Tin-copper-antimony lead-free solder and preparation method thereof

By introducing nano-Al and nano-Ni particles into the tin-copper-antimony lead-free solder and adopting a specific preparation method, the problems of re-fracture and insufficient microhardness of the existing lead-free solder are solved, and the welding performance and working life are significantly improved. , forming solder joints with high microhardness and excellent mechanical properties.

CN115008061BActive Publication Date: 2024-10-01SHENZHEN YUHANG NEW METAL MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210681754.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-15
Publication Date
2024-10-01
Estimated Expiration
2042-06-15

AI Technical Summary

Technical Problem

Existing lead-free solder is prone to re-fracture after long-term use, and its microhardness is relatively average, so it cannot effectively replace the performance of traditional high-lead solder.

Method used

Tin-copper-antimony lead-free solder is used, and nano-Al particles and nano-Ni particles are introduced into it. Specific smelting and grinding methods are used to form a composite molten liquid of nano-particles. The temperature and cooling rate are adjusted to produce a product with high microhardness and excellent mechanics. Performance solder joints.

Benefits of technology

The microhardness is significantly increased, the solder joints are firmly bonded, the growth of the intermetallic compound layer at the interface is delayed, the welding performance and working life are improved, and the structural stability and mechanical properties of the tin-copper-antimony lead-free solder are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003696534120000111
    Figure BDA0003696534120000111
Patent Text Reader

Abstract

The invention relates to the technical field of solders and discloses a tin-copper-antimony lead-free solder, which is prepared from the following components by weight percentage: 0.5-1.5% Cu, 0.3-1.2% Sb, 0.02-0.04% Ni, 0.02-0.04% Al, 0.2-1.4% P, 0.1-0.6% Ce, and the balance is Sn. The tin-copper-antimony lead-free solder prepared by the invention not only has excellent welding performance, but also has uniform microstructure distribution after welding, high microhardness of solder joints, firm bonding, and excellent mechanical properties, thereby greatly improving its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solder, in particular to a tin-copper-antimony lead-free solder and a preparation method thereof. Background Art

[0002] Brazing filler refers to the filler added in or beside the gap between two materials (or parts) to achieve the combination of the two materials (or parts). Brazing filler refers to the filler material used to form the weld during brazing.

[0003] Lead-free solder (Pb-free solder) means that the chemical composition of the solder does not contain lead (Pb). The Rohs directive requires that the Pb content does not exceed 1000PPM, or 0.1%.

[0004] For example, the Chinese invention patent with the prior art publication number CN103934590B discloses a ZnAlMgIn high-temperature lead-free solder, which belongs to the technical field of lead-free solder manufacturing for primary electronic packaging in the microelectronics industry. The composition of the present invention (mass percentage): Al3.9-4.1%, Mg2.4-3.1%, In0.5-3.0%, or P0.05-1.0%, and the balance is Zn. The solder of the present invention is smelted by a molten salt protection method, with less alloy burn loss and uniform structure. The present invention proposes to add trace amounts of In and P elements on the basis of the Zn4Al3Mg near-eutectic alloy to reduce the melting point of the alloy and improve the oxidation resistance and wetting properties of the alloy. The solder of the present invention has low cost, does not contain toxic elements such as Pb, has good wettability, good mechanical properties, and meets the requirements for replacing traditional high-lead solder. However, its microhardness is relatively general, and after use, it is easy to cause re-fracture for a long time.

[0005] Based on this, we proposed a tin-copper-antimony lead-free solder, hoping to solve the shortcomings of the existing technology. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a tin-copper-antimony lead-free solder.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions:

[0008] A tin-copper-antimony lead-free solder is made of the following components by weight percentage: 0.5-1.5% Cu, 0.3-1.2% Sb, 0.02-0.04% Ni, 0.02-0.04% Al, 0.2-1.4% P, 0.1-0.6% Ce, and the balance is Sn.

