrolyte is 0.4 mol / L K4Fe(CN)6, and the supporting electrolyte is 1.0 mol / L KOH; the negative electrode active material is 1.0 mol / L K2S, and the supporting electrolyte is 0.5 mol / L KOH; the diaphragm is a modified Nafion conductive K + Separator; carbon felt is used as the positive electrode, and modified nickel mesh is used as the negative electrode.
[0143] The alkaline iron-sulfur flow battery of comparative example 3 was subjected to constant current charge-discharge cycle performance test. The flow rates of the positive and negative electrolytes were both 20 mL / min, the charge cut-off voltage was 1.3 V, the discharge cut-off voltage was 0.4 V, and the current density was 20 mA / cm 2 .like Fig. 20 As shown, the battery in this comparative example can operate, but due to the low concentration of potassium ferrocyanide on the positive electrode side, the volume capacity is low. In practical applications, iron-sulfur flow batteries are limited by the low solubility of ferrocyanide / ferrocyanide on the positive electrode side. In many literatures, the solubility of ferrocyanide / ferrocyanide is only 0.4M (for example: Science, 349, 1529-1532, 2015; Nature Energy, 1, 16102, 2016; Advanced Energy Materials, 9,1900039, 2019), which is obviously difficult to meet actual needs.
[0144] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A high energy density alkaline iron-sulfur flow battery, comprising a positive electrolyte, a negative electrolyte, a separator, and positive and negative electrodes, characterized in that: The active substance in the positive electrode electrolyte is ferrocyanide or ferrocyanide ion, and the concentration of the active substance on the positive electrode side is 0.1M to 1.7M; The active material in the negative electrode electrolyte is a sulfide solution, and the concentration range of the negative electrode active material is 0.1M to 15M; The supporting electrolytes in the positive and negative electrolytes are LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO with a molar concentration of 0.1M to 6M. 3、 One or more of Li2CO3, LiHCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O; no matter how many supporting electrolytes are present at the positive and negative electrodes, it is necessary to ensure that the supporting electrolytes at the positive and negative electrodes have a common cation; The diaphragm is any one of a porous membrane, a ceramic membrane or an ion exchange membrane that has been ionized; The concentration range of the regulating ions in the positive and negative electrode electrolytes is 0.1M to 2.0M, and the regulating ions are the same as the cations of the negative electrode active material and the supporting electrolyte; Among them, the preparation of the negative electrode electrolyte: take potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, thiol, thiophenol or thioether, dissolve in an alkaline solution to obtain an alkaline solution of sulfide; then add 0.1M to 2.0M of regulating ions, the regulating ions are any one of LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4 or a mixture of multiple solutions, and use a magnetic stirrer to fully stir and dissolve; Preparation of positive electrode electrolyte: dissolve one or more of potassium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, sodium ferrocyanide, ammonium ferrocyanide, ammonium ferrocyanide, lithium ferrocyanide or lithium ferrocyanide in an alkaline solution to prepare an alkaline solution of ferrocyanide / ferrocyanide; then add 0.1M to 2.0M of regulating ions, wherein the regulating ions are any one of LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl or (NH4)2SO4, or a mixture of multiple solutions, and stir and dissolve them thoroughly using a magnetic stirrer; The alkaline solution in the preparation of the negative electrode electrolyte and the preparation of the positive electrode electrolyte is a supporting electrolyte, and the preparation method is: using deionized water to prepare LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO 3、 One or more alkaline solutions of Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O.
2. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: The positive and negative electrodes are any one of carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode.
3. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: The ion exchange membrane is any one of a perfluorosulfonic acid membrane, a sulfonated polyetheretherketone membrane, a sulfonated polyimide membrane, a sulfonated polyfluorene ether ketone membrane, a polyvinylidene fluoride membrane, a polyethersulfone membrane, a sulfonated polyaryletherketone membrane, a polyaryletherketone membrane, a polysulfone fiber membrane, a polyphthalazine etherketone membrane, a sulfonated polyethersulfone membrane, a tetrafluoroethylene membrane, a polystyrene membrane, a polyethylene membrane, a polyphenylene membrane, a polybenzimidazole membrane, a sulfonated polyarylether membrane, a polyparaphenylene membrane, a sulfonated polydiallyl bisphenol ether ketone membrane, a polyfluorene ether ketone sulfone membrane, a polyfluorene ether membrane, a polyvinyl chloride acylation membrane, a polyphenylene ether membrane or a polyphenyl membrane.
4. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: The sulfide solution is a mixture of one or more of potassium sulfide, potassium polysulfide, sodium sulfide, sodium polysulfide, lithium sulfide, lithium polysulfide, calcium sulfide, calcium polysulfide, rubidium sulfide, cesium sulfide, aluminum sulfide, magnesium sulfide, zinc sulfide, benzenesulfonic acid, mercaptan, thiophenol or thioether in any mass ratio.
5. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: When there are two types of supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.1M to 6M, and the molar ratio of the two supporting electrolytes is in the range of 1 / 6 to 6 / 1.
6. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: When there are three types of supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.5M to 5.0M, and the molar ratio of the three supporting electrolytes is in the range of 1:1:1 to 6:3:
1.
7. A high energy density alkaline iron-sulfur flow battery according to claim 1, characterized in that: When there are four supporting electrolytes in the positive and negative electrode electrolytes, the total molar concentration is 0.5M to 4.0M, and the molar ratio of the four supporting electrolytes is in the range of 1:1:1:1 to 6:1:1:
1.
8. A method for preparing a high energy density alkaline iron-sulfur flow battery as claimed in claim 1, characterized in that: The following steps are included: Preparation of the diaphragm: the diaphragm is any one of an ion exchange membrane, a porous membrane or a ceramic membrane; when the diaphragm is an ion exchange membrane, an ionization treatment is performed; Preparation of electrodes: using carbon cloth, carbon paper, carbon felt, graphite felt, graphite plate, graphene-modified carbon felt, graphyne-modified carbon felt, nickel mesh, modified nickel mesh, CuS2-modified electrode, CuS-modified electrode, MoS2-modified electrode, CoS2-modified electrode, CoS-modified electrode, NiS-modified electrode, PbS-modified electrode, SnS2-modified electrode, VS2-modified electrode, WS2-modified electrode or FeS2-modified electrode as electrode materials for batteries; Preparation of negative electrode electrolyte; Preparation of positive electrode electrolyte; The prepared positive and negative electrolytes, separators, positive and negative electrodes are assembled into an alkaline redox flow battery.
9. The method for preparing a high energy density alkaline iron-sulfur liquid flow battery according to claim 8, characterized in that: In the preparation of the diaphragm, the ion exchange membrane is ionized by: the ion exchange membrane is heated at a constant temperature by any alkaline solution of LiOH, NaOH, KOH, NH3·H2O, NH4HCO3, (NH4)2CO3, Li2CO3, Li2HCO3, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2O, Na2O or K2O with a concentration of 0.1M to 6.0M, the heating temperature is 40 to 100°C, the heating time is 0.5h to 8h, and after the ionization process is completed, it is washed with deionized water and immersed in deionized water to obtain K + 、Na + , Li + or NH4 + type ion exchange membrane, and finally immersed in a 0.1M to 2.0M LiCl, KCl, NaCl, LiBr, KBr, NaBr, LiI, KI, NaI, Li2SO4, LiNO3, K2SO4, KNO3, Na2SO4, NaNO3, NH4Cl, NH4Br or (NH4)2SO4 solution for standby use.