[0009] As a further technical solution, the Ni used is nano Ni particles;

[0010] The Al used is nano Al particles.

[0011] As a further technical solution, the mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1.

[0012] As a further technical solution, the method for preparing nano Ni particles comprises the following steps:

[0013] (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution;

[0014] (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion;

[0015] (3) drying by rotary evaporation to obtain coated nickel oxide particles;

[0016] (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles;

[0017] (5) The coated nickel oxide fine particles are calcined under an inert atmosphere to obtain nano-Ni particles.

[0018] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 10-12%.

[0019] As a further technical solution, the nickel oxide particles and the polyvinyl alcohol solution are mixed in a mass ratio of 1:10-15.

[0020] As a further technical solution, the grinding method is:

[0021] Glycerin is used as a grinding aid;

[0022] Grinding is carried out according to the ball-to-material ratio of 10:1-2, and the grinding is divided into 3 stages;

[0023] In the first stage, the grinding temperature is 25-28°C, the grinding speed is 1000-1100r / min, and the grinding time is 30-40min;

[0024] In the second stage, the grinding temperature is 30-35°C, the grinding speed is 1500-1600r / min, and the grinding time is 30-40min;

[0025] In the third stage, the grinding temperature is 40-42°C, the grinding speed is 1800-2000r / min, and the grinding time is 30-40min.

[0026] As a further technical solution, the calcination temperature is 415-440°C.

[0027] A method for preparing a tin-copper-antimony lead-free solder comprises the following steps:

[0028] (1) except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid;

[0029] (2) Smelting under vacuum: Add the molten liquid of step (1) into a smelting device, evacuate the vacuum degree in the smelting device to 0.01-0.04 Pa, let it stand for 15-20 min, then introduce neon gas into the smelting device, and at the same time, increase the temperature in the smelting device to 500-580° C., add nano-Al particles, and keep the temperature for 3-5 min under high-frequency electromagnetic oscillation to obtain a composite molten liquid;

[0030] (3) adding the nano-Ni particles to the composite melt in step (2), adjusting the temperature to 520-550° C., and keeping the temperature under high-frequency electromagnetic oscillation for 3-5 min and 50-60 min;

[0031] (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

[0032] As a further technical solution, the cooling rate is 5-8°C / s.

[0033] The interfacial intermetallic compound (IMC) layer of the tin-copper-antimony lead-free solder joint prepared by the present invention can have a certain tendency to slow down its growth and thicken over time, thereby improving the bonding firmness of the solder joint. During the soldering process, the molten tin-copper-antimony lead-free solder reacts with the Cu, Ni and other pads to generate an interfacial IMC layer, thereby forming an effective metallurgical bond, thereby significantly improving the strength of the solder joint.

[0034] The present invention introduces nano-Al particles and nano-Ni particles into the tin-copper-antimony lead-free solder, thereby strengthening the strength of the solder joint, especially significantly improving the microhardness of the solder joint. At the same time, the reliability of the solder joint during service can be guaranteed, and the excessive growth of the interface IMC layer can be suppressed, thereby avoiding the increase of the brittleness of the solder joint caused by the excessive growth.

[0035] By adding nano-Al particles and nano-Ni particles in a specific mass ratio, the wettability of the tin-copper-antimony lead-free solder can be significantly improved, so that the molten tin-copper-antimony lead-free solder can spread faster and connect the welded parts together. Through the synergistic promotion of the two, the microstructure of the tin-copper-antimony lead-free solder can be significantly refined, the performance of the tin-copper-antimony lead-free solder can be significantly improved, and the organizational stability and mechanical properties of the tin-copper-antimony lead-free solder can be significantly improved.

[0036] By introducing nanoparticles of Ni and Al, the prepared tin-copper-antimony lead-free solder has increased wetting force, reduced wetting time, increased diffusion rate, and significantly improved wetting performance, thereby improving the spreading performance of the tin-copper-antimony lead-free solder.

[0037] Compared with the prior art, the present invention provides a tin-copper-antimony lead-free solder, which has the following beneficial effects:

[0038] The tin-copper-antimony lead-free solder prepared by the invention not only has excellent welding performance, but also has uniform tissue distribution after welding, high solder joint microhardness, firm bonding and excellent mechanical properties, thereby greatly improving its service life. DETAILED DESCRIPTION

[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0040] The following are specific embodiments:

[0041] Example 1

[0042] A tin-copper-antimony lead-free solder is made of the following components by weight percentage: 0.5% Cu, 0.3% Sb, 0.02% Ni, 0.02% Al, 0.2% P, 0.1% Ce, and the balance is Sn.

[0043] As a further technical solution, the Ni used is nano Ni particles;

[0044] The Al used is nano Al particles.

[0045] As a further technical solution, the mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1.

[0046] As a further technical solution, the method for preparing nano Ni particles comprises the following steps:

[0047] (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution;

[0048] (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion;

[0049] (3) drying by rotary evaporation to obtain coated nickel oxide particles;

[0050] (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles;

[0051] (5) The coated nickel oxide fine particles are calcined under an inert atmosphere to obtain nano-Ni particles.

[0052] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 10%.

[0053] As a further technical solution, the nickel oxide particles and the polyvinyl alcohol solution are mixed in a mass ratio of 1:10.

[0054] As a further technical solution, the grinding method is:

[0055] Glycerin is used as a grinding aid;

[0056] Grinding is carried out at a ball-to-material ratio of 10:1, and the grinding is divided into three stages;

[0057] In the first stage, the grinding temperature was 25 °C, the grinding speed was 1000 r / min, and the grinding time was 30 min;

[0058] In the second stage, the grinding temperature was 30°C, the grinding speed was 1500 r / min, and the grinding time was 30 min;

[0059] In the third stage, the grinding temperature is 40°C, the grinding speed is 1800r / min, and the grinding time is 30min.

[0060] As a further technical solution, the calcination temperature is 415°C.

[0061] A method for preparing a tin-copper-antimony lead-free solder comprises the following steps:

[0062] (1) except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid;

[0063] (2) Smelting under vacuum: Add the molten liquid of step (1) into a smelting device, evacuate the vacuum degree in the smelting device to 0.01 Pa, let it stand for 15 minutes, then introduce neon gas into the smelting device, and at the same time, increase the temperature in the smelting device to 500° C., add nano-Al particles, and keep the temperature for 3 minutes under high-frequency electromagnetic oscillation to obtain a composite molten liquid;

[0064] (3) adding the nano-Ni particles to the composite melt in step (2), adjusting the temperature to 520° C., and keeping the temperature under high-frequency electromagnetic oscillation for 3 min and 50 min;

[0065] (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

[0066] As a further technical solution, the cooling rate is 5°C / s.

[0067] Example 2

[0068] A tin-copper-antimony lead-free solder is made of the following components by weight percentage: 1.5% Cu, 1.2% Sb, 0.04% Ni, 0.04% Al, 1.4% P, 0.6% Ce, and the balance is Sn.

[0069] As a further technical solution, the Ni used is nano Ni particles;

[0070] The Al used is nano Al particles.

[0071] As a further technical solution, the mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1.

[0072] As a further technical solution, the method for preparing nano Ni particles comprises the following steps:

[0073] (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution;

[0074] (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion;

[0075] (3) drying by rotary evaporation to obtain coated nickel oxide particles;

[0076] (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles;

[0077] (5) The coated nickel oxide fine particles are calcined under an inert atmosphere to obtain nano-Ni particles.

[0078] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 12%.

[0079] As a further technical solution, the nickel oxide particles and the polyvinyl alcohol solution are mixed in a mass ratio of 1:15.

[0080] As a further technical solution, the grinding method is:

[0081] Glycerin is used as a grinding aid;

[0082] Grinding is carried out at a ball-to-material ratio of 10:2, and the grinding is divided into three stages;

[0083] In the first stage, the grinding temperature was 28 °C, the grinding speed was 1100 r / min, and the grinding time was 40 min;

[0084] In the second stage, the grinding temperature was 35 °C, the grinding speed was 1600 r / min, and the grinding time was 40 min;

[0085] In the third stage, the grinding temperature was 42°C, the grinding speed was 2000r / min, and the grinding time was 40min.

[0086] As a further technical solution, the calcination temperature is 440°C.

[0087] A method for preparing a tin-copper-antimony lead-free solder comprises the following steps:

[0088] (1) except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid;

[0089] (2) Smelting under vacuum: the molten liquid of step (1) is added into a smelting device, the vacuum degree in the smelting device is evacuated to 0.04 Pa, and the smelting device is allowed to stand for 20 min, and then neon gas is introduced into the smelting device. At the same time, the temperature in the smelting device is increased to 580° C., nano-Al particles are added, and the temperature is kept under high-frequency electromagnetic oscillation for 5 min to obtain a composite molten liquid;

[0090] (3) adding nano-Ni particles to the composite melt in step (2), adjusting the temperature to 550° C., and keeping the temperature under high-frequency electromagnetic oscillation for 5 min and 60 min;

[0091] (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

[0092] As a further technical solution, the cooling rate is 8°C / s.

[0093] Example 3

[0094] A tin-copper-antimony lead-free solder is made of the following components by weight percentage: 1.2% Cu, 0.8% Sb, 0.035% Ni, 0.035% Al, 0.9% P, 0.4% Ce, and the balance is Sn.

[0095] As a further technical solution, the Ni used is nano Ni particles;

[0096] The Al used is nano Al particles.

[0097] As a further technical solution, the mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1.

[0098] As a further technical solution, the method for preparing nano Ni particles comprises the following steps:

[0099] (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution;

[0100] (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion;

[0101] (3) drying by rotary evaporation to obtain coated nickel oxide particles;

[0102] (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles;

[0103] (5) The coated nickel oxide fine particles are calcined under an inert atmosphere to obtain nano-Ni particles.

[0104] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 10.5%.

[0105] As a further technical solution, the nickel oxide particles and the polyvinyl alcohol solution are mixed in a mass ratio of 1:12.

[0106] As a further technical solution, the grinding method is:

[0107] Glycerin is used as a grinding aid;

[0108] Grinding is carried out at a ball-to-material ratio of 10:1.2, and the grinding is divided into three stages;

[0109] In the first stage, the grinding temperature was 26 °C, the grinding speed was 1050 r / min, and the grinding time was 36 min;

[0110] In the second stage, the grinding temperature was 32 °C, the grinding speed was 1550 r / min, and the grinding time was 36 min;

[0111] In the third stage, the grinding temperature was 41°C, the grinding speed was 1900 r / min, and the grinding time was 36 min.

[0112] As a further technical solution, the calcination temperature is 420°C.

[0113] A method for preparing a tin-copper-antimony lead-free solder comprises the following steps:

[0114] (1) except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid;

[0115] (2) Smelting under vacuum: the molten liquid of step (1) is added into a smelting device, the vacuum degree in the smelting device is evacuated to 0.02 Pa, and the smelting device is allowed to stand for 16 min, and then neon gas is introduced into the smelting device. At the same time, the temperature in the smelting device is increased to 510° C., nano-Al particles are added, and the smelting device is kept warm for 4 min under high-frequency electromagnetic oscillation to obtain a composite molten liquid;

[0116] (3) adding the nano-Ni particles to the composite melt in step (2), adjusting the temperature to 530° C., and keeping the temperature under high-frequency electromagnetic oscillation for 4 min and 55 min;

[0117] (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

[0118] As a further technical solution, the cooling rate is 6°C / s.

[0119] Example 4

[0120] A tin-copper-antimony lead-free solder is made of the following components by weight percentage: 1.1% Cu, 0.6% Sb, 0.03% Ni, 0.03% Al, 0.7% P, 0.5% Ce, and the balance is Sn.

[0121] As a further technical solution, the Ni used is nano Ni particles;

[0122] The Al used is nano Al particles.

[0123] As a further technical solution, the mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1.

[0124] As a further technical solution, the method for preparing nano Ni particles comprises the following steps:

[0125] (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution;

[0126] (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion;

[0127] (3) drying by rotary evaporation to obtain coated nickel oxide particles;

[0128] (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles;

[0129] (5) The coated nickel oxide fine particles are calcined under an inert atmosphere to obtain nano-Ni particles.

[0130] As a further technical solution, the mass fraction of the polyvinyl alcohol solution is 11%.

[0131] As a further technical solution, the nickel oxide particles and the polyvinyl alcohol solution are mixed in a mass ratio of 1:14.

[0132] As a further technical solution, the grinding method is:

[0133] Glycerin is used as a grinding aid;

[0134] Grinding is carried out at a ball-to-material ratio of 10:1.5, and the grinding is divided into three stages;

[0135] In the first stage, the grinding temperature was 27 °C, the grinding speed was 1080 r / min, and the grinding time was 35 min;

[0136] In the second stage, the grinding temperature was 32°C, the grinding speed was 1530 r / min, and the grinding time was 35 min;

[0137] In the third stage, the grinding temperature was 41°C, the grinding speed was 1850 r / min, and the grinding time was 35 min.

[0138] As a further technical solution, the calcination temperature is 430°C.

[0139] A method for preparing a tin-copper-antimony lead-free solder comprises the following steps:

[0140] (1) except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid;

[0141] (2) Smelting under vacuum: the molten liquid of step (1) is added into a smelting device, the vacuum degree in the smelting device is evacuated to 0.03 Pa, and the smelting device is allowed to stand for 18 min, and then neon gas is introduced into the smelting device. At the same time, the temperature in the smelting device is increased to 530° C., nano-Al particles are added, and the temperature is kept for 4 min under high-frequency electromagnetic oscillation to obtain a composite molten liquid;

[0142] (3) adding nano-Ni particles to the composite melt in step (2), adjusting the temperature to 540° C., and keeping the temperature under high-frequency electromagnetic oscillation for 4 min and 58 min;

[0143] (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

[0144] As a further technical solution, the cooling rate is 7°C / s.

[0145] Comparative Example 1: The difference from Example 1 is that no nano-Al particles are added;

[0146] Comparative Example 2: The difference from Example 1 is that no nano Ni particles are added;

[0147] test:

[0148] The spreading performance of the embodiments and comparative examples was tested with reference to GB / T11364-1989;

[0149] Table 1

[0150] <![CDATA[Spreading area / mm 2 > Example 1 312.2 Example 2 308.6 Example 3 311.5 Example 4 310.7 Comparative Example 1 246.1 Comparative Example 2 258.5

[0151] It can be seen from Table 1 that the spreading area of ​​the tin-copper-antimony lead-free solder prepared by the present invention is greatly increased, thereby improving its welding performance.

[0152] The microhardness of the embodiments and comparative examples was tested according to GB / T11364-1989.

[0153] Table 2

[0154] Microhardness / HV Example 1 155.2 Example 2 153.8 Example 3 152.6 Example 4 155.9 Comparative Example 1 108.4 Comparative Example 2 136.7

[0155] It can be seen from Table 2 that the tin-copper-antimony lead-free solder prepared by the method of the present invention has excellent microhardness.

[0156] Further experiments were conducted, using Example 1 as the basic sample, to compare the effects of different mass ratios of nano-Al particles to nano-Ni particles on the microhardness of tin-copper-antimony lead-free solder;

[0157] Table 3

[0158]

[0159] It can be seen from Table 3 that different mass ratios of nano-Al particles to nano-Ni particles have different effects on the tin-copper-antimony lead-free solder. The use of a mass ratio of nano-Al particles to nano-Ni particles of 1:1 can maximize the improvement of the microhardness of the tin-copper-antimony lead-free solder, thereby improving the performance of the tin-copper-antimony lead-free solder.

[0160] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A tin-copper-antimony lead-free solder, characterized in that: Made of the following ingredients by weight: 0.5-1.5% Cu, 0.3-1.2% Sb, 0.02-0.04% Ni, 0.02-0.04% Al, 0.2-1.4% P, 0.1-0.6% Ce, and the balance is Sn; the Ni is nano Ni particles; the Al is nano Al particles; The mixing mass ratio of the nano-Al particles to the nano-Ni particles is 1:1; The method for preparing nano Ni particles comprises the following steps: (1) adding polyvinyl alcohol to deionized water and stirring to dissolve the mixture to obtain a polyvinyl alcohol solution; (2) adding nickel oxide particles to a polyvinyl alcohol solution and dispersing the particles by ultrasonic to obtain a composite dispersion; (3) drying by rotary evaporation to obtain coated nickel oxide particles; (4) grinding the coated nickel oxide particles to obtain fine coated nickel oxide particles; (5) The coated nickel oxide particle fine material is calcined under the protection of an inert atmosphere to obtain nano-Ni particles.

2. The tin-copper-antimony lead-free solder according to claim 1, characterized in that: The mass fraction of the polyvinyl alcohol solution is 10-12%.

3. The tin-copper-antimony lead-free solder according to claim 1, characterized in that: The mass ratio of the nickel oxide particles to the polyvinyl alcohol solution is 1:10-15.

4. The tin-copper-antimony lead-free solder according to claim 1, characterized in that: The grinding method is: Glycerin is used as a grinding aid; Grinding is carried out according to the ball-to-material ratio of 10:1-2, and the grinding is divided into 3 stages; In the first stage, the grinding temperature is 25-28°C, the grinding speed is 1000-1100r / min, and the grinding time is 30-40min; In the second stage, the grinding temperature is 30-35°C, the grinding speed is 1500-1600r / min, and the grinding time is 30-40min; In the third stage, the grinding temperature is 40-42°C, the grinding speed is 1800-2000r / min, and the grinding time is 30-40min.

5. The tin-copper-antimony lead-free solder according to claim 1, characterized in that: The inert atmosphere is nitrogen; The calcination temperature is 415-440°C.

6. A method for preparing a tin-copper-antimony lead-free solder according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Except Al and Ni, the other components are melted according to weight percentage to obtain a molten liquid; (2) Smelting under vacuum: Add the molten liquid of step (1) into a smelting device, evacuate the vacuum degree in the smelting device to 0.01-0.04 Pa, let it stand for 15-20 min, then introduce neon gas into the smelting device, and at the same time, increase the temperature in the smelting device to 500-580°C, add nano-Al particles, and keep the temperature for 3-5 min under high-frequency electromagnetic oscillation to obtain a composite molten liquid; (3) Adding nano-Ni particles to the composite melt in step (2), adjusting the temperature to 520-550°C, and keeping the temperature under high-frequency electromagnetic oscillation for 3-5 minutes and 50-60 minutes; (4) Cooling and solidification are performed to obtain tin-copper-antimony lead-free solder.

7. The method for preparing a tin-copper-antimony lead-free solder according to claim 6, characterized in that: The cooling rate is 5-8°C / s.

Citation Information

Patent Citations

  • A kind of znalmgin high temperature lead-free solder

    CN103934590B

  • Leadless high-temperature electronic solder and preparation

    CN101239425A

  • Leadless soft soldering material and manufacture method thereof

    CN101456103A

  • Maritime-climate-resistance tin solder and preparing method thereof

    CN105215568A

  • Lead-free sn-ni system solder alloy and solder alloy powder

    JP2009275241